Magnetic orientation graphene / carbon composite material and preparation method thereof

By using porous carbon matrix and magnetic graphene synthesized by plant sugar in graphene thermally-reinforced composite materials, the directional and low-temperature and high-temperature treatment of graphene are solved in the prior art, and the cumbersome and cost of preparing graphene thermally-reinforced composite materials in the prior art. The high problem has achieved efficient and low-cost directional and large-scale production of graphene nanosheets, improving the thermal conductivity and thermal insulation performance of the material.

CN118993050AActive Publication Date: 2024-11-22SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202411079519.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing preparation methods of graphene thermally reinforcing composite materials have problems such as cumbersome preparation process, high cost, and difficulty in achieving efficient orientation and large-scale production of graphene nanosheets.

Method used

The porous carbon matrix synthesized by plant sugar and magnetic graphene composite material is used to orient the graphene using a rotating magnetic field through a magnetic orientation device, and the low-temperature pre-carbonization and high-temperature graphitization are carried out to form an ordered magnetically oriented graphene layer, which is simplified. Preparation process and reduce costs.

Benefits of technology

The orderly orientation of graphene in the composite matrix is ​​achieved, the thermal conductivity and thermal insulation properties of the material are improved, the preparation process is simplified, the cost is reduced, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993050A_ABST
    Figure CN118993050A_ABST
Patent Text Reader

Abstract

The invention discloses a magnetic orientation graphene / carbon composite material and a preparation method thereof, and belongs to the technical field of composite materials. The magnetic orientation graphene / carbon composite material is composed of a porous carbon matrix and a plurality of magnetic orientation graphene layers which are alternately arranged in the porous carbon matrix in parallel in the vertical direction; the porous carbon matrix is formed by connecting carbon nano-particles converted from a plant sugar precursor, and the carbon nano-particles in the porous carbon matrix are mutually connected to form micro-nano-sized closed pores; the magnetic orientation graphene layer is formed by mutually lapping two-dimensional reduced graphene oxide nanosheets. The preparation method comprises the following steps: preparing magnetic graphene dispersion liquid and plant sugar precursor sol, and then stirring and mixing the magnetic graphene dispersion liquid and the plant sugar precursor sol to obtain mixed sol; orienting the magnetic graphene in the mixed sol by using a magnetic orienting device, and then adding an initiator to cure the mixed sol into gel; and performing low-temperature pre-carbonization and high-temperature graphitization on the gel to obtain the magnetic orientation graphene / carbon composite material. The preparation method is simple, the graphene orientation is controllable, the cost is low, and the composite material can be prepared through integrated molding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a magnetically oriented graphene / carbon composite material and a preparation method thereof. Background Art

[0002] As a new type of material, graphene has ultra-high strength and an in-plane thermal conductivity of more than 5000 W / (m·K). Using graphene as a thermal conductivity enhancing filler provides a rare opportunity for the development of a new generation of heat dissipation materials. However, due to the very small size of graphene itself (less than 1 nanometer in thickness and tens of microns in two-dimensional directions), it is difficult to control at the nanoscale. At the same time, when graphene is used as a thermal conductivity enhancing filler, it is easy to agglomerate, and the graphene inside the agglomerate is highly disordered, especially when the graphene concentration is high, which will aggravate the agglomeration and disorder of graphene. In addition, phonons in two-dimensional materials can only propagate effectively in the in-plane lattice, and the thermal conductivity of graphene is highly anisotropic (two orders of magnitude different between in-plane and out-of-plane), so the improvement of the thermal conductivity enhancement effect of graphene is closely related to the ordered orientation of graphene nanosheets in the matrix. In summary, orderly orienting graphene in the matrix is ​​the key and difficulty in fully utilizing the high thermal conductivity of graphene. Otherwise, it will not only fail to enhance thermal conductivity, but will have an adverse effect.

