Surface film for photomask and method for manufacturing the same

By using the recovery layer formed by catecholamines in the photomask surface film to fill the pinholes of the base layer to form a hexagonal aromatic ring with an SP2 covalent bond structure, the problem of insufficient protection of the photomask in the photolithography process is solved. Improved optical properties and mechanical strength, suitable for extreme ultraviolet lithography.

CN110609435BActive Publication Date: 2024-10-11SAMSUNG ELECTRONICS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN201910504878.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-15
Filing Date
2019-06-12
Publication Date
2024-10-11
Estimated Expiration
2039-06-12

AI Technical Summary

Technical Problem

The existing photomask surface film cannot effectively protect the photomask from damage by external contaminants during the photolithography process, and its optical properties, mechanical strength and durability are insufficient, especially in extreme ultraviolet lithography, where the wavelength of the light source is shortened. problem.

Method used

Adopt a surface film structure including a base layer and a recovery layer. The recovery layer is formed by heat treatment of catecholamines to fill the pinholes in the base layer to form a hexagonal aromatic ring with an SP2 covalent bond structure to enhance the optical properties of the film. and mechanical strength.

Benefits of technology

It improves the optical properties, durability and mechanical strength of the surface film, reduces hydrogen damage in the photolithography process, ensures the reliability and durability of the photomask, and is suitable for extreme ultraviolet lithography processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110609435B_ABST
    Figure CN110609435B_ABST
Patent Text Reader

Abstract

Disclosed are a pellicle for a photomask and a method for manufacturing the same. The pellicle for a photomask includes a pellicle sheet. The pellicle sheet includes a base layer having a first surface and a second surface opposite to the first surface, and a first recovery layer covering the first surface of the base layer. SP between carbon atoms included in the first recovery layer 2 The content of covalent bonds is less than or equal to the SP between carbon atoms contained in the base layer. 2 Covalent bond content.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2018-0069205 filed on June 15, 2018 in the Korean Intellectual Property Office, the entire contents of which are hereby incorporated by reference. Technical Field

[0003] The inventive concepts relate to pellicles for photomasks and / or methods of making the same. Background Art

[0004] The pellicle for photomask can be provided on the photomask in the form of a film to protect the photomask from external contaminants (e.g., dust, photoresist, and / or the like) during photolithography, such as EUV photolithography. The pellicle for photomask should have high transmittance for light used in the photolithography process and other characteristics such as high thermal radiation tolerance, mechanical strength, uniformity, durability, and stability. As the line width of semiconductor devices and electronic circuits has been reduced, the wavelength of light used in the photolithography process has become shorter and the development of suitable pellicle materials based on the light source used in the photolithography process is underway. Summary of the invention

[0005] Some example embodiments of the inventive concepts provide a pellicle for a photomask having excellent optical characteristics, durability, and mechanical strength.

[0006] Some example embodiments of the inventive concepts provide methods of manufacturing a pellicle for a photomask having excellent optical characteristics, durability, and mechanical strength.

[0007] According to some example embodiments of the inventive concept, a pellicle for a photomask includes a pellicle membrane. The pellicle membrane includes a base layer having a first surface and a second surface opposite to the first surface, and a first recovery layer covering the first surface of the base layer. SP between carbon atoms included in the first recovery layer 2 The content of covalent bonds is less than or equal to SP between carbon atoms contained in the base layer. 2 Covalent bond content.

[0008] According to some example embodiments of the inventive concept, a method of manufacturing a pellicle for a photomask includes providing a pellicle sheet and transferring the pellicle sheet to a frame. Providing the pellicle sheet includes forming a base layer having a first surface and a second surface opposite to the first surface, coating a second carbonaceous material on the first surface of the base layer, and performing a first heat treatment process at a first process temperature to form a first recovery layer bonded to the base layer. The second carbonaceous material includes catecholamine.

[0009] According to some example embodiments of the inventive concept, a pellicle for a photomask includes a pellicle sheet. The pellicle sheet includes a base layer having a first surface and a second surface opposite to the first surface, a first recovery layer covering the first surface of the base layer, and a support layer covering the second surface of the base layer. The base layer, the first recovery layer, and the support layer each include carbon atoms. SP between carbon atoms included in the first recovery layer 2 The content of covalent bonds is less than or equal to SP between carbon atoms contained in the base layer. 2 Covalent bond content. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 illustrating a cross-sectional view showing a pellicle for a photomask according to some example embodiments of the inventive concepts,

[0011] Figure 2 Description Display Figure 1 An enlarged view of section P1;

[0012] Figure 3-6 Explain the carbon bond structure of atomic layers at different heights;

[0013] Figure 7 A flowchart showing a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts is illustrated;

[0014] Figure 8 and 10 illustrating a cross-sectional view showing a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts;

[0015] Fig. 9 Description Display Figure 8 An enlarged view of section P2;

[0016] Fig.11 Description Display Fig.10 An enlarged view of section P3;

[0017] Fig.12 perspective views illustrating steps shown in a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts;

[0018] Fig.13A optical images illustrating base layers fabricated according to some example embodiments of the inventive concepts;

[0019] Fig. 13B Instructions for applying catecholamines to Fig.13A An optical image obtained after that on the base layer;

[0020] Fig. 13CDescription: Through heat treatment Fig. 13B The optical image obtained after the catecholamines form a recovery layer;

[0021] Fig.14 illustrates graphs showing Raman spectra of a defect-free graphite layer and a pellicle sheet manufactured by a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts;

[0022] Fig.15 The illustration shows a cross-sectional view of a pellicle for a photomask according to some example embodiments of the inventive concepts.

