A porous metal capillary permeation microneedle electrode and preparation method thereof

Through the design of porous metal capillary microneedle electrodes, the porous microneedle array electrode sheet and capillary liquid absorbing core ring directly contact the skin, solving the problems of poor signal quality and skin damage in traditional bioelectric sensors, and achieving high signal-to-noise ratio electrical signal acquisition and artifact reduction.

CN109330711BActive Publication Date: 2024-11-05GUANGDONG ZHONGSHENG HUAKONG INTELLIGENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811377733.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-11-19
Publication Date
2024-11-05
Estimated Expiration
2038-11-19

AI Technical Summary

Technical Problem

Traditional bioelectric sensors require conductive paste during the process of collecting electrical signals, resulting in increased contact impedance, poor signal quality, and long-term use will damage the skin and prone to signal artifacts.

Method used

Design a porous metal capillary microneedle electrode, using a porous microneedle array electrode sheet sealed and spliced ​​with an insulating shell, built-in capillary liquid absorbing core ring and electrical signal line, and directly contact the skin dermis layer through normal saline as a conductive medium, reducing Impedance and slip, reducing artifacts.

Benefits of technology

It realizes high signal-to-noise ratio electrical signal acquisition, reduces signal artifacts, avoids damage to the skin by conductive paste, improves signal quality, and is suitable for long-term continuous use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109330711B_ABST
    Figure CN109330711B_ABST
Patent Text Reader

Abstract

The present invention discloses a porous metal capillary permeation microneedle electrode and a preparation method thereof. The porous metal capillary permeation microneedle electrode comprises a porous microneedle array electrode sheet, an insulating shell, an electrical signal line and a capillary wick ring. The porous microneedle array electrode sheet is provided with a plurality of porous microneedles with grooves; a cavity is formed inside the insulating shell, and an opening is provided on one side; the porous microneedle array electrode sheet and the opening of the insulating shell are sealed and assembled into a cavity, and the capillary wick ring is filled in the cavity; the groove is connected to the cavity. Based on the advantages of the microneedle structure, the present invention utilizes the adsorption and conductivity of the porous groove structure to the solution and the conductivity of the solution to achieve direct contact between the sensor and the dermis layer of the skin, greatly reduce the contact impedance, and can collect bioelectric signals with a high signal-to-noise ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical devices, and in particular to a porous metal capillary permeation microneedle electrode and a preparation method thereof. Background Art

[0002] With the development of electronic technology and the advancement of medical detection technology, human bioelectricity extraction can provide an important basis for disease diagnosis and prevention. Sensors that can be used continuously for a long time and collect high signal-to-noise ratio signals are receiving more and more attention.

[0003] The electrode sheet is the core component of the bioelectric sensor, and its performance is directly related to the results of signal acquisition. At present, the electrodes of the commonly used EEG sensors and myoelectric sensors on the market need to be used with conductive paste in the process of collecting electrical signals. Before the test, apply the conductive paste on the skin, and then place the electrode on the conductive paste for testing. During the test, the electrode only contacts the epidermis and cannot directly touch the dermis. The presence of conductive paste and epidermal stratum corneum increases the impedance link of the test process, resulting in poor quality of the obtained electrical signal. At the same time, the loss or evaporation of the conductive paste will also cause the signal-to-noise ratio of the electrical signal to be low, and long-term use will also damage the skin. On the other hand, the surface of traditional electrode sheets is relatively smooth, and it is easy to slide relative to the skin, so that the collected electrical signals contain a large number of artifacts. Summary of the invention

[0004] The main purpose of the present invention is to address the shortcomings of the traditional bioelectric sensor during use, propose a porous metal capillary permeation microneedle electrode and a preparation method, achieve high signal-to-noise ratio electrical signal acquisition, and reduce signal artifacts.

[0005] To achieve the above object, the present invention is implemented according to the following technical solutions.