[0003] At present, many researchers have controlled the orientation of graphene. For example, Chinese patent publication number CN112225204A - Method and equipment for controlling graphene orientation in graphene sponge and Chinese patent publication number CN112357910A - Method for preparing an oriented graphene composite macrobody both use the ice template method to induce the preparation of oriented graphene aerogels. Although this method can prepare graphene with orderly and controllable orientation, the process is time-consuming and costly, and is not suitable for large-scale preparation.

[0004] For example, in the existing paper "Orientation Control of Graphene Flakes by Magnetic Field: Broad Device Applications of Macroscopically Aligned Graphene" (Adv. Mater. 2016, DOI: 10.1002 / adma.201604453), Lin et al. used an external constant magnetic field to deflect graphene, but the static magnetic field used in this method can only control the degree of freedom of the graphene nanosheet in one direction, and cannot achieve the parallel arrangement of two-dimensional graphene nanosheets.

[0005] The preparation route of traditional graphene thermally conductive enhanced composite materials is: first prepare a thermally conductive skeleton preform, then increase the volume density of the composite material through repeated impregnation of the matrix or repeated CVI densification and other processes, and finally obtain a high-strength, high-thermal-conductivity composite material. For example, the Chinese patent with publication number CN110452414A - a method for preparing a highly oriented graphene-enhanced bismaleimide resin-based composite material and the Chinese patent with publication number CN109705817A - a high-thermal-conductivity, fast-response phase-change energy storage composite material and its preparation method both first prepare the graphene preform skeleton by freeze-drying, and then use vacuum impregnation to backfill the skeleton. The block material prepared by this process has high strength and excellent thermal properties, but this preparation process requires repeated densification, and the preparation process is cumbersome, resulting in a long product preparation cycle, which is not conducive to large-scale preparation. For example, in the existing paper "Magnetic Field-Induced Aligned Graphene / Cellulose Conductive Composites for Electroluminescent Devices" (ACS Appl. Nano Mater. 2023, DOI: 10.1021 / acsanm.3c03678), Zhi et al. used an external single static magnetic field to integrate the preparation of graphene / cellulose composites. Although this method can achieve the ordered orientation of graphene in the composite material, it can only prepare thin film materials. The thin films need to be stacked to obtain bulk materials, which is not conducive to large-scale preparation.

[0006] In summary, the existing preparation methods of oriented graphene thermally conductive enhanced composite materials lack a method that is simple in preparation method, has controllable graphene orientation, is low in cost, and can be integrated into a composite material. Summary of the invention

[0007] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a magnetically oriented graphene / carbon composite material and a preparation method thereof, which is simple, has controllable graphene orientation, low cost and can be integrated to prepare the composite material.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] The present invention provides a magnetically oriented graphene / carbon composite material, which is composed of a porous carbon matrix and a plurality of magnetically oriented graphene layers alternately arranged in parallel along a vertical direction inside the porous carbon matrix;

[0010] The porous carbon matrix is ​​formed by connecting carbon nanoparticles converted from plant sugar precursors, and the carbon nanoparticles in the porous carbon matrix are interconnected to form closed pores of micro-nano size;

[0011] The magnetically oriented graphene layer is formed by overlapping two-dimensional reduced graphene oxide nanosheets.

[0012] In one embodiment, the magnetically oriented graphene / carbon composite material is anisotropic, and the thermal conductivity in the horizontal direction parallel to the magnetically oriented graphene layer is 10-20 W / mk, and the thermal conductivity in the vertical direction perpendicular to the magnetically oriented graphene layer is 0.35-0.65 W / mk.

[0013] The present invention also provides a method for preparing the magnetically oriented graphene / carbon composite material, comprising the following steps:

[0014] S1: preparing a magnetic graphene dispersion and a plant sugar precursor sol, and then stirring and mixing the two to obtain a mixed sol;

[0015] S2: Orient the magnetic graphene in the mixed sol using a magnetic orientation device, and then add an initiator to solidify the mixed sol into a gel;

[0016] S3: The gel is subjected to low-temperature pre-carbonization and high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0017] In one embodiment, in S1, the method for preparing the magnetic graphene dispersion is as follows:

[0018] The graphene oxide, the ferrofluid and the water are mixed in a mass ratio of (1-20): (3-50): (10-40) to prepare a magnetic graphene dispersion;

[0019] The graphene oxide is a single-layer graphene oxide or a multi-layer graphene oxide; the magnetic graphene is a graphene oxide attached with ferroferric oxide nanoparticles in a ferromagnetic fluid.