[0023] Fig.16 Description Display Fig.15 An enlarged view of section P4;

[0024] Figure 17-19 and 21-23 illustrate cross-sectional views showing pellicles for photomasks according to some example embodiments of the inventive concepts;

[0025] Fig. 20 Description Display Fig.19 An enlarged view of section P5;

[0026] Fig.24 illustrating a cross-sectional view of a reticle including a pellicle according to some example embodiments of the inventive concepts; and

[0027] Fig.25 Schematic diagrams showing a photolithography process using a mask including a pellicle according to some example embodiments of the inventive concepts are illustrated. DETAILED DESCRIPTION

[0028] Some example embodiments of the inventive concept will now be described in detail with reference to the accompanying drawings to help clearly explain the inventive concept.

[0029] When a value or equation is used herein without any further modification, it is intended that the associated value includes tolerances such as engineering tolerances around the stated value or equation known to those of ordinary skill in the art. When a range is stated, the range includes all values ​​therein, for example in increments of 0.1%.

[0030] Figure 1 The illustration shows a cross-sectional view of a pellicle for a photomask according to some example embodiments of the inventive concepts. Figure 2 Description Display Figure 1 An enlarged view of section P1. Figure 3-6 Illustrate the carbon bond structure of atomic layers at different heights.

[0031] Reference Figure 1, a pellicle 50 for a photomask may include a pellicle film sheet 20 and a pellicle frame 30 attached to the edge of the pellicle film sheet. The pellicle 50 may be applied to, for example, used in an EUV mask for extreme ultraviolet (EUV) lithography. The pellicle film sheet 20 may include a base layer 1 and a recovery layer 3. The base layer 1 may have a first surface 1a and a second surface 1b opposite to each other. The recovery layer 3 may be on the first surface 1a of the base layer 1. The pellicle frame 30 may be on the second surface 1b of the base layer 1. The base layer 1 and the recovery layer 3 may both contain carbon. The base layer 1 may be or may include, for example, at least one of a graphene thin layer or a graphite thin layer. The recovery layer 3 may have a structure similar to that of the base layer 1. The bond structure between carbon atoms contained in the base layer 1 may mainly include a SP as a planar bond structure. 2 covalent bonds, and secondly SP as a tetrahedral bond structure 3 Covalent bonds. For example, in base layer 1, SP 2 Covalent bond to SP 3 The content ratio of covalent bonds may be about 70:30 to 90:10 or about 84:16 to 83:17. The film frame 30 may have, for example, one of a regular square shape and a rectangular shape each having two pairs of parallel sides. The film frame 30 may include a metal or an alloy of the metal such as aluminum, zinc, magnesium, stainless steel, molybdenum, zirconium, tungsten, or a combination thereof, or diamond-like carbon (DLC), and the metal or the alloy of the metal may be treated by anodizing technology.

[0032] Reference Figure 1 and 2 , at least one pinhole or hole 1r may exist on the first surface 1a of the base layer 1. The recovery layer 3 may fill the pinhole 1r while covering the first surface 1a of the base layer 1. The recovery layer 3 may have a structure that is the same as or similar to that of graphene or graphite. The bond structure between carbon atoms included in the recovery layer 3 may mainly include SP as a planar bond structure. 2 covalent bonds, and secondly SP as a tetrahedral bond structure 3 Covalent bond. SP between carbon atoms contained in the recovery layer 3 2 The content / density of covalent bonds may be less than or equal to the SP between carbon atoms included in the base layer 1. 2 The recovery layer 3 may include at least one of nitrogen, hydrogen, or oxygen, or a combination thereof, or a sub-combination thereof. The content / density of at least one of nitrogen, hydrogen, or oxygen contained in the recovery layer 3 may be greater than the content / density of at least one of nitrogen, hydrogen, or oxygen contained in the base layer 1.

[0033] The base layer 1 may include first and second base atomic layers Ala and Alm therein. The first and second base atomic layers Ala and Alm may include a first base atomic layer Ala and a second base atomic layer Alm spaced apart from the first base atomic layer Ala in a direction corresponding to the C-axis direction. The pinhole 1r may be formed in the second base atomic layer Alm. The C-axis direction may be perpendicular to the surfaces of the first and second base atomic layers Ala and Alm, or may be a thickness direction of the base layer 1. Figure 3 and 5 As shown in , the first and second base atomic layers A1a and Alm may each include first carbon atoms C1 forming a hexagonal structure.

[0034] The recovery layer 3 may include recovery atomic layers Cln spaced apart from each other in the C-axis direction. Figure 4 As shown in , the recovery atomic layers Cln may each include second carbon atoms C2 forming a hexagonal structure. The carbon bonds in the first and second base atomic layers A1a and Alm and the recovery atomic layer Cln may mainly include SPs oriented in a direction perpendicular to the C-axis direction. 2 Covalent bonds. The carbon bonds in the first and second base atomic layers A1a and Alm and the recovery atomic layer Cln may slightly include SP oriented in a direction parallel to the C axis. 3 Covalent bond. SP between carbon atoms contained in the recovery layer 3 3 The content / density of covalent bonds may be greater than the SP between carbon atoms included in the base layer 1. 3 The content / density of covalent bonds.

[0035] like Figure 5 As shown in FIG. 1 , the second base atomic layer Alm may include a pinhole 1r, which is a hollow region in which the first carbon atom C1 does not exist. Dangling bonds DB and / or broken bonds of the first carbon atom C1 may exist on the sidewalls of the pinhole 1r. When the base layer 1 excluding the recovery layer 3 is used as a pellicle film, the base layer 1 may suffer from the combination of the dangling bonds DB and the gas supplied in the photolithography process, such as hydrogen (for example, when the first carbon atom C1 is evaporated into methane (CH 4 ) may be caused by damage such as partial loss of an aperture. Therefore, the damaged pellicle film may not be able to protect the photomask, and foreign matter may be attached to the photomask, and as a result, the photolithography process may not be reliably performed.

