A casting sand core box and a manufacturing method thereof
Through block design and material optimization, the problems of insufficient strength and long production cycle of existing casting sand core boxes have been solved, efficient and low-cost sand core production and maintenance have been achieved, and the production needs of complex profiles of large hydraulic turbine blades have been met. .
Patent Information
- Application Number
- CN201910200321.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-03-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2039-03-16
AI Technical Summary
The main material of the existing casting sand core box has low strength, is easy to deform, has a long production cycle, and the repair cycle and cost are high, making it difficult to meet the complex profile and mass production needs of large hydraulic turbine blades.
Adopting the basic and shaped block design, through the splicing of regular shaped blocks and shaped blocks, combined with positioning rods and dovetail groove/pin positioning, a high-strength and maintainable core box model is formed, using modeling sand. and wood mold/resin mold materials to shorten the production cycle and reduce costs.
It improves the strength and dimensional control accuracy of the core box, shortens the production cycle, reduces production costs, and simplifies the maintenance process, meeting the mass production needs of large hydraulic turbine blades.
Smart Images

Figure CN109822046B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting, and mainly relates to a casting sand core box and a manufacturing method thereof. Background Art
[0002] The surface of large turbine blades is curved, with large outline dimensions, strict tolerances, complex process modeling, high overall requirements, and easy deformation during the casting process. Therefore, large turbine blades usually adopt the three-dimensional core assembly modeling method. Compared with traditional modeling methods, the three-dimensional core assembly modeling method has the advantages of light sand core lifting weight, simple operation and easy control, and short production cycle. It greatly reduces the equipment requirements for blade production and solves the problem of insufficient previous production capacity, realizing mass production of blades. At present, the core box used in the three-dimensional core assembly method to make sand cores is usually a wooden core box, which has the following three main disadvantages:
[0003] 1) The main material of the core box has low strength and is easy to change. The sand core of a large turbine blade is about 70 tons. Due to the high structural strength requirements of the core box, a wooden frame structure core box is used. For batch parts, the core box is very easy to deform and damage, resulting in deformation of the sand core, and the core setting process will cause the sand core to be inconsistent with the size;
[0004] 2) The core box production cycle is long. Due to the complex blade profile, it needs to be processed by a 5-axis machining center. The traditional wooden core box cycle is about 25 days, accounting for one-fifth of the total blade blank production cycle, affecting the overall delivery time of the product;
[0005] 3) The core box repair cycle is long and the cost is high. The core box and live block of large turbine blades are prone to deformation and damage of the main material during the core making and demolding process. At the same time, the complex curved surface size is not easy to repair. Summary of the invention
[0006] The invention aims at the defects in the prior art and provides a casting sand core box and a manufacturing method thereof.
[0007] The technical solution of the present invention is: the core box includes a core box model, and the core box model includes a basic type and a surface type; the working surface of the surface type matches the shape of the casting; the surface opposite to the working surface of the surface type matches the installation surface of the basic type, and the installation surface of the basic surface is a regular structure that undulates up and down.
[0008] Preferably, the basic type includes a plurality of regularly shaped blocks, and the regularly shaped blocks are spliced with each other to form the basic type.
[0009] Preferably, the surface shape includes a plurality of surface shape blocks, and the surface shape blocks are spliced with each other to form the surface shape.
[0010] Preferably, the shaped surface mold further comprises a shaped surface mold movable block, and the shaped surface mold movable block is installed at the starting position of the shaped surface mold.
[0011] Preferably, the thickness of the profile block is less than 300 mm.
[0012] Preferably, the machining error of the side surface of the profile block is 0 mm to -10 mm, and the machining error of the profile surface is -3 mm to +3 mm.
[0013] Preferably, the regular-shaped blocks are made of molding sand as raw material.
[0014] Preferably, a basic frame is provided inside the regular-shaped molding block to reduce the amount of molding sand.
[0015] Preferably, the shaped surface of the shaped block is made of a wooden mold, a lost foam mold or a resin mold.
[0016] The method for making the casting sand core box as described above comprises the following steps:
[0017] The core box model is divided into a basic type and a surface type, and a working surface of the surface type is manufactured according to the outer shape structure of the casting; and a surface opposite to the working surface of the surface type is manufactured according to the installation surface of the basic type;
[0018] Assemble the basic type and the shape type, and harden and polish the working surface of the shape type to form a core box model. Place the core box model in the core box frame to complete the production of the core box.
[0019] The invention provides a casting sand core box, the core box comprising a core box model, the core box model comprising a basic type and a surface type; the thickness of the basic type is as thick as possible to reduce the material used in the surface type, the surface of the basic type is as few and flat as possible, and is easy to be scraped and formed; the basic type is mainly generated by assembling a plurality of regular-shaped blocks, and positioning rods are accurately preset according to positioning coordinates for accurate installation; a basic frame is arranged inside the regular-shaped block, which is prefabricated in the core box frame to reduce the amount of sand used in the regular-shaped block; the regular-shaped block uses modeling sand as a raw material, which can ensure the strength of the core box, and can be recycled and reused to reduce costs. The surface mold is mainly assembled by several surface mold blocks. The parts of the surface mold that affect the molding are made into movable blocks. Dovetail grooves and / or latches are used to locate the surface mold blocks and the remaining molds are made into a whole to ensure the strength of the surface mold. The thickness of the surface mold block is less than 300mm, the processing error of the side of the surface mold block is 0mm~-10mm, and the processing error of the surface is -3mm~+3mm to ensure the dimensional accuracy of the surface mold. The surface of the surface mold block adopts a wooden mold or a resin mold to enhance the strength of the surface mold and meet the mass production of castings.
[0020] The core box provided by the present invention can be manufactured in parallel with the basic type and the surface type. The basic type and the surface type are respectively divided into a plurality of corresponding blocks, and each module can be processed separately in parallel, which significantly shortens the production cycle of the core box; and the core box adopts a block design method. When the surface type is damaged and repaired, the damaged part of the surface type block can be disassembled, the basic surface is kept unchanged, and the damaged surface type is selected for partial reprocessing. After the processing, the surface type is directly assembled to the corresponding part, fixed and surface treated, so as to achieve the purpose of core box repair and maintenance. The modeling sand used in the basic type of the present invention can be reused, so as to achieve the purpose of saving resources and reducing costs.
[0021] The novel core box and the manufacturing method thereof provided by the present invention ensure the strength of the core box, are conducive to the control of the sand core size, shorten the production cycle, reduce the production cost, and are easy to maintain. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Attached Figure 1 It is a basic schematic diagram of the core box of the present invention;
[0023] Attached Figure 2 It is a schematic diagram of the working profile of the core box of the present invention;
[0024] Attached Figure 3 It is a schematic diagram of the surface relative to the working surface of the core box of the present invention;
[0025] Attached Figure 4 It is a schematic diagram of the basic type and the surface type of the core box of the present invention being assembled into one;
[0026] In the figure: 10-basic type; 20-surface type. DETAILED DESCRIPTION
[0027] In conjunction with the accompanying drawings of the present invention, a technical solution of an embodiment of the invention is further elaborated in detail.
[0028] In the present invention, unless otherwise clearly specified and limited, the terms should be understood in a broad sense, and a person of ordinary skill in the art can understand the specific meaning of the terms in the present invention according to specific circumstances.
[0029] A casting sand core box, see attached Figures 1 to 4 As shown, the core box includes a core box model, and the core box model includes a basic mold 10 and a surface mold 20; the working surface of the surface mold 20 matches the shape of the casting; the surface opposite to the working surface of the surface mold 20 matches the mounting surface of the basic mold 10, and the mounting surface of the basic mold 10 is a regular shaped structure that undulates up and down.
[0030] In one embodiment, the basic type 10 includes a plurality of regular-shaped blocks, and the regular-shaped blocks are spliced with each other to form the basic type 10 .
[0031] In one embodiment, the surface shape includes a plurality of surface shape blocks, and the surface shape blocks are spliced with each other to form the surface shape.
[0032] Specifically, the face mold 20 also includes a face mold movable block, which is installed at the starting position of the face mold.
[0033] It should be noted that a casting sand core box mainly includes a basic mold 10 and a shaped surface mold 20. The thickness of the basic mold 10 is as thick as possible to reduce the material used for the shaped surface mold. The shaped surface of the basic mold 10 is as few and flat as possible, and is easy to scrape and mold. The basic mold 10 is mainly assembled by a number of regular-shaped blocks, and a positioning rod is accurately preset according to the positioning coordinates for accurate installation. The shaped surface mold 20 is mainly assembled by a number of shaped surface blocks. The part of the shaped surface mold 20 that affects the molding is made into a movable block. The shaped surface blocks and the movable blocks are positioned by dovetail grooves and / or latches. The rest of the mold is made into a whole to ensure the strength of the shaped surface mold.
[0034] In one embodiment, the thickness of the profile block is less than 300 mm.
[0035] Specifically, the machining error of the side surface of the profile block is 0mm to -10mm, and the machining error of the profile surface is -3mm to +3mm, so as to ensure the dimensional accuracy of the profile.
[0036] In one embodiment, the regular-shaped blocks are made of molding sand, which can ensure the strength of the core box and can be recycled to reduce costs.
[0037] Specifically, a basic frame is provided inside the regular-shaped block to reduce the amount of molding sand.
[0038] It should be noted that a basic frame is provided inside the regular-shaped block, which is prefabricated in the core box frame, thereby reducing the amount of sand used in the regular-shaped block and reducing production costs.
[0039] In one of the embodiments, the surface of the shaped block is made of a wooden mold, a lost foam mold or a resin mold to enhance the strength of the shaped block and meet the requirements of mass production of castings.
[0040] A method for making more than one casting sand core box comprises the following steps:
[0041] Step S001, dividing the core box model into a basic mold 10 and a surface mold 20, manufacturing a working surface of the surface mold 20 according to the casting shape structure; manufacturing a surface opposite to the working surface of the surface mold 20 according to the installation surface of the basic mold 10;
[0042] Step S002, assembling the basic mold 10 and the shape mold 20, and hardening and polishing the working surface of the shape mold 20 to form a core box model, placing the core box model in the core box frame, and completing the production of the core box.
[0043] It should be noted that a gypsum layer with a thickness greater than or equal to 2 mm is scraped on the entire surface of the shape 20. After the gypsum layer hardens, the surface is polished using a flat grinder, which ensures the surface quality of the shape 20 and increases the surface strength of the shape.
[0044] In one of the embodiments, in the above step S001, the shape surface type 20 is divided into a number of shape surface type blocks according to the casting structure and the on-site machine tool processing size range, and the shape surface type blocks are numbered and manufactured; the shape surface type blocks are assembled according to the numbers with the lowest point of the shape surface type 20 as the starting point, and the shape surface type is positioned by marking and tightened to form the shape surface type 20.
[0045] It should be noted that when assembling various types of blocks, an absolute reference is set, and the deviation between each block and the absolute reference is measured to reduce the cumulative deviation when the blocks are connected; and when assembling various types of blocks, the positioning rods are accurately preset according to the positioning coordinates for accurate installation; an adjustment gap of about 5mm is set between the positioning rods and the surface blocks, and the surface is positioned by marking, and finally tightened to form the overall surface shape, and the positioning rods are used to prevent misalignment between the surface blocks.
[0046] In one embodiment, in the above step S001, the basic mold 10 is divided into a number of regular-shaped blocks, which are numbered and manufactured; and the regular-shaped blocks are assembled according to the numbers to form the basic mold 10.
[0047] The core box provided by the present invention can be manufactured in parallel with the basic type and the surface type. The basic type and the surface type are respectively divided into a plurality of corresponding blocks, and each module can be processed separately in parallel, which significantly shortens the manufacturing cycle of the core box. In addition, the core box adopts a block design method. When the surface type is damaged and needs to be repaired, the damaged part of the surface type block can be disassembled, the basic surface is kept unchanged, and the damaged surface type is selected to be partially reprocessed. After the processing, the surface type is directly assembled to the corresponding position, fixed and surface treated, so as to achieve the purpose of repairing and maintaining the core box.
[0048] The novel core box and the manufacturing method thereof provided by the present invention ensure the strength of the core box, are conducive to the control of the sand core size, shorten the production cycle, reduce the production cost, and are easy to maintain.
[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention shall be included in the protection scope of the present invention.
Claims
1. A casting sand core box, characterized in that: The core box includes a core box model, and the core box model includes a basic type and a shaped surface type; the working shaped surface of the shaped surface type matches the shape of the casting; the surface opposite to the working shaped surface of the shaped surface type matches and is installed with the mounting surface of the basic type, and the mounting surface of the basic type is a regular shaped structure that fluctuates up and down; the basic type includes a plurality of regular shaped blocks, and each of the regular shaped blocks is spliced with each other to form the basic type; the shaped surface type includes a plurality of shaped surface blocks, and each of the shaped surface blocks is spliced with each other to form the shaped surface type; the regular shaped blocks use molding sand as raw material; a basic frame is provided inside the regular shaped blocks to reduce the amount of molding sand; the working shaped surface surface of the shaped surface block uses a wooden mold, a lost foam mold or a resin mold.
2. The casting sand core box according to claim 1, characterized in that: The shaped surface mold further comprises a shaped surface mold movable block, and the shaped surface mold movable block is installed at the starting position of the shaped surface mold.
3. The casting sand core box according to claim 1, characterized in that: The thickness of the profile block is less than 300 mm.
4. The casting sand core box according to claim 3, characterized in that: The machining error of the side surface of the shape block is 0mm to -10mm, and the machining error of the shape surface is -3mm to +3mm.
5. A method for manufacturing a casting sand core box according to any one of claims 1 to 4, characterized in that: The steps include: The core box model is divided into a basic type and a surface type, and a working surface of the surface type is manufactured according to the outer shape structure of the casting; and a surface opposite to the working surface of the surface type is manufactured according to the installation surface of the basic type; Assemble the basic type and the shape type, and harden and polish the working surface of the shape type to form a core box model. Place the core box model in the core box frame to complete the production of the core box.