Bonded magnet and method for manufacturing the same
By introducing the unextracted components of nylon 12 and the contact heat treatment of SmFeN-based magnetic powder and amorphous reagent into the bonded magnet, the problem of insufficient heat resistance of the bonded magnet is solved, and the stable performance in a high-temperature environment is achieved. It is suitable for High temperature uses such as engines.
Patent Information
- Application Number
- CN201910915658.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-09
- Filing Date
- 2019-09-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-09-25
AI Technical Summary
The existing bonded magnets are insufficient in heat resistance and are difficult to meet the needs of certain high-temperature applications.
The unextracted component from nylon 12 is introduced into the bonded magnet, and heat treatment is carried out by contacting the SmFeN-based magnetic powder and the amorphizing agent, thereby suppressing oxidation deterioration and improving heat resistance.
It significantly improves the heat resistance of bonded magnets, can maintain mechanical properties and magnetic properties under high temperature conditions, and is suitable for applications in high temperature environments.
Smart Images

Figure CN110970188B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a bonded magnet and a method for manufacturing the same. Background Art
[0002] Patent Document 1 discloses a bonded magnet having a nylon film formed on the surface of magnetic powder. Patent Document 2 discloses a bonded magnet containing a nylon 6 resin as a crystalline resin and an amorphous nylon resin.
[0003] The above-mentioned documents disclose the heat resistance of each bonded magnet, but further improvement of the heat resistance is desired.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2005-116789
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 9-12869 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] An object of the present invention is to provide a bonded magnet having excellent heat resistance.
[0010] Means of solving the problem
[0011] The present inventors conducted various studies with the purpose of improving the heat resistance of bonded magnets and found that if unextracted components from nylon 12 that are not extracted by hexafluoroisopropanol are present in the bonded magnet, oxidative degradation is suppressed and heat resistance is improved, thereby completing the present invention.
[0012] That is, the present invention relates to a bonded magnet comprising SmFeN-based magnetic powder, nylon 12, and unextracted components relative to hexafluoroisopropanol. In addition, the present invention relates to a method for manufacturing a bonded magnet, the method comprising the steps of bringing the bonded magnet comprising the SmFeN-based magnetic powder and nylon 12 into contact with an amorphizing agent, and heat-treating the bonded magnet in contact with the amorphizing agent.
[0013] Effects of the Invention
[0014] Since the bonded magnet of the present invention contains unextracted components from hexafluoroisopropanol, the heat resistance is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a photograph of a test piece after the bonded magnet produced in Example 1 was subjected to Soxhlet extraction with hexafluoroisopropanol. DETAILED DESCRIPTION
[0016] Hereinafter, the embodiments of the present invention will be described in detail. However, the embodiments shown below are examples for concretizing the technical ideas of the present invention, and the present invention is not limited to the following embodiments. It should be noted that in this specification, the term "process" not only refers to an independent process, but also includes it in this term as long as the intended purpose of the process is achieved, even if it cannot be clearly distinguished from other processes.
[0017] The bonded magnet of the present embodiment (hereinafter referred to as bonded magnet (A)) is characterized by containing SmFeN-based magnetic powder, nylon 12, and unextracted components from hexafluoroisopropanol.
[0018] The SmFeN-based magnetic powder contained in the bonded magnet (A) has Th2Zn 17 The crystal structure of this type is based on the general formula Sm x Fe 100-x-y N y The nitride represented by is composed of rare earth metal Sm, iron Fe and nitrogen N. Here, the atomic % x value of the rare earth metal Sm is in the range of 8.1 to 10%, the atomic % y value of N is in the range of 13.5 to 13.9 (atomic %), and the balance is mainly Fe. In addition, SmFeN-based magnetic powder is more commonly Sm2Fe 17 N3 indicates. The SmFeN series has stronger magnetic force than the ferrite series, and can generate high magnetic force even in a small amount. In addition, compared with other rare earth series such as the NdFeB series and the SmCo series, the SmFeN series has a smaller particle size, is suitable as a filler for the matrix resin, and is not easy to rust. In addition, the bonded magnet (A) may further contain rare earth magnetic powders of the NdFeB series and the SmCo series, and ferrite magnetic powders.