[0036] According to the inventive concept, the pinhole 1r can be filled with the recovery layer 3 to remedy or reduce the effect of defects such as the pinhole 1r of the base layer 1. Figure 6 As shown in FIG. 1 , the second carbon atom C2 included in the recovery atomic layer Cln of the recovery layer 3 may be bonded to the first carbon atom C1 included in the second base atomic layer Alm, and as a result, a layer having SP may be formed.2 The hexagonal aromatic ring of the covalent bond structure. The dangling bond DB of the pinhole 1r can then be removed to prevent or reduce the influence of damage caused by hydrogen in the photolithography process. Therefore, the photolithography process can be performed more reliably and the surface film 50 can be increased in life or durability. The recovery atomic layer Cln can partially have SP in the pinhole 1r. 3 Covalent bond structure.

[0037] In some example embodiments, because the surface film 50 for a photomask includes a recovery layer 3 containing atoms having a structure similar to those of the atoms of the base layer 1, or because the recovery layer 3 has a carbon bond structure that is the same as or similar to that of the base layer 1, such as a graphene thin layer, the surface film 50 may have optical, physical, and / or chemical properties similar to those of the base layer 1.

[0038] Figure 7 A flow chart showing a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts is illustrated. Figure 8 and 10 A cross-sectional view illustrating a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts is illustrated. Fig. 9 Description Display Figure 8 An enlarged view of section P2. Fig.11 Description Display Fig.10 An enlarged view of section P3. Fig.12 Illustrations illustrate perspective views showing steps in a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts.

[0039] Reference Figure 7-9, a first carbonaceous material may be provided to form a base layer 1 including pinholes 1r (S10). The base layer 1 may be formed using a deposition process such as thermal chemical vapor deposition (TCVD), plasma enhanced chemical vapor deposition (PECVD), microwave enhanced chemical vapor deposition (MECVD), inductively coupled plasma chemical vapor deposition (ICPCVD), low pressure chemical vapor deposition (LPCVD), atomic layer deposition (ALD), chemical vapor deposition (CVD), and / or molecular layer deposition (MLD). The above-mentioned plasma may be generated by radio frequency (RF), alternating current (AC) frequency, or direct current (DC) discharge. For example, a vapor of a first carbonaceous material may be provided on a catalytic metal substrate 40 to grow graphene or a graphite thin layer. The catalytic metal substrate 40 may mainly include carbon-adsorbing transition metals such as nickel, copper, iron, or cobalt, and may further include precious metals such as gold, platinum, or silver. When the base layer 1 is formed by PECVD using plasma, the PECVD may be performed at a relatively low process temperature of about 300-700°C. When plasma is not used in the deposition process for forming the base layer 1, the catalytic metal substrate 40 or a chuck (not shown) supporting the catalytic metal substrate 40 may be at a temperature of about 1000°C or higher. The first carbon-containing material may be or may include, for example, at least one of alkanes, alkenes, and alkynes each containing 1-10 carbon atoms. When carbon bonds in the first carbon-containing material are broken during the deposition process, and then carbon atoms derived from the broken carbon bonds are provided on the surface of the catalytic metal substrate 40, graphene or a graphite layer may be grown from carbon atoms arranged to follow the crystal planes of the surface of the catalytic metal substrate 40. The base layer 1 may be formed to have a thickness of, for example, about 0.34-50nm. The base layer 1 may include a plurality of base atomic layers Ala and Alm, and further include at least one pinhole 1r on its surface. The description of the base atomic layers Ala and Alm may be the same as that regarding Figure 3 and 5 The descriptions discussed are the same or similar. Figure 5 As shown in , a dangling bond DB may exist in the pinhole 1r.

[0040] Reference Figure 7 , 10 , and 11, the second carbon-containing material may be coated on the base layer 1 to fill the pinholes 1r (S20). The coating of the second carbon-containing material may form a second carbon-containing material layer 3c that not only fills the pinholes 1r but also covers the first surface 1a of the base layer 1. The second carbon-containing material easily coats and fully wets the base layer 1 to successfully fill the pinholes 1r. After the heat treatment process, the second carbon-containing material may be decomposed to react with the first carbon atoms (see Figure 3 C1) forms SP 2Covalent bond. The second carbonaceous material may be or may include a polymer or compound containing carbon and at least one of nitrogen, oxygen, and hydrogen. The second carbonaceous material may be or may include, for example, catecholamines. Catecholamines may include dopamine (DA), polydopamine (PD), norepinephrine, or epinephrine. Catecholamines may be polymers of polyethyleneimine (PEI) and pyrogallol (PG). The second carbonaceous material may be at least one of fullerenes, carbon black, activated carbon, charcoal, carbon nanobelts, graphene quantum dots, graphene oxide, and nanodiamonds. The second carbonaceous material may exclude, i.e. may not include, aromatic compounds having two or more benzene rings. The second carbonaceous material may be used alone or in the form of a solution with a solvent. Catecholamines may be formed by mixing and polymerizing polyethyleneimine (PEI) and pyrogallol (PG). Water may be used as a solvent.

[0041] As an example, the first solution may be prepared to include polyethyleneimine (PEI), pyrogallol (PG), and water. The preparation of the first solution may be as follows. First, polyethyleneimine and water may be mixed to prepare a first preliminary solution in which polyethyleneimine is dissolved in water. The first preliminary solution may have a polyethyleneimine concentration of about 1.25-20% by weight. Next, pyrogallol and water may be mixed to prepare a second preliminary solution in which pyrogallol is dissolved in water. The second preliminary solution may have a pyrogallol concentration of about 0.0125-0.2M. The first solution may be prepared by mixing the first preliminary solution and the second preliminary solution in a volume ratio of 1:1. The first solution may include catecholamines formed by polymerization of polyethyleneimine and pyrogallol. The first solution may be applied to the base layer 1. The first solution may be applied to the base layer 1 using a spin coating process. The spin coating process may be performed, for example, at about 2,500-7,000rpm for about 30-240 seconds.