[0006] A porous metal capillary permeation microneedle electrode comprises: an insulating shell, wherein a cavity is formed inside the insulating shell and an opening is provided on one side, wherein an electric signal line hole and a solution injection hole are provided on the insulating shell; a porous microneedle array electrode sheet, wherein the porous microneedle array electrode sheet is sealed and spliced ​​with the opening of the insulating shell, wherein the porous microneedle array electrode sheet is provided with a plurality of porous microneedles with grooves, wherein the grooves are parallel to the central axis of the microneedles, and wherein the grooves penetrate the porous metal microneedle array electrode sheet and are connected with the cavity; a capillary wick ring, wherein the capillary wick ring is filled in the cavity and is used for absorbing physiological saline entering through the solution injection hole; and an electric signal line, wherein the electric signal line penetrates from the electric signal line hole and passes through the capillary wick ring and then is connected with the porous microneedle array electrode sheet.

[0007] Furthermore, the porous metal microneedle array electrode sheet has a thickness of 1-2 mm and is made of a titanium metal material having a plurality of interconnected micropores and a porosity of 30-50%. Titanium metal is not only conductive but also has good biocompatibility with the human body. The plurality of interconnected micropores on the microneedle array electrode sheet allow liquid drugs or electrolytes to penetrate into the dermis of the skin through the microneedles.

[0008] Furthermore, the microneedle array is a rectangular array, the microneedles are conical, the bottom diameter of the microneedles is 200-500 μm, the height is 400-100 μm, the spacing between each microneedle is 1 mm; the channel diameter is 50-150 μm.

[0009] Furthermore, the inner wall of the channel has a fine velvet fin structure, which can adjust the capillary suction and permeability of the channel, thereby adjusting the flow of liquid.

[0010] Furthermore, the connection between the opening of the insulating shell and the porous microneedle array electrode sheet is sealed by an adhesive; the material of the insulating shell is one or more of silicone and plastic; the adhesive is epoxy resin or silicone elastic sealant. The insulating shell and the porous microneedle array electrode sheet are sealed and spliced ​​by the adhesive, which can effectively prevent leakage.

[0011] Furthermore, the porosity of the capillary absorbent core ring is 50-70%, and physiological saline is contained in the capillary absorbent core ring. The porosity of 50-70% can better ensure the storage and adsorption amount of liquid electrolyte in the capillary absorbent core ring.

[0012] Furthermore, the electrical signal line is connected to the porous microneedle array electrode sheet by welding.

[0013] The present invention also provides a method for preparing any of the porous metal capillary permeation microneedle electrodes described above, comprising the following steps:

[0014] 1) Mix titanium metal particles, ethanol, polyvinyl butyral, butyl benzyl phthalate, and dispersant in a mass fraction ratio of 46:46:1:6.5-7:1-1.5, and stir magnetically for 0.5-2h to form a titanium metal particle suspension for use;

[0015] 2) Prepare a stainless steel microneedle array template and an uncured PDMS mold, press the microneedle array surface of the stainless steel template onto the PDMS mold, perform vacuum curing, copy the microneedle array structure onto the PDMS mold, remove the stainless steel template, and obtain a cured PDMS mold;

[0016] 3) pouring the titanium metal particle suspension obtained in step 1) onto the cured PDMS mold, and using ultrasonic vibration to fully fill the mold cavity with the suspension, and then placing it in a vacuum chamber for 10-20 minutes to remove bubbles, and air-drying it at room temperature until the suspension agglomerates, and removing the suspension agglomerates from the PDMS mold after the alcohol is completely evaporated;

[0017] 4) Place the suspension agglomerate in a tube furnace and sinter it at 1240-1250°C for 2 hours in a chemically inert gas atmosphere. After sintering, cool it to room temperature in the tube furnace and take it out to obtain a porous metal microneedle electrode sheet;

[0018] 5) After the porous microneedle array electrode sheet is clamped and fixed, a groove is machined downward on the conical surface of each microneedle, and a fine velvety fin structure is formed on the inner wall of the groove;

[0019] 6) Insert the electric signal line through the electric signal line hole of the insulating shell and pass through the capillary absorbent core ring, and then weld and connect it to the porous microneedle array electrode sheet. Then, seal and assemble the porous microneedle array electrode sheet and the open opening of the insulating shell. The connection is sealed by an adhesive 5 to form a cavity structure inside. Fill and fix the capillary absorbent core ring in the cavity, and inject physiological saline into the capillary absorbent core ring through the solution injection hole of the insulating shell to make a porous metal capillary permeation microneedle electrode.