[0019] The average particle size of the magnetic powder is not particularly limited. In the case of the SmFeN system, the lower limit of the average particle size is preferably 0.1 μm or more, more preferably 0.5 μm or more, and the upper limit of the average particle size is preferably 10 μm or less, more preferably 5 μm or less. If the thickness is less than 0.1 μm, the magnetic particles are easily oxidized and the magnetic properties are reduced, and if the thickness exceeds 10 μm, the magnetic particles are easily formed into a multi-domain structure and the magnetic properties are reduced. It should be noted that the average particle size is measured in the form of a particle size equivalent to 50% of the volume accumulation starting from the small particle size side in the particle size distribution.
[0020] The content of nylon 12 contained in the bonded magnet (A) is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, relative to 100 parts by mass of magnetic powder, and the upper limit is preferably 15 parts by mass or less, more preferably 10 parts by mass or less. If the content of nylon is less than 3 parts by mass, the mechanical properties are greatly reduced due to the small amount of resin layer. If the content of nylon exceeds 15 parts by mass, it cannot become a strong magnet due to the reduced proportion of the magnetic layer. In addition, other resins may be contained as long as they have no effect on the heat resistance of the bonded magnet (A), for example, PPS (polyphenylene sulfide) resin, PP (polypropylene) resin, etc.
[0021] Regarding the unextracted components relative to hexafluoroisopropanol contained in the bonded magnet (A), when the bonded magnet (A) is subjected to Soxhlet extraction using hexafluoroisopropanol, nylon 12 is extracted by being dissolved in hexafluoroisopropanol, and the remaining extraction residue contains a magnetic powder component and unextracted components relative to hexafluoroisopropanol. In this embodiment, the unextracted components relative to hexafluoroisopropanol refer to the material obtained by subjecting the bonded magnet (A) to Soxhlet extraction for 24 hours and removing the magnetic powder component from the remaining extraction residue. In addition, if the solubility relative to hexafluoroisopropanol is taken into consideration, it can be inferred that the unextracted components relative to hexafluoroisopropanol are cross-linked products of nylon 12.
[0022] The content of the unextracted components contained in the bonded magnet (A) only needs to be more than 0.1% by mass and less than 5% by mass, and more preferably more than 0.15% by mass and less than 1% by mass. When the content of the unextracted components is less than 0.1% by mass, it is difficult to obtain high mechanical heat resistance as a magnet because the crosslinking density of the nylon on the surface of the magnet is low. If the content of the unextracted components exceeds 5% by mass, the proportion of nylon 12 contained in the bonded magnet (A) is reduced, so the elasticity is reduced and it is easy to break due to thermal shock. Here, the content of the unextracted components can be calculated by subtracting the mass of the unextracted components that can be calculated from the mass of the remaining extraction residue from the content of the magnetic powder component and dividing it by the mass of the bonded magnet before Soxhlet extraction. It should be noted that the content of the magnetic powder component can be calculated based on the content of the metal component from the magnetic powder obtained by ICP-AES analysis after the extraction residue is completely dissolved.
[0023] The unextracted components contained in the bonded magnet (A) may be contained in at least a part of the surface layer of the bonded magnet (A). In view of the heat resistance of the bonded magnet, the unextracted components are preferably contained in the surface layer more than the central part of the bonded magnet (A). In view of the heat resistance, the thickness of the surface layer is preferably 10 μm or more and 1 mm or less in the depth direction from the surface.
[0024] The bonded magnet (A) may contain components generally formulated into bonded magnets, such as an antioxidant, a heavy metal deactivator, a lubricant, a plasticizer, and the like.
[0025] The method for manufacturing a bonded magnet according to the present embodiment is characterized by comprising:
[0026] A step of bringing a bonded magnet comprising SmFeN-based magnetic powder and nylon 12 (hereinafter referred to as bonded magnet (B)) into contact with an amorphization agent;
[0027] The step of heat treating the bonded magnet in contact with the amorphization agent.
[0028] It is generally believed that when a bonded magnet (B) containing SmFeN-based magnetic powder and nylon 12 is brought into contact with an amorphizing agent and then subjected to heat treatment, the SmFeN-based magnetic powder acts as a catalyst, thereby generating a nylon 12 cross-linked product as an unextracted component relative to hexafluoroisopropanol, thereby improving the heat resistance of the obtained bonded magnet. It should be noted that the amorphizing agent contains a component that can dissolve crystalline nylon 12 and amorphize it.