[0020] In one embodiment, in S1, the method for preparing the plant sugar precursor sol is as follows:

[0021] The plant sugar, acrylamide, methylene bisacrylamide and water are mixed in a mass ratio of (10-100): (1-100): (0.1-10): (50-200) to prepare a plant sugar precursor sol;

[0022] The plant sugar is one or more of glucose, sucrose, starch, fructose, maltose and xylose.

[0023] In one embodiment, the mass proportion of magnetic graphene in the mixed sol is 2% to 20%.

[0024] In one embodiment, in S2, the magnetic orientation device comprises a neodymium iron boron magnet, a motor, a carrier plate, and a suspendable glass container;

[0025] The rotating shaft of the motor is connected to the center of the loading plate, the suspendable glass container is arranged above the loading plate, the two NdFeB magnets are arranged on the loading plate in parallel, and the NdFeB magnets are symmetrically arranged on both sides of the suspendable glass container.

[0026] In one embodiment, in S2, the process of orienting the magnetic graphene in the mixed sol using a magnetic orientation device is as follows:

[0027] The mixed sol is placed in a suspendable glass container, and a motor drives a parallel NdFeB magnet to rotate around the suspendable glass container to generate a rotating magnetic field to orient the magnetic graphene in the mixed sol;

[0028] The rotation speed is 1-50r / s.

[0029] In one embodiment, in S2, the initiator is one or more of ammonium persulfate, potassium persulfate, azobisisobutyronitrile and hydrogen peroxide.

[0030] In one embodiment, in S3, the low-temperature pre-carbonization process is as follows: heat treatment at a heating rate of 5°C / h for 36h in an air atmosphere;

[0031] In S3, the high temperature graphitization process is as follows: heat treatment at a temperature of 1800-2800° C. for 2 h in an argon-hydrogen mixed atmosphere.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention provides a method for preparing a magnetically oriented graphene / carbon composite material, which uses highly crystalline carbon synthesized from plant sugar as a carbon matrix, and uses cheap, easily available, recyclable plant sugar as a carbon source, and has high carbon yield, low cost and is environmentally friendly. Graphene oxide is used as a precursor of graphene. Graphene oxide has high surface activity and excellent dispersibility in plant sugar sol, which is conducive to large-scale preparation of composite materials. After the graphene oxide is converted into magnetic graphene, the magnetic graphene is oriented by the force of an external rotating magnetic field, so that the graphene nanosheets can be quickly oriented in the precursor solution. In addition, high-temperature graphitization treatment is performed, which not only improves the crystallinity of the composite material, but also converts the graphene oxide in the graphene layer into reduced graphene oxide to form a magnetically oriented graphene layer, which is conducive to reducing the defects of graphene and improving the performance of the composite material. Compared with the preparation method in the existing research on graphene thermal conductive enhanced composite materials, the entire preparation method simplifies the preparation process, shortens the preparation cycle, can realize the directional and orderly arrangement of graphene in the composite material matrix, and is conducive to low-cost and large-scale preparation of composite materials.

[0034] Furthermore, graphene oxide is easier for ferroferric oxide nanoparticles in ferromagnetic fluid to adhere to. By using simple mechanical stirring, ferroferric oxide nanoparticles in ferromagnetic fluid can be attached to the surface of graphene oxide. After the superparamagnetic ferroferric oxide nanoparticles are attached to the surface of graphene oxide, the graphene oxide can have an extremely strong magnetic response.

[0035] The present invention provides a magnetically oriented graphene / carbon composite material, which adopts reduced graphene oxide as a thermal conductivity enhancer, and a magnetically oriented graphene layer formed by overlapping reduced graphene oxide nanosheets is filled in a carbon matrix converted from plant sugar, so as to prepare an anisotropic graphene / carbon composite material with high thermal conductivity, high thermal insulation and high strength. Reduced graphene oxide nanosheets overlap each other to form a magnetically oriented graphene layer with directional order. The two-dimensional magnetically oriented graphene layers are arranged parallel to each other, forming a good heat transfer path in the horizontal direction parallel to the magnetically oriented graphene layers, which is conducive to the rapid dissipation of heat; in the vertical direction perpendicular to the magnetically oriented graphene layers, the magnetically oriented graphene layers act as layers of barriers to phonon diffusion, which can effectively block the transmission of heat. In addition, due to the presence of micro-nano-sized closed pores in the porous carbon matrix formed by the conversion of plant sugar precursors, thermal convection and thermal collision of gas molecules are limited, further reducing the heat transfer of the material in the vertical direction, so that the material has both high thermal conductivity and high thermal insulation, which can meet the needs of the thermal management field for materials with excellent heat dissipation and thermal insulation properties. At the same time, the magnetically oriented graphene layer also plays a role in mechanical enhancement in the porous carbon matrix. When the material is subjected to external stress, the crack propagates in the porous carbon matrix and encounters the magnetically oriented graphene layer, which can cause the crack to be deflected, consuming the crack propagation fracture energy while reducing the crack propagation rate; the crack will bifurcate at the interface, changing the propagation direction and extending the crack propagation path, delaying the damage and failure of the material; in addition, the removal of the magnetically oriented graphene layer can also consume external stress, thereby further improving the mechanical properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Figures a and b are optical photographs of the magnetically oriented graphene / carbon composite material prepared in Example 1 of the present invention;

[0037] Figure 2 This is a SEM photo of the magnetically oriented graphene / carbon composite material prepared in Example 1 of the present invention;

[0038] Figure 3 The Raman spectrum of the magnetically oriented graphene / carbon composite material prepared in Example 1 of the present invention;

[0039] Figure 4 This is an infrared thermal imaging image of the magnetically oriented graphene / carbon composite material prepared in Example 1 of the present invention during heating on the surface of a heating platform (200° C.);

[0040] Figure 5 The compressive strength comparison diagram of magnetically oriented graphene / carbon composite materials with different magnetic graphene contents prepared in Example 1, Example 2, and Example 3 of the present invention; wherein, Figure a is a stress-strain curve diagram, and Figure b is a relationship diagram between the amount of magnetic graphene added and the ultimate compressive strength of the composite material;

[0041] Figure 6 The structural design diagram of the magnetically oriented graphene / carbon composite material prepared by the present invention;

[0042] Figure 7 A schematic diagram of a magnetic orientation device used in the present invention;

[0043] Among them, 1-suspendable glass container, 2-NdFeB magnet, 3-carrying plate, 4-motor, 5-rotating shaft; 6-porous carbon matrix, 7-magnetically oriented graphene layer. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0045] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0046] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0047] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0048] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0049] It should be noted that the horizontal directions in this article are all directions parallel to the magnetically oriented graphene layer; and the vertical directions are all directions perpendicular to the magnetically oriented graphene layer.

[0050] The invention provides a magnetically oriented graphene / carbon composite material and a preparation method thereof.

[0051] On the one hand, a method for preparing a magnetically oriented graphene / carbon composite material is provided, and the preparation method comprises the following steps: preparing a magnetic graphene dispersion and a plant sugar precursor sol, and fully stirring and mixing the two to obtain a mixed sol; orienting the magnetic graphene in the mixed sol using a magnetic orientation device, and then adding an initiator to solidify the mixed sol into a gel; and subjecting the prepared gel to low-temperature pre-carbonization and high-temperature graphitization treatment to obtain a magnetically oriented graphene / carbon composite material.