[0020] Furthermore, in step (1), the particle size of the metal particles is less than or equal to 10 μm.

[0021] Furthermore, in step (4), the chemically inert gas is nitrogen or argon.

[0022] Compared with the prior art, the present invention has the following advantages and effects:

[0023] (1) The porous metal liquid-permeable microneedle electrode of the present invention does not require conductive paste during use. The liquid electrolyte is used as a conductive enhancement medium, which can simplify a large amount of preparation work before testing and prevent the conductive paste from damaging the skin.

[0024] (2) The porous metal liquid-permeable microneedle electrode of the present invention forms a cavity with the insulating shell, and a capillary wick ring is arranged in the cavity, which can efficiently absorb physiological saline. The cavity is connected to the groove, and the liquid electrolyte can directly reach the dermis of the skin through the central groove, thereby achieving direct contact between the electrode and the dermis of the skin, greatly reducing the contact impedance, and at the same time reducing the relative slip between the electrode and the skin, reducing signal artifacts, and collecting bioelectric signals with a high signal-to-noise ratio.

[0025] (3) The porous metal capillary permeation microneedle electrode of the present invention adopts a porous microneedle structure with a central channel and a capillary liquid absorption core ring with a larger porosity, making full use of the capillary suction and permeability of the pores and channels to the physiological saline to maintain the wettability of the microneedle. At the same time, the capillary liquid absorption core ring with a larger porosity can provide physiological saline for the microneedle with a smaller porosity, and can also inhibit the volatilization and overflow of liquid during use. The setting of the capillary liquid absorption core ring and the channel can not only ensure the smooth flow of physiological saline, but also control the circulation speed of physiological saline. The fine velvety fin structure on the inner wall of the channel can adjust the capillary suction and permeability of the channel, thereby adjusting the flow of liquid, so that the amount and speed of liquid electrolyte flowing into the skin are more reasonable, which is more suitable for signal collection.

[0026] (4) Compared with traditional electrodes, the porous metal liquid-permeable microneedle electrode of the present invention uses a microneedle array electrode, which can directly reach the dermis of the skin without damaging the dermis tissue, greatly reducing the electrical impedance of the skin-electrode, while reducing the relative slip between the electrode and the skin, reducing signal artifacts, and achieving high-quality signal acquisition.

[0027] (5) The preparation method of the porous metal liquid-permeable microneedle electrode of the present invention is simple and efficient, and can be easily implemented in low-cost large-scale batch production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A cross-sectional view of a porous metal capillary permeation microneedle electrode according to the present invention;

[0029] Figure 2 It is a schematic diagram of the structure of a porous microneedle array electrode sheet;

[0030] Figure 3 for Figure 2 SEM image of center A;

[0031] Figure 4 It is a structural schematic diagram of the insulating housing;

[0032] Figure 5 Schematic diagram of preparing a PDMS mold with a microneedle array structure in Example 1;

[0033] Figure 6 Schematic diagram of the preliminary forming process of the porous metal microneedle electrode sheet in Example 1;

[0034] Figure 7 This is a schematic diagram of the structure of the porous microneedle array electrode sheet processed in Example 1;

[0035] Figure 8 This is a scanning electron microscope image of the fine velvety fin structure in the groove;

[0036] Fig. 9 for Figure 8A partial enlarged view of B.

[0037] In the attached figure: 1. porous microneedle array electrode sheet; 2. insulating shell; 3. electric signal line; 4. capillary wick ring; 5. adhesive; 7. stainless steel microneedle array template; 8. PDMS mold; 9. electric signal line hole; 10. solution injection hole; 11. suspension agglomerate; 12. groove. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with relevant drawings and specific embodiments, but the implementation mode of the present invention is not limited to the following embodiments.

[0039] Example 1

[0040] like Figure 1-9 As shown, Figure 1 A cross-sectional view of a porous metal capillary permeation microneedle electrode according to the present invention; Figure 2 It is a schematic diagram of the structure of a porous microneedle array electrode sheet; Figure 4 It is a schematic diagram of the structure of the insulating shell.