[0042] Reference Figure 7 , 1 , and 2, after coating the second carbonaceous material, a heat treatment process may be performed at a first process temperature to form a recovery layer 3 (S30). The first process temperature may be, for example, in the range of about 900° C. to about 2,000° C. The heat treatment process may break bonds between carbon atoms and nitrogen, hydrogen, and oxygen atoms contained in the second carbonaceous material, so that nitrogen, hydrogen, and oxygen atoms may be removed and the remaining carbon atoms (corresponding to Figure 4 The second carbon atom C2 of the base layer 1 can be connected with the first carbon atom C2 of the base layer 1 Figure 3The base layer 1 may be used as a seed layer in the heat treatment process. The recovery layer 3 may have a thickness of about 0.5-10 nm. Through the above process, the pellicle membrane 20 may be formed to include the base layer 1 and the recovery layer 3. An inert gas such as argon may be supplied during the heat treatment process. Hydrogen may be additionally supplied during the heat treatment process. The flow ratio of argon to hydrogen may be, for example, about 90:10 to 99:1.

[0043] The recovery layer 3 finally formed by the heat treatment process may have the same Figure 3 , 4 , and 6. For example, the bond structure between carbon atoms included in the recovery layer 3 may mainly include SP as a planar bond structure. 2 Covalent bonds, and slightly including SP as a tetrahedral bond structure 3 Covalent bond. SP between carbon atoms contained in the recovery layer 3 2 The content / density of covalent bonds may be less than or equal to the SP between carbon atoms included in the base layer 1. 2 The content / density of covalent bonds. Nitrogen, hydrogen, and oxygen contained in the second carbonaceous material may not be completely removed during the heat treatment process, but may be partially retained in the recovery layer 3. The recovery layer 3 may then include at least one of nitrogen, hydrogen, or oxygen, or a subcombination thereof, or a combination thereof. The content / density of nitrogen, hydrogen, and / or oxygen contained in the recovery layer 3 may be greater than the content / density of nitrogen, hydrogen, and / or oxygen contained in the base layer 1.

[0044] The pellicle membrane 20 may be separated from the catalytic metal substrate 40. The separation of the pellicle membrane 20 may be performed in a first liquid. For example, the catalytic metal substrate 40 on which the pellicle membrane 20 is formed may be provided in the first liquid, and then the pellicle membrane 20 may be separated from the catalytic metal substrate 40. The first liquid may be or may include, for example, one or more of an aqueous solution of ferric chloride, an aqueous solution of ammonium persulfate, an aqueous solution of cerium ammonium nitrate, and an aqueous solution of dimethylformamide. The separated pellicle membrane 20 may be additionally subjected to a cleaning process using a second liquid. The second liquid may include at least one of deionized water, nitric acid, hydrochloric acid, acetic acid, hydrofluoric acid, aqua regia, ethanol, methanol, and isopropanol.

[0045] Reference Figure 1 and 12, the separated pellicle membrane sheet 20 can be transferred to the pellicle frame 30. The transfer process can be performed in the third liquid 24. For example, the third liquid 24 can be provided in the water tank 22, and the pellicle membrane sheet 20 can be floated on the third liquid 24. The pellicle frame 30 can be lifted from the inside of the third liquid 24 and then attached to the pellicle membrane sheet 20. The third liquid 24 can be at least one of deionized water and alcohol. The alcohol can include at least one of methanol, ethanol, and isopropanol. The pellicle frame 30 and the pellicle membrane sheet 20 can be attached to each other, such as directly attached, without any glue material between the pellicle frame 30 and the pellicle membrane sheet 20 by, for example, van der Waals force. After that, the pellicle frame 30 and the pellicle membrane sheet 20 can be dried. Alternatively, the pellicle membrane sheet 20 can be attached to the pellicle frame by a dry method performed under atmospheric or vacuum conditions, not in the third liquid 24. At this stage, a heat treatment process can be additionally performed or an adhesive can be used.

[0046] In some example embodiments, the recovery layer 3 can be formed by using catecholamine, which is easily coated on the base layer 1, fills the pinholes or holes 1r with little to no effort, and combines with the base layer 1 to successfully form regular hexagonal aromatic rings. In this way, a pellicle 50 for a photomask having increased surface uniformity of the pellicle film 20 and having excellent optical characteristics, durability, and mechanical strength can be provided.

[0047] Fig.13A Optical images of base layers fabricated according to some example embodiments of the inventive concepts are illustrated. Fig.13A The base layer 1 may be a graphene or graphite sheet. The base layer 1 may have a defect-free area (in Fig.13A ), there is no pinhole 1r on the defect-free area and the surface of the defect-free area is relatively uniform and neat.

[0048] Fig. 13B Instructions for applying catecholamines to Fig.13A The optical image obtained afterwards on the base layer. Fig. 13C Description By Fig. 13B Optical image obtained after heat treatment of catecholamine to form a recovery layer. Fig. 13C As shown in , the recovery layer 3 has a uniform and neat surface and has no pinholes 1r. Fig. 13C Display and Fig.13A The recovery layer 3 may have a surface that is the same as or similar to that of a graphene or graphite thin layer that has no defects such as the pinhole 1r.

[0049] Fig.14Graphs showing a first Raman spectrum A of a defect-free graphite layer and a second Raman spectrum B of a pellicle sheet manufactured by a method of manufacturing a pellicle for a photomask according to some example embodiments of the inventive concepts are illustrated.

[0050] Reference Fig.14 The surface film 20 may have a second Raman spectrum B, wherein the intensity ratio of the D peak to the G peak, or the D / G intensity ratio, is about 0-1, or about 0.06-0.17. The G peak may appear at about 1580 cm -1 The Raman shift is caused by the SP 2 The stretching vibration mode between carbon-carbon bonds of the covalent bond structure corresponds to the vibration mode and provides information on whether a hexagonal aromatic ring is included. The D peak may appear at about 1340-1350 cm -1 The Raman shift is caused by defects such as SP 3 Carbon atoms and carbon vacancies in covalent bond structure. Fig.14 The carbon bonds in the surface film 20 may have a ratio of SP 3 SP with relatively more covalent bond structures 2 Covalent bond structure. Fig.14 It also shows that the second Raman spectrum B of the pellicle sheet 20 may have a shape similar to the first Raman spectrum A of the defect-free graphite thin layer. For example, the base layer 1 and the recovery layer 3 included in the pellicle sheet 20 may each have a structure similar to that of the defect-free graphite thin layer.

[0051] The pellicle film 20 may have an absorption coefficient (or extinction coefficient) of about 0.01 or less, or about 0.0069-0.01 for light having a wavelength of about 13.5 nm. The term "absorption coefficient" or "extinction coefficient" may mean a coefficient indicating the degree of reduction in the amount of wavelength (light) or radiation when passing through a certain layer. Since the pellicle film 20 has an absorption coefficient (or extinction coefficient) of about 0.01 or less, the pellicle film 20 may not absorb or may absorb very little light. Therefore, the pellicle film 20 may be applicable to EUV lithography processes and may contribute to the formation of ultra-fine patterns, such as ultra-fine patterns used in semiconductor manufacturing.

[0052] The pellicle membrane 20 may have a tensile strength of, for example, about 200 MPa to about 3 GPa. The tensile strength of about 200 MPa to about 3 GPa may refer to the tensile strength in the horizontal direction, which is, for example, perpendicular to the horizontal direction. Figure 2 In such a case, tearing or wrinkling of the pellicle membrane 20 can be prevented or significantly reduced, which can lead to a reduction in process faults (failures).

[0053] Fig.15 The illustration shows a cross-sectional view of a pellicle for a photomask according to some example embodiments of the inventive concepts. Fig.16 Description Display Fig.15 An enlarged view of section P4.

[0054] Reference Fig.15 and 16 The pellicle 50a for the photomask may include a pellicle sheet 20a, and Figure 1 Compared with the pellicle membrane 20 in the embodiment of the present invention, it further includes a support layer 5 on the second surface 1b of the base layer 1. The support layer 5 may have a crystal structure different from the crystal structure of the base layer 1. The base layer 1 may have a tensile strength in the C-axis direction that is smaller than the tensile strength in the thickness direction (e.g., C-axis direction) of the support layer 5. The support layer 5 may be or may include, for example, at least one of diamond-like carbon (DLC) and carbon nanotubes. Fig.16 An example is shown in which the support layer 5 is a carbon nanotube. The carbon nanotube has a cylindrical shape and thus has a tensile strength in the C-axis direction (e.g., in a direction perpendicular to the longitudinal direction of the carbon nanotube) greater than that of graphene or a graphite sheet. The carbon bonds in the carbon nanotube may form SP 2 The covalent bond structure forms a regular hexagonal aromatic ring. The recovery layer 3 and the base layer 1 can be connected with Figure 1-6 The SP between carbon atoms contained in the recovery layer 3 is the same as or similar to those discussed above. 2 The content / density of covalent bonds may be less than the SP between carbon atoms included in the support layer 5. 2 The content / density of covalent bonds. The content / density of nitrogen, hydrogen, and / or oxygen contained in the recovery layer 3 may be greater than the content / density of nitrogen, hydrogen, and / or oxygen contained in the support layer 5. The support layer 5 may include at least one of iron, cobalt, and nickel.

[0055] The following describes the production Fig.15 The process of the surface membrane 20a. Figure 7-11 As discussed, a base layer 1 and a recovery layer 3 may be formed. The base layer 1 and the recovery layer 3 may be separated from the catalytic metal substrate 40. The support layer 5 may be formed separately. When the support layer 5 includes carbon nanotubes, arc discharge, thermal deposition, or plasma deposition may be performed to form the support layer 5 on the second catalytic metal substrate. The second catalytic metal substrate may be or may include at least one of iron, cobalt, and nickel. The support layer 5 may be separated from the second catalytic metal substrate. At this stage, at least one of the iron, cobalt, and nickel constituting the second catalytic metal substrate may remain on the support layer 5. The support layer 5 may therefore include at least one of iron, cobalt, and nickel. The support layer 5 may be placed on the second surface 1b of the base layer 1, and a heat treatment process may be performed at a second process temperature. The second process temperature may be less than about Figure 7 The second process temperature may be in the range of, for example, about 100° C. to about 300° C. Alternatively, similar to the first process temperature discussed above, Fig.12 As discussed, the support layer 5 and the base layer 1 may be attached to each other in a liquid. In this case, the support layer 5 and the base layer 1 may be bonded to each other by van der Waals forces.

[0056] Figure 17-19 and 21 - 23 illustrate cross-sectional views showing pellicles for photomasks according to some example embodiments of the inventive concepts. Fig. 20 Description Display Fig.19 An enlarged view of section P5.

[0057] Reference Fig.17 The pellicle 50b for the photomask may include a pellicle sheet 20b, which is further Fig.15 The recovery layer 3 includes a capping layer 7. The capping layer 7 may include at least one of boron, boron carbide, and boron nitride. The capping layer 7 may have a function of preventing or reducing the possibility of a reaction between hydrogen supplied in a photolithography process and the surface of one of the recovery layer 3 and the base layer 1. Other structural features may be the same as those described above. Fig.15 The same or similar to those discussed.

[0058] Reference Fig.18 The pellicle 50c for the photomask may include a pellicle sheet 20c, which is further Fig.15 The recovery layer 3 includes a first capping layer 7a and a Fig.15 The second capping layer 7b is included below the support layer 5. The first and second capping layers 7a and 7b may each include at least one of boron, boron carbide, and boron nitride.

[0059] Alternatively, the support layer 5 may be excluded so that the second capping layer 7b may be attached, for example directly, to the second surface 1b of the base layer 1 .

[0060] Reference Fig.19 and 20 The pellicle 50d for the photomask may include a pellicle sheet 20d, which is further Fig.17 The base layer 1 and the support layer 5 include a second recovery layer 3 b between them. Fig.19 The first recovery layer 3a may correspond to Fig.17 The recovery layer 3 of the base layer 1 may also be formed with a lower pinhole 1rb on the second surface 1b of the base layer 1. The base layer 1 may further include a third base atomic layer Almb adjacent to the second surface 1b. The lower pinhole 1rb may be formed in the third base atomic layer Almb. The third base atomic layer Almb may have Figure 5 The second recovery layer 3b may fill the lower pinhole 1rb. The second recovery layer 3b may be similar to the carbon bond structure of the second basic atomic layer Alm discussed above. Figure 1-6The second recovery layer 3b may be the same or similar to the recovery layer 3 discussed above. For example, the second recovery layer 3b may include a second recovery atomic layer Clnb. The second recovery atomic layer Clnb may have the same Figure 4 The carbon bond structure of the recovery atomic layer Cln discussed above is the same as or similar to the carbon bond structure of the recovery atomic layer Cln. For example, the second recovery layer 3b can remedy defects such as the lower pinhole 1rb. Figure 6 Similar to the description, the second carbon atom C2 included in the second recovery atomic layer Cln of the second recovery layer 3b may be bonded to the first carbon atom C1 included in the third base atomic layer Almb, and as a result, a structure having SP 2 The hexagonal aromatic ring of the covalent bond structure. Thus, the dangling bond DB of the pinhole 1rb can be removed to prevent or reduce the influence of damage caused by hydrogen in the photolithography process. The SP between the carbon atoms included in the second recovery layer 3b 2 The content / density of covalent bonds may be less than or equal to the SP between carbon atoms included in the base layer 1. 2 The content / density of covalent bonds. The content / density of nitrogen, hydrogen, and / or oxygen contained in the second recovery layer 3b may be greater than the content / density of nitrogen, hydrogen, and / or oxygen contained in the base layer 1. The formation of the second recovery layer 3b may be related to Figure 7 The formation of the recovery layer 3 discussed is the same or similar.

[0061] Reference Fig.21 The pellicle 50e for the photomask may include a pellicle sheet 20e, which is further Fig.19 The first recovery layer 3a includes a first cover layer 7a and a Fig.19 The support layer 5 includes a second capping layer 7b below. Other structural features may be the same or similar to those discussed above.

[0062] Reference Fig. 22 The pellicle 50f for the photomask may include a pellicle sheet 20f. Fig.21 The pellicle membrane 20e of FIG. 1 is different in that the support layer 5 is interposed between the first recovery layer 3a and the first cover layer 7a, rather than between the second recovery layer 3b and the second cover layer 7b. Other structural features may be the same or similar to those discussed above.

[0063] Reference Fig.23 , the pellicle 50g for the photomask may include a pellicle sheet 20g, wherein a first recovery layer 3a and a first capping layer 7a are sequentially stacked on a first surface 1a of a base layer 1. The pellicle sheet 20g may further include a second base layer 10. A support layer 5, a second base layer 10, a second recovery layer 3b, and a second capping layer 7b may be sequentially provided on a second surface 1b of the base layer 1. The base layer 1 may be referred to as a first base layer. The first and second base layers 1 and 10 may each be related to Figure 1-6The base layer 1 discussed is the same or similar.

[0064] Fig.24 The illustration shows a cross-sectional view of a reticle including a pellicle according to some example embodiments of the inventive concepts.

[0065] Reference Fig.24 , the mask plate 70 may include a photomask 60, for example, Figure 1 The film 50 is attached to the photomask 60. The photomask 60 may include a mask substrate 61 and a mask pattern 63 on the mask substrate 61. The shape, size, and spacing of the mask pattern 63 may be only examples and may be varied. The mask substrate 61 may include, for example, quartz. The mask substrate 61 may include a chromium nitride layer, a quartz layer, and / or a ruthenium capping layer. Molybdenum layers and silicon layers stacked alternately and repeatedly may be provided between the quartz layer and the ruthenium capping layer. The mask pattern 63 may include a tantalum-based absorber (absorber) and an anti-reflection layer on the absorber.

[0066] Fig.24 The display mask 70 includes Figure 1 The surface film 50, but the mask 70 may include about Fig.15 , 17 -19, and 21-23, any of the surface films 50a-50g discussed in place of the surface film 50.

[0067] Fig.25 Schematic diagrams showing a photolithography process using a mask including a pellicle according to some example embodiments of the inventive concepts are illustrated.

[0068] Reference Fig.25 According to some example embodiments of the inventive concept, a reflective lithography process may be performed. In the reflective lithography process, a mask 70 having a pellicle 50 attached thereto may be loaded downward on a reticle stage 140 of a reflective lithography system 100. In addition to the reticle stage 140, the reflective lithography system 100 further includes a light source 110, an illumination mirror system 120, a cover 160, a projection mirror system 170, and a wafer stage 180.