[0052] The specific steps of the above preparation method are as follows:

[0053] Step 1) preparing a magnetic graphene dispersion and a plant sugar precursor sol, and fully stirring and mixing the two to obtain a mixed sol.

[0054] Step 2) Orient the magnetic graphene in the mixed sol prepared in step 1 using a magnetic orientation device, and then add an initiator to solidify the mixed sol into a gel.

[0055] Step 3) The gel prepared in step 2 is subjected to low-temperature pre-carbonization and high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0056] The specific dosage and process conditions are as follows:

[0057] In step 1), the preparation method of the magnetic graphene dispersion is: graphene oxide, ferrofluid, and water are fully mixed in a mass ratio of (1-20): (3-50): (10-40) to obtain a magnetic graphene dispersion.

[0058] Among them, the graphene oxide is commercial single-layer or multi-layer graphene oxide; the magnetic graphene is graphene oxide attached with iron oxide nanoparticles in ferrofluid.

[0059] The preparation method of the plant sugar precursor sol is as follows: plant sugar, acrylamide, methylene bisacrylamide and water are fully mixed in a mass ratio of (10-100): (1-100): (0.1-10): (50-200) to obtain the plant sugar precursor sol.

[0060] The plant sugar may be one or a combination of glucose, sucrose, starch, fructose, maltose and xylose.

[0061] Specifically, the mass proportion of the magnetic graphene in the mixed sol is 2% to 20%.

[0062] In step 2), if Figure 7 As shown, the magnetic orientation device includes a NdFeB magnet 2, a motor 4, a loading plate 3, and a suspendable glass container 1; the rotating shaft 5 of the motor 4 is connected to the central part of the loading plate 3, the suspendable glass container 1 is arranged above the loading plate 3, two NdFeB magnets 2 are arranged parallel to each other on the loading plate 3, and the NdFeB magnets 2 are symmetrically arranged on both sides of the suspendable glass container 1.

[0063] The process of orienting the magnetic graphene in the mixed sol using the magnetic orientation device is as follows:

[0064] The mixed sol is placed in a suspendable glass container 1, and a motor 4 drives a parallel NdFeB magnet 2 to rotate around the suspendable glass container 1 to generate a rotating magnetic field to orient the magnetic graphene in the mixed sol; the rotation speed is 1 to 50 r / s.

[0065] Specifically, the magnetic orientation device consists of two parallel NdFeB magnets 2, a motor 4 with adjustable speed, an acrylic disc and a hangable glass container 1; the magnetic orientation is driven by the motor 4 to drive the parallel NdFeB magnets 2 to rotate around the hangable glass container 1 to generate a rotating magnetic field.

[0066] Specifically, the initiator is one or a combination of ammonium persulfate, potassium persulfate, azobisisobutyronitrile, and hydrogen peroxide.

[0067] In step 3), the low-temperature pre-carbonization process is as follows: heat treatment for 36 hours at a heating rate of 5°C / h in an air atmosphere; the high-temperature graphene process is as follows: heat treatment for 2 hours at 1800-2800°C in an argon-hydrogen mixed atmosphere.

[0068] On the other hand, the present invention also provides a magnetically oriented graphene / carbon composite material, such as Figure 6 As shown, the magnetically oriented graphene / carbon composite material is composed of a porous carbon matrix 6 and a plurality of magnetically oriented graphene layers 7 arranged alternately and parallelly in the vertical direction inside the porous carbon matrix 6; the porous carbon matrix 6 is formed by connecting carbon nanoparticles converted from plant sugar precursors, and the carbon nanoparticles in the porous carbon matrix 6 are interconnected to form closed pores of micro-nano size; the magnetically oriented graphene layer 7 is formed by overlapping two-dimensional reduced oxide graphene nanosheets.

[0069] like Figure 1 As shown, the magnetically oriented graphene / carbon composite material is a black three-dimensional block with a density of 0.15-0.35 g / cm 3; The main components of the magnetically oriented graphene / carbon composite material are carbon and reduced graphene oxide; in the magnetically oriented graphene / carbon composite material, the two-dimensional magnetically oriented graphene layers 7 are arranged in parallel; in the magnetically oriented graphene / carbon composite material, the porous carbon matrix 6 is composed of carbon nanoparticles formed by the conversion of plant sugar precursors, and the carbon nanoparticles in the porous carbon matrix 6 are interconnected to form closed pores of micro-nano size; the constituent element of the magnetically oriented graphene / carbon composite material is C.

[0070] The magnetically oriented graphene / carbon composite material is anisotropic, has a high thermal conductivity of 10 to 20 W / mk in the horizontal direction, and has a low thermal conductivity of 0.35 to 0.65 W / mk in the vertical direction; the magnetically oriented graphene / carbon composite material has excellent mechanical properties, and the compressive strength can reach up to 43.59 MPa.

[0071] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0072] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0073] Embodiment 1:

[0074] Step 1) 1g of graphene oxide, 3g of ferrofluid, and 10g of water are mixed and stirred evenly to obtain a magnetic graphene dispersion, and then 10g of glucose, 1g of acrylamide, 0.1g of methylene bisacrylamide and 50g of water are mixed and stirred evenly to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 20%.

[0075] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 1 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding ammonium persulfate to solidify the mixed sol into a gel.

[0076] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 2500°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0077] The density of the prepared magnetically oriented graphene / carbon composite material is 0.20 g / cm 3 , the thermal conductivity in the horizontal direction at room temperature is 15W / mk, the thermal conductivity in the vertical direction is 0.42W / mk, and the compressive strength of the material is 43.59MPa. Figure 1 It can be seen that the magnetically oriented graphene / carbon composite material appears as black three-dimensional blocks.

[0078] Depend on Figure 2 It can be seen that in the magnetically oriented graphene / carbon composite material, the reduced graphene oxide overlaps each other to form a parallel two-dimensional magnetically oriented graphene layer 7, and the porous carbon matrix 6 is formed by connecting carbon nanoparticles converted from plant sugar precursors, and the carbon nanoparticles in the porous carbon matrix 6 are connected to each other to form closed pores of micro-nano size. Figure 3 It can be seen that after low-temperature pre-carbonization and high-temperature graphitization, the magnetically oriented graphene / carbon composite material has fewer defects in the Raman spectrum and higher crystallinity. Highly crystalline carbon is beneficial to improving the phonon transmission rate, thereby improving the thermal conductivity of the material, and is also beneficial to improving the mechanical strength of the material. Figure 4 It can be seen that the upper surface temperature of the magnetically oriented graphene / carbon composite material is still relatively low (about 60°C) after being placed on a heating platform at 200°C for 10 minutes, which proves that due to the thermal barrier effect of the magnetically oriented graphene layer 7, the prepared composite material has excellent thermal insulation properties in the direction perpendicular to the magnetically oriented graphene layer 7.

[0079] Embodiment 2:

[0080] Step 1) 1g of graphene oxide, 3g of ferrofluid, and 10g of water are mixed and stirred evenly to obtain a magnetic graphene dispersion, and then 10g of glucose, 1g of acrylamide, 0.1g of methylene bisacrylamide and 50g of water are mixed and stirred evenly to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 10%.

[0081] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 1 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding ammonium persulfate to solidify the mixed sol into a gel.

[0082] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 2500°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0083] Embodiment 3:

[0084] Step 1) 1g of graphene oxide, 3g of ferrofluid, and 10g of water are mixed and stirred to obtain a magnetic graphene dispersion, and then 10g of glucose, 1g of acrylamide, 0.1g of methylene bisacrylamide and 50g of water are mixed and stirred to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 2%.

[0085] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 1 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding ammonium persulfate to solidify the mixed sol into a gel.

[0086] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 2500°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0087] Depend on Figure 5 It can be seen that when other variables are controlled consistently, within the range of 2% to 20% of the mass ratio of magnetic graphene, as the mass ratio of magnetic graphene increases, the ultimate compressive strength of the composite material also increases. This shows that the magnetically oriented graphene layer, as a mechanical reinforcement phase, effectively improves the mechanical strength of the composite material.

[0088] Embodiment 4:

[0089] Step 1) 20g of graphene oxide, 50g of ferrofluid, and 40g of water are mixed and stirred evenly to obtain a magnetic graphene dispersion, and then 100g of sucrose, 100g of acrylamide, 10g of methylene bisacrylamide and 200g of water are mixed and stirred evenly to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 10%.

[0090] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 50 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding potassium persulfate to solidify the mixed sol into a gel.

[0091] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 2200°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0092] Embodiment 5:

[0093] Step 1) 5 g of graphene oxide, 20 g of ferrofluid, and 40 g of water are mixed and stirred to obtain a magnetic graphene dispersion, and then 50 g of starch, 10 g of acrylamide, 2 g of methylene bisacrylamide and 150 g of water are mixed and stirred to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 2%.

[0094] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 25 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding azobisisobutyronitrile to solidify the mixed sol into a gel.

[0095] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 2000°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0096] Embodiment 6:

[0097] Step 1) 10g of graphene oxide, 3g of ferrofluid, and 10g of water are mixed and stirred evenly to obtain a magnetic graphene dispersion, and then 50g of fructose, 1g of acrylamide, 0.1g of methylene bisacrylamide and 50g of water are mixed and stirred evenly to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 15%.

[0098] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 20 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding ammonium persulfate to solidify the mixed sol into a gel.

[0099] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 1800°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0100] Embodiment 7:

[0101] Step 1) 3g of graphene oxide, 3g of ferrofluid, and 15g of water are mixed and stirred evenly to obtain a magnetic graphene dispersion, and then 5g of maltose, 2g of acrylamide, 3g of methylene bisacrylamide and 150g of water are mixed and stirred evenly to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 5%.

[0102] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 1 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding hydrogen peroxide to solidify the mixed sol into a gel.

[0103] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 2800°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0104] Embodiment 8:

[0105] Step 1) 1g of graphene oxide, 3g of ferrofluid, and 10g of water are mixed and stirred to obtain a magnetic graphene dispersion, and then 10g of xylose, 1g of acrylamide, 0.1g of methylene bisacrylamide and 50g of water are mixed and stirred to obtain a plant sugar precursor sol, and then the magnetic graphene dispersion and the plant sugar precursor sol are fully mixed to obtain a mixed sol, wherein the mass proportion of magnetic graphene in the mixed sol is 2%.

[0106] Step 2) placing the mixed sol prepared in step 1 in a magnetic orientation device, adjusting the speed of motor 4 to 1 r / s to generate a rotating magnetic field, magnetically orienting the magnetic graphene in the mixed sol, and then adding ammonium persulfate to solidify the mixed sol into a gel.

[0107] Step 3) placing the gel prepared in step 2 in a heating device, heat treating it in an air atmosphere at a heating rate of 5°C / h for 36 hours for low-temperature pre-carbonization, and then heat treating it in an argon-hydrogen mixed atmosphere at 1800°C for 2 hours for high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

[0108] In summary, the magnetically oriented graphene / carbon composite material prepared by the present invention can realize the oriented and orderly arrangement of the magnetically oriented graphene layer in the composite material matrix by a simple and quick method, which is conducive to simplifying the preparation process of the composite material, shortening the preparation cycle, and reducing the preparation cost. The prepared composite material has excellent compressive strength, excellent thermal conductivity and thermal insulation performance, and can be prepared on a large scale, and has great application potential in thermal management fields such as aerospace, communication base stations and electronic equipment.

[0109] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A magnetically oriented graphene / carbon composite material, characterized in that: The magnetically oriented graphene / carbon composite material is composed of a porous carbon matrix and a plurality of magnetically oriented graphene layers arranged alternately and parallelly in the vertical direction inside the porous carbon matrix; The porous carbon matrix is ​​formed by connecting carbon nanoparticles converted from plant sugar precursors, and the carbon nanoparticles in the porous carbon matrix are connected to each other to form closed pores of micro-nano size; The magnetically oriented graphene layer is formed by overlapping two-dimensional reduced graphene oxide nanosheets.

2. The magnetically oriented graphene / carbon composite material according to claim 1, characterized in that: The magnetically oriented graphene / carbon composite material has anisotropy, and the thermal conductivity in the horizontal direction parallel to the magnetically oriented graphene layer is 10-20 W / mk, and the thermal conductivity in the vertical direction perpendicular to the magnetically oriented graphene layer is 0.35-0.65 W / mk.

3. A method for preparing a magnetically oriented graphene / carbon composite material according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1: preparing a magnetic graphene dispersion and a plant sugar precursor sol, and then stirring and mixing the two to obtain a mixed sol; S2: Orient the magnetic graphene in the mixed sol using a magnetic orientation device, and then add an initiator to solidify the mixed sol into a gel; S3: The gel is subjected to low-temperature pre-carbonization and high-temperature graphitization to obtain a magnetically oriented graphene / carbon composite material.

4. The method for preparing a magnetically oriented graphene / carbon composite material according to claim 3, characterized in that: In S1, the preparation method of the magnetic graphene dispersion is as follows: The graphene oxide, the ferrofluid and the water are mixed in a mass ratio of (1-20): (3-50): (10-40) to prepare a magnetic graphene dispersion; The graphene oxide is a single-layer graphene oxide or a multi-layer graphene oxide; the magnetic graphene is a graphene oxide attached with ferroferric oxide nanoparticles in a ferromagnetic fluid.

5. The method for preparing a magnetically oriented graphene / carbon composite material according to claim 3, characterized in that: In S1, the preparation method of the plant sugar precursor sol is as follows: The plant sugar, acrylamide, methylene bisacrylamide and water are mixed in a mass ratio of (10-100):(1-100):(0.1-10):(50-200) to prepare a plant sugar precursor sol.

6. The method for preparing a magnetically oriented graphene / carbon composite material according to claim 3, characterized in that: The plant sugar is one or more of glucose, sucrose, starch, fructose, maltose and xylose.

7. The method for preparing a magnetically oriented graphene / carbon composite material according to claim 3, characterized in that: The mass proportion of magnetic graphene in the mixed sol is 2% to 20%.

8. The method for preparing a magnetically oriented graphene / carbon composite material according to claim 3, characterized in that: In S2, the initiator is one or more of ammonium persulfate, potassium persulfate, azobisisobutyronitrile and hydrogen peroxide.

9. The method for preparing a magnetically oriented graphene / carbon composite material according to claim 3, characterized in that: In S3, the low-temperature pre-carbonization process is as follows: heat treatment for 36 hours at a heating rate of 5°C / h in an air atmosphere.

10. The method for preparing a magnetically oriented graphene / carbon composite material according to claim 3, characterized in that: In S3, the high temperature graphitization process is as follows: heat treatment at a temperature of 1800-2800° C. for 2 h in an argon-hydrogen mixed atmosphere.

Citation Information

Patent Citations

  • Magnetic graphene-based aerogel material with ordered structure and preparation method thereof

    CN109320286A

  • Preparation method for structurally ordered graphene / Fe3O4 aerogel

    CN110065938A

  • Method for preparing flexible conductive composite material through regulating graphene arrangement by magnetic field

    CN110283450A

  • High-thermal-conductivity graphene composite film and preparation method thereof

    CN114716704A

  • Method for preparing high-orientation-degree graphite film by using small-molecular carbohydrates

    CN116873919A

Cited By

  • Method for preparing fiber electrode by utilizing magnet to induce Fe3O4-coated GO to carry out directional arrangement

    CN119020885A