[0041] like Figure 1 and Figure 4 As shown, a porous metal capillary permeation microneedle electrode comprises an insulating shell 2, wherein a cavity is formed inside the insulating shell 2 and an opening is provided on one side, wherein an electric signal line hole 9 and a solution injection hole 10 are provided on the insulating shell; a porous microneedle array electrode sheet 1, wherein the porous microneedle array electrode sheet 1 is sealed and spliced ​​with the opening of the insulating shell 2, wherein the porous microneedle array electrode sheet 1 is provided with a plurality of porous microneedles with grooves 12, wherein the grooves 12 are parallel to the central axis of the microneedles, and wherein the grooves 12 penetrate the porous metal microneedle array electrode sheet 1 and are connected with the cavity; a capillary wick ring 4, wherein the capillary wick ring 4 is filled in the cavity and is used for absorbing physiological saline entering through the solution injection hole 10; and an electric signal line 3, wherein the electric signal line 3 penetrates from the electric signal line hole 9 and passes through the capillary wick ring and is connected with the porous microneedle array electrode sheet.

[0042] Preferably, Figure 2 and 3 As shown, the porous metal microneedle array electrode sheet 1 has a thickness of 2 mm and is made of a titanium metal material having a plurality of interconnected micropores and a porosity of 30-50%.

[0043] Preferably, the microneedle array is a rectangular array, preferably a square array, and is arranged in a 7*7 structure. The microneedles are conical and have a bottom diameter of 500 μm and a height of 1000 μm. The spacing between each microneedle is 1 mm. The groove 12 passes through the porous microneedle array electrode sheet 1 and is connected to the cavity. The groove 12 has a diameter of 100 μm, and the inner wall of the groove 12 has a fine velvety fin structure, such as Figure 8 As shown, Figure 8 This is a scanning electron microscope image of the fine velvety fin structure in the groove. Fig. 9 for Figure 8 A partial enlarged view of B in the middle. From the picture, we can see the fine velvety fin structure in the groove.

[0044] Preferably, the opening of the insulating shell 2 is formed by splicing the porous microneedle array electrode sheet 1 with the adhesive 5; the material of the insulating shell 2 is plastic; and the adhesive 5 is epoxy resin. The insulating shell 2 should match the porous microneedle array electrode sheet 1, and the shape of the cavity formed is not limited, and can be square or circular, or any other shape. In the present invention, it is preferably square. The capillary wick ring 4 is fixedly filled in the cavity, and the porosity of the capillary wick ring 4 is 50-70%. The capillary wick ring 4 is used to hold saline solution, and the saline solution is injected through the solution injection hole 10.

[0045] Preferably, the electrical signal line 3 is connected to the porous microneedle array electrode sheet 1 by welding.

[0046] Compared with traditional electrodes, the porous metal capillary permeation microneedle electrode of the present invention can pass through the epidermis to reach the dermis when in use, and the length of the microneedle is specially designed and will not touch the user's nerves and will not cause pain. The porous metal capillary permeation microneedle electrode is connected to an external instrument through an electrical signal line 3 to obtain an electrical signal, and the capillary wick ring 4 can reasonably control the circulation and flow rate of physiological saline due to its capillary suction and penetration force, control the flow rate, and effectively inhibit the volatilization and overflow of liquid during use. The setting of the capillary wick ring 4 and the groove 12 can not only maintain the wettability of the microneedle, but also provide physiological saline for the microneedle, and the physiological saline can penetrate into the skin through the pores of the porous microneedle array electrode sheet 1 to improve the measured electrical signal.

[0047] The present invention also provides a method for preparing the porous metal capillary permeation microneedle electrode, comprising the following steps:

[0048] (1) Titanium metal particles with a particle size of 10 μm, ethanol, PVB (polyvinyl butyral), BBP (butyl benzyl phthalate), and a dispersant were mixed in a mass fraction ratio of 46:46:1:7:1, and magnetically stirred for 1 hour to form a titanium metal particle suspension for use.

[0049] (2) Figure 5 As shown, a stainless steel microneedle array template 7 and an uncured PDMS mold 8 are prepared. The microneedle array is a square array, the microneedle bottom diameter is 500μm, the height is 1000μm, and the spacing is 1mm. The microneedle array surface of the stainless steel microneedle array template 7 is pressed onto the PDMS mold 8, and then vacuum curing is performed to copy the microneedle array structure onto the PDMS mold 8. The stainless steel template is removed to obtain a cured PDMS mold 8.

[0050] (3) Figure 6 As shown, the titanium metal particle suspension prepared in step (1) is poured into the solidified PDMS mold 8, and ultrasonic vibration is performed for 5 minutes to allow the suspension to fully fill the mold cavity. The mold is then placed in a vacuum chamber for 15 minutes to remove bubbles, and air-dried at room temperature until the suspension agglomerates 11. After the alcohol is completely evaporated, the suspension agglomerates 11 are removed from the PDMS mold 8.

[0051] (4) Place the suspension agglomerate 11 in a tube furnace and sinter at 1240°C-1250°C for 2 hours in a flowing argon atmosphere. After sintering, cool the tube furnace to room temperature and take out the finished porous metal microneedle electrode sheet 1. Figure 7 shown.

[0052] (5) After the porous microneedle array electrode sheet 1 is clamped and fixed, a micro-milling cutter with a diameter of 100 μm is used to machine a groove 12 downward on the conical surface of each microneedle, so that the inner wall of the machined groove 12 forms a fine velvety fin structure, such as Figure 8-9 shown.

[0053] (6) The electric signal line 3 is inserted into the electric signal line hole 9 of the insulating shell 2 and passes through the capillary wick ring 4, and then connected to the porous microneedle array electrode sheet 1 by welding. The porous microneedle array electrode sheet 1 and the open opening of the insulating shell 2 are then sealed and assembled. The connection is sealed by an adhesive 5. The capillary wick ring 4 is fixedly filled in the cavity, and physiological saline is injected into the capillary wick ring 4 through the solution injection hole 10 of the insulating shell 2 to make a porous metal capillary permeation microneedle electrode.

[0054] The dispersant mentioned above is preferably polyethylene glycol or methyl styrene.

[0055] Compared with the prior art, the method for preparing the porous metal liquid-permeable microneedle electrode of the present invention is simple. Figure 2 and Figure 3It can be seen that in addition to the grooves 12, the obtained porous metal microneedle electrode sheet also has many interconnected micropores, and the formed micropores have adsorption properties to the solution, and the capillary liquid absorption core ring 4 with a larger porosity can provide physiological saline for the microneedles with a smaller porosity, and can also inhibit the volatilization and overflow of liquid during use. Physiological saline can enhance conductivity, improve the ability to extract signals, reduce physiological signal noise, and improve the signal-to-noise ratio.

[0056] Example 2

[0057] The porous metal capillary permeation microneedle electrode of this embodiment is the same as that of embodiment 1, except that the thickness of the porous metal microneedle array electrode sheet is 1.5 mm. The bottom diameter of the microneedle is 300 μm, the height is 500 μm, the spacing is 1 mm, and the diameter of the groove 12 is 100 μm. The material of the insulating shell 2 is silicone, and the adhesive 5 is silicone elastic sealant.

[0058] The preparation method of the porous metal capillary permeation microneedle electrode is similar to that of Example 1, except that the titanium metal particles have a diameter of 5 μm, and the titanium metal particles, ethanol, PVB, BBP, and dispersant are mixed in a mass fraction ratio of 46:46:1:6.5:1.5. In step (4), sintering is performed in a nitrogen atmosphere.

[0059] The specific embodiments of the present invention are only examples for clarifying the present invention, and are not intended to limit the embodiments of the present invention. For technical workers in the corresponding fields, similar changes can be made on the basis of the above description, and changes within the scope of the claims can also be realized. It is impossible and unnecessary to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A porous metal capillary permeation microneedle electrode, characterized in that: include, An insulating shell, wherein a cavity is formed inside the insulating shell and an opening is provided on one side, and an electric signal line hole and a solution injection hole are provided on the insulating shell; A porous microneedle array electrode sheet, the porous microneedle array electrode sheet is sealed and spliced ​​with the opening of the insulating shell, the porous microneedle array electrode sheet is provided with a plurality of porous microneedles with grooves, the grooves are parallel to the central axis of the microneedles, and the grooves penetrate the porous metal microneedle array electrode sheet and communicate with the cavity; the inner wall of the grooves has a fine velvety fin structure; a capillary wick ring, which is filled in the cavity and is used to absorb the physiological saline entering through the solution injection hole; an electric signal line, the electric signal line passes through the electric signal line hole and through the capillary wick ring and then is connected to the porous microneedle array electrode sheet; The method for preparing the porous metal capillary permeation microneedle electrode comprises the following steps: 1) Mix titanium metal particles, ethanol, polyvinyl butyral, butyl benzyl phthalate, and dispersant in a mass fraction ratio of 46:46:1:6.5-7:1-1.5, and stir magnetically for 0.5-2h to form a titanium metal particle suspension for use; 2) Prepare a stainless steel microneedle array template and an uncured PDMS mold, press the microneedle array surface of the stainless steel template onto the PDMS mold, perform vacuum curing, copy the microneedle array structure onto the PDMS mold, remove the stainless steel template, and obtain a cured PDMS mold; 3) pouring the titanium metal particle suspension obtained in step 1) onto the cured PDMS mold, and using ultrasonic vibration to fully fill the mold cavity with the suspension, and then placing it in a vacuum chamber for 10-20 minutes to remove bubbles, and air-drying it at room temperature until the suspension agglomerates, and removing the suspension agglomerates from the PDMS mold after the alcohol is completely evaporated; 4) Place the suspension agglomerate in a tube furnace and sinter it at 1240-1250°C for 2 hours in a flowing chemically inert gas atmosphere. After sintering, cool it to room temperature in the tube furnace and take it out to obtain a porous metal microneedle electrode sheet; 5) After the porous microneedle array electrode sheet is clamped and fixed, a groove is machined downward on the conical surface of each microneedle, and a fine velvety fin structure is formed on the inner wall of the groove; 6) Insert the electric signal line through the electric signal line hole of the insulating shell and pass through the capillary absorbent core ring, and then weld and connect it to the porous microneedle array electrode sheet. Then, seal and assemble the porous microneedle array electrode sheet and the open opening of the insulating shell. The connection is sealed with an adhesive to form a cavity structure inside. Fill and fix the capillary absorbent core ring in the cavity, and inject physiological saline into the capillary absorbent core ring through the solution injection hole of the insulating shell to make a porous metal capillary permeation microneedle electrode.

2. A porous metal capillary permeation microneedle electrode according to claim 1, characterized in that: The porous metal microneedle array electrode sheet has a thickness of 1-2 mm and is made of a titanium metal material having a plurality of interconnected micropores and a porosity of 30-50%.

3. The porous metal capillary permeation microneedle electrode according to claim 1, characterized in that: The microneedle array is a rectangular array, the microneedles are conical, the bottom diameter of the microneedles is 200-500 μm, the height is 400-1000 μm, and the spacing between each microneedle is 1 mm; the channel diameter is 50-150 μm.

4. The porous metal capillary permeation microneedle electrode according to claim 1, characterized in that: The connection between the opening of the insulating shell and the porous microneedle array electrode sheet is sealed by an adhesive; the material of the insulating shell is one or more of silicone and plastic; the adhesive is epoxy resin or silicone elastic sealant.

5. The porous metal capillary permeation microneedle electrode according to claim 1, characterized in that: The porosity of the capillary wick ring is 50-70%.

6. The porous metal capillary permeation microneedle electrode according to claim 1, characterized in that: The electric signal line is connected to the porous microneedle array electrode sheet by welding.

7. The porous metal capillary permeation microneedle electrode according to claim 1, characterized in that: In step 1), the particle size of the metal particles is less than or equal to 10 μm.

8. The porous metal capillary permeation microneedle electrode according to claim 1, characterized in that: In step 4), the chemically inert gas is nitrogen or argon.