[0069] The light source 110 may generate extreme ultraviolet (EUV) radiation. Light having a wavelength of about 13.5 nm, for example, extreme ultraviolet (EUV) radiation may be generated from the light source 110 using plasma generated when a carbon dioxide laser is irradiated onto a small amount of tin (Sn) droplets. The light source 110 may include a light collector 115. The light collector 115 may collect EUV radiation generated from the light source 110 and may control the EUV radiation to move in a certain single direction. The EUV radiation generated from the light source 110 may pass through the light collector 115 and may then be irradiated onto the illumination mirror system 120.

[0070] The illumination mirror system 120 may include a plurality of illumination mirrors 121, 122, 123, and 124. The illumination mirrors 121-124 may be configured to converge EUV radiation so that the possibility of EUV radiation being lost from the mirror radiation path can be prevented or reduced. The illumination mirrors 121-124 may also be configured to control the EUV radiation to have a generally uniform intensity distribution. Therefore, the illumination mirrors 121-124 may each include a concave lens or a convex lens to variously change the path of the EUV radiation. The illumination mirror system 120 may shape the EUV radiation into a square, circular, or strip-shaped EUV radiation, which may be transmitted to the mask stage 140.

[0071] The mask stage 140 may load the mask 70 on the bottom surface and move in the horizontal direction. Fig.25 The mask stage 140 may include an electrostatic chuck (ESC). The mask 70 may be placed on the lower surface of the mask stage 140 so that the mask pattern side of the mask 70 may face downward.

[0072] The hood 160 may be below the reticle stage 140. The hood 160 may include a slit 162 and a plate 164. The slit 162 may have an opening (aperture) shape. The slit 162 may shape the EUV radiation delivered from the illumination mirror system 120 to the reticle 70 on the reticle stage 140. The EUV radiation from the illumination mirror system 120 may pass through the slit 162 and then may be irradiated on the reticle 70 on the reticle stage 140. The EUV radiation reflected from the reticle 70 on the reticle stage 140 may pass through the slit 162 and travel to the projection mirror system 170. The plate 164 may block the EUV radiation irradiated on the area other than the slit 162. Therefore, the hood 160 may allow a portion of the EUV radiation to pass through the slit 162, and another portion of the EUV radiation may be blocked using the plate 164. The slits 162 may allow passage of EUV radiation reflected from the reticle 70 placed on the bottom surface of the reticle stage 140 .

[0073] The projection mirror system 170 may receive EUV radiation that has been reflected from the reticle 70 and passed through the slit 162, and may transmit the EUV radiation to the wafer 190 on the wafer stage 180. The projection mirror system 170 may include a plurality of projection mirrors 171, 172, 173, 174, 175, and 176. The EUV radiation incident on the wafer 190 through the projection mirrors 171-176 may have information about a virtual aerial image of the optical pattern on the reticle 70. The EUV radiation irradiated on the wafer 190 may maintain its shape when passing through the slit 162. The plurality of projection mirrors 171-176 may correct various deviations.

[0074] The wafer stage 180 can accommodate the wafer 190 and move in the horizontal direction. Fig.25 1. Wafer stage 180 may move in the direction of the arrow shown in FIG. 1. Wafer stage 180 may move in the same direction and at the same rate as reticle stage 140 at the same time. For example, wafer stage 180 may move in a step-and-scan manner. EUV radiation irradiated from projection mirror system 170 may have a focus located on the surface of wafer 190. For example, a photoresist layer having a predetermined thickness may be provided on wafer 190, and the focus of the EUV radiation may be located inside the photoresist layer.

[0075] Reference Fig.24 and 25 , pellicle 50 may protect photomask 60 from contamination caused by particles during a photolithography process, and even when pellicle 50 is contaminated on its surface with foreign matter that misaligns the EUV radiation focus, formation of a photoresist pattern may not be affected.

[0076] As the photolithography process continues, the pellicle membrane 20 may change in pressure and temperature. The pellicle membrane 20 may locally bulge downward due to the change in its volume. The distance d1, for example, the maximum distance between the normally flat bottom surface of the pellicle membrane 20 and the maximally convex bottom surface of the pellicle membrane 20, may be less than or equal to, for example, about 500 μm.

[0077] During the photolithography process, hydrogen gas may be supplied to remove defects (e.g., photoresist residues) adhered to the surfaces of the mirrors 121-124 and 171-176. In the case where the pellicle membrane 20 does not include the recovery layer 3, the pellicle membrane 20 may suffer damage caused when hydrogen atoms are bonded to dangling bonds DB in the pinholes 1r. In some example embodiments of the inventive concept, since the pellicle membrane 20 includes the recovery layer 3 filling the pinholes 1r, the pellicle membrane 20 may not be damaged or may be reduced in damage.

[0078] exist Fig.25 , the path of EUV radiation is conceptually illustrated to help clearly understand the inventive concept.

[0079] According to some example embodiments of the inventive concept, a pellicle for a photomask may include a recovery layer to remedy or reduce the effects of defects such as pinholes or holes that may exist on a base layer. The recovery layer may fill the pinholes or holes so that it may be possible to prevent or reduce the possibility of the occurrence of dangling bonds in the pinholes or holes. The possibility of the occurrence of damage to the pellicle due to hydrogen atoms during a photolithography process may then be prevented or reduced, and thus the photolithography process may be performed more reliably and the pellicle may be increased in terms of lifespan or durability.

[0080] Furthermore, like in the base layer, the recovery layer may include a layer containing carbon and thus have optical, physical, and chemical properties similar to those of the base layer.

[0081] In a method of manufacturing a pellicle for a photomask, a recovery layer may be formed using catecholamine, wherein the catecholamine is easily coated on a base layer, fills pinholes or holes with little to no effort, and combines with the base layer to form an aromatic ring. The pellicle for a photomask may have increased surface uniformity of the pellicle film sheet and have improved or excellent optical properties, durability, and mechanical strength.

[0082] Although the present invention has been described with respect to the embodiments of the invention shown in the accompanying drawings, it will be appreciated by those skilled in the art that various changes and modifications may be made without departing from the technical spirit and essential features of the present invention. It will therefore be appreciated that the embodiments described above are merely illustrative in all aspects and not restrictive.

Claims

1. Surface film for photomask, include: The pellicle membrane sheet, wherein the pellicle membrane sheet comprises: a base layer having a first surface and a second surface opposite to the first surface, and a first recovery layer covering the first surface of the base layer, wherein the SP between the carbon atoms contained in the first recovery layer 2 The content of covalent bonds is less than or equal to the SP between carbon atoms contained in the base layer. 2 The content of covalent bonds, The base layer includes a first base atomic layer and a second base atomic layer having a first pinhole, the first pinhole including a dangling bond of a first carbon atom on a sidewall, and The first recovery layer fills the first pinhole while covering the first surface of the base layer, the first recovery layer includes a recovery atom layer, and second carbon atoms in the recovery atom layer are bonded to first carbon atoms of the dangling bonds in the second base atom layer.

2. The pellicle membrane of claim 1, wherein the pellicle membrane further comprises a support layer at at least one of: (A) between the base layer and the first recovery layer, or (B) on the second surface of the base layer, The base layer has a different crystal structure from that of the support layer. 3 . The pellicle film according to claim 1 , wherein the pellicle film sheet further comprises a support layer covering the second surface of the base layer and comprising carbon atoms.

4. The pellicle according to claim 1 or 3, wherein the content of at least one of nitrogen, hydrogen, or oxygen contained in the first recovery layer is greater than the corresponding content of the at least one of nitrogen, hydrogen, or oxygen contained in the base layer.

5. The pellicle according to claim 2 or 3, wherein The base layer comprises one of: graphene, graphite, or both graphene and graphite, and The support layer includes one of: diamond-like carbon, carbon nanotubes, or both diamond-like carbon and carbon nanotubes.

6. The pellicle of claim 2 or 3, wherein the support layer comprises at least one of iron, cobalt, or nickel.

7. The surface film according to claim 2 or 3, wherein the tensile strength of the base layer in the thickness direction of the base layer is smaller than the tensile strength of the support layer in the thickness direction of the support layer.

8. The pellicle membrane of claim 1, wherein the pellicle membrane further comprises a capping layer at at least one of: (A) on a surface of the first recovery layer opposite to a surface thereof proximate to the first surface of the base layer, or (B) on the second surface of the base layer, The capping layer includes at least one of boron, boron carbide, or boron nitride.

9. The pellicle of claim 1, wherein the D / G intensity ratio in the Raman spectrum of the pellicle film piece is in the range of 0-1.

10. The pellicle film according to claim 1, wherein the pellicle film sheet has an absorption coefficient of 0.01 or less for light having a wavelength of 13.5 nm.

11. The pellicle membrane of claim 1, wherein the pellicle membrane sheet has a tensile strength of 200 MPa-3 GPa.

12. The pellicle according to claim 1, wherein The base layer further comprises a second pinhole on the second surface, The pellicle film further includes a second recovery layer covering the second surface of the base layer and filling the second pinholes, and SP between carbon atoms contained in the second recovery layer 2 The content of covalent bonds is less than or equal to the SP between carbon atoms contained in the base layer. 2 Covalent bond content.

13. The pellicle membrane of claim 12, wherein the pellicle film sheet further comprises a support layer on a surface of the second recovery layer opposite to a surface thereof adjacent to the base layer.

14. The pellicle film according to claim 3, wherein the SP between carbon atoms contained in the first recovery layer is 2 The content of covalent bonds is less than or equal to the SP between carbon atoms contained in the support layer. 2 Covalent bond content.

15. The pellicle membrane of claim 3, wherein the pellicle membrane further comprises a capping layer at at least one of: (A) on a surface of the first recovery layer opposite to a surface thereof proximate to the first surface of the base layer, and (B) on a surface of the support layer opposite to a surface thereof proximate to the second surface of the base layer, The capping layer includes at least one of boron, boron carbide, or boron nitride.

16. The pellicle of claim 3, wherein the content of at least one of nitrogen, hydrogen, or oxygen contained in the first recovery layer is greater than the corresponding content of the at least one of nitrogen, hydrogen, or oxygen contained in the support layer.

17. A method for manufacturing a pellicle for a photomask as described in any one of 1 to 16, wherein the method include: Provide surface membrane film; and Transferring the pellicle membrane to a frame, The surface membrane sheet provided herein comprises: forming a base layer having a first surface and a second surface opposite to the first surface, coating a second carbonaceous material on the first surface of the base layer, and performing a first heat treatment process at a first process temperature to form a first recovery layer bonded to the base layer, Wherein the second carbonaceous material comprises catecholamines.

18. The method of claim 17, wherein providing the pellicle membrane further comprises: include: forming a support layer; providing the support layer on the second surface of the base layer; and A second heat treatment process is performed at a second process temperature to bond the support layer to the base layer.

19. The method of claim 18, wherein The first process temperature is in the range of 900-2,000°C, and The second process temperature is in the range of 100-300°C.

20. The method of claim 17, wherein The base layer includes one of: graphene, graphite, or both graphene and graphite.

21. The method of claim 17, wherein forming the base layer comprises providing a vapor of a first carbon-containing material to deposit carbon atoms on a catalytic metal substrate.

Citation Information

Patent Citations

  • Method and system for controlling high voltage battery of vehicle

    KR1020180069205A

  • Pellicle for photomask, reticle including the same, and exposure apparatus for lithography

    CN108121153A

  • Pellicles for use during EUV photolithography processes

    US20130250260A1

  • Methods of manufacturing pellicles having graphite layers

    US20160139500A1

  • Layered product and process for producing same

    US20170106626A1