[0029] The SmFeN-based magnetic powder in the bonded magnet (B) is as described above, and therefore its description is omitted here. It can be produced by the method disclosed in Japanese Patent No. 3698538, for example.
[0030] The bonded magnet (B) may further contain NdFeB-based, SmCo-based rare earth magnetic powders, and ferrite-based magnetic powders. NdFeB-based magnetic powders may be produced, for example, by the HDDR method described in Japanese Patent No. 3565513, and may be suitably used. 3 ) NdFeB-based magnetic powder. In addition, Sm-Co magnetic powder can be produced, for example, according to Japanese Patent No. 3505261, and Sm-Co magnetic powder having an average particle size of 10 to 30 μm can be used.
[0031] The content of nylon 12 contained in the bonded magnet (B) is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and the upper limit is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of magnetic powder. If the content of nylon 12 is less than 3 parts by mass, the resin layer is less, so the mechanical properties are greatly reduced. If it exceeds 15 parts by mass, the proportion of the magnetic layer is reduced, so it cannot become a strong magnet. In addition, as long as it has no effect on the heat resistance of the bonded magnet (B), other resins may be contained, for example, PPS resin, PP resin, etc.
[0032] The bonded magnet (B) may contain commonly formulated components such as an antioxidant, a heavy metal deactivator, a lubricant, a plasticizer, and the like.
[0033] The bonded magnet (B) can be obtained by melt-kneading magnetic powder and nylon 12 to make a composite, and molding these composites. There is no particular limitation on the melt-kneading machine used when making the composite, and a single-axis screw mixer, a twin-axis screw mixer, a mixing roll, a kneading machine, a Banbury mixer, an intermeshing twin-axis screw extruder, a non-intermeshing twin-axis screw extruder, etc. can be used. When nylon 12 is used, the melt-kneading temperature can be set to above 180°C and below 250°C. In addition, there is no particular limitation on the molding method of the obtained composite, and injection molding, compression molding, extrusion molding, calendering molding, etc. can be used. When using SmFeN-based magnetic powder, it is preferably mechanically oriented or magnetically oriented to arrange the magnetic powder inside the bonded magnet composition.
[0034] The amorphizing agent includes a component (A) capable of dissolving crystalline nylon 12 to amorphize the nylon 12 and an organic solvent (B), and the content of each component in the amorphizing agent is 10 to 30% by mass of the component (A) capable of dissolving nylon 12 to amorphize the nylon 12 and 70 to 90% by mass of the organic solvent (B). Examples of the amorphizing agent include Japanese Patent Application Publication No. 2003-89131.
[0035] The component (A) that dissolves crystalline nylon 12 to make it amorphous is a component that dissolves a part of the crystalline region of nylon 12 to make it amorphous and enters the gaps between polymer chains to widen the gaps between polymer chains. Examples thereof include divalent or higher phenols, fluorinated alcohols containing fluorine atoms, and benzenesulfonamides having a -SO2NH2 group that strongly hydrogen bonds with nylon resin.
[0036] The dihydric or higher phenols refer to benzene compounds having two or more hydroxyl groups in the molecule, and examples thereof include dihydric phenols such as 1,3-dihydroxybenzene, 1,2-dihydroxybenzene, 1,4-dihydroxybenzene, 1-chloro-2,4-dihydroxybenzene, 2-chloro-1,3-dihydroxybenzene, 1,3-dihydroxy-4-methylbenzene, 1,3-dihydroxy-2-methylbenzene, 3,5-dihydroxybenzoic acid, and 2,4-dihydroxybenzoic acid, and trihydric phenols such as 1,2,3-trihydroxybenzene, 1,2,4-trihydroxybenzene, 1,3,5-trihydroxybenzene, 3,4,5-trihydroxybenzoic acid, and 2,4,6-trihydroxybenzoic acid. Among them, dihydric phenols having excellent solubility in solvents are preferred, and 1,3-dihydroxybenzene is more preferred from the viewpoint of availability.
[0037] Fluorinated alcohols containing fluorine atoms can be classified by the names of fluorine-containing alcohols or fluorine-based alcohols, and examples thereof include 1,2,3-trifluoroethanol, 1,1,1,3,3,3-hexafluoro-2-propanol (HFIP), 2,2,3,3-tetrafluoro-1-propanol, 2-perfluoroalkylethanol, etc. Among them, 1,1,1,3,3,3-hexafluoro-2-propanol (HFIP) is preferred because of its excellent solubility in nylon 12 resin.
[0038] Benzenesulfonamides having a -SO2NH2 group that is strongly hydrogen-bonded to nylon resins refer to compounds having a sulfonamide group (-SO2NH2) in the structure, represented by the structures of primary sulfonamide R-SO2NH2, secondary sulfonamide R-SO2NHR′ and tertiary sulfonamide R-SO2NR′R″. In each formula, R is an aromatic hydrocarbon group that may be substituted by halogens such as Cl, NH2 groups, sulfonamide groups, etc. R′ and R″ are C n H 2n+1 (n=1 to 4). Examples thereof include benzenesulfonamide, 1,2-benzenedisulfonamide, 2-chlorobenzenesulfonamide, 4-chlorobenzenesulfonamide, 2-methylbenzenesulfonamide, 4-methylbenzenesulfonamide, 3-aminobenzenesulfonamide, 4-aminobenzenesulfonamide, 4-(2-aminoethyl)benzenesulfonamide, etc. Among them, primary sulfonamide (R-SO2NH2) which easily forms a strong hydrogen bond association with the amide group of the nylon resin is preferred, and benzenesulfonamide in which R is a benzene ring is more preferred from the viewpoint of solvent solubility and thermal stability.
[0039] As the organic solvent (B), alcohols are preferred, and examples thereof include methanol, ethanol, propanol, isopropanol, butanol, pentanol, tert-butanol, and hexanol.
[0040] The amorphizing agent may further contain a component (C) that can maintain the widening of the polymer chains caused by the above-mentioned component (A). As component (C), it is a substance with a solubility parameter (SP value) in the range of 9 to 13, and substances having functional groups that can form hydrogen bonds with the amide groups of nylon 12 and bulky molecular structures can be listed. It is generally believed that component (C) enters the polymer chains generated by component (A) and forms hydrogen bonds with each polymer chain, so that component (C) plays a role as a pillar, thereby maintaining the widening of the polymer chains. As component (C), for example, nylons other than nylon 12, compounds with a fluorene skeleton, etc. can be listed. The content of component (C) in the amorphizing agent can be set to 10 to 20% by mass.
[0041] Examples of nylons other than nylon 12 include nylon 6 (SP value: 11.6), nylon 6,6 (SP value: 11.6), nylon 11 (SP value: 10.1), nylon 6,12 (SP value: 11.6), nylon 6,10 (SP value: 10.8), nylon 6,66 (SP value: 11.6), and nylon MXD6 (SP value: 11.6). These may be used alone or in combination of two or more.
[0042] Examples of the compound having a fluorene skeleton include low molecular weight fluorene compounds such as bisaminobenzenefluorene (SP value: 12.7), bistoluidine fluorene (SP value: 12.3), bisphenoxyethanol fluorene (SP value: 12.3), and 2-aminofluorene (SP value: 12.7), or oligomers or polymers having a fluorene structure (e.g., fluorene oligomers, OGSOL MF-11, manufactured by Osaka Gas Chemical Co., Ltd.), etc. These may be used alone or in combination of a plurality of them.
[0043] The method for bringing the bonded magnet (B) into contact with the amorphizing agent is not particularly limited as long as the two can be brought into contact, and examples thereof include a method of immersing the bonded magnet (B) in the amorphizing agent, a method of coating or spraying the amorphizing agent on the bonded magnet (B), etc.
[0044] Next, the bonded magnet in contact with the amorphizing agent is heat-treated. The nylon 12 that has been in contact with the amorphizing agent and amorphized is cross-linked by the heat treatment and becomes an unextracted component relative to hexafluoroisopropanol. The SmFeN-based magnetic powder contained in the bonded magnet (B) functions as a catalyst, thereby promoting the cross-linking reaction and significantly shortening the heat treatment time.
[0045] The lower limit of the heat treatment temperature is preferably 150° C. or higher, and more preferably 160° C. or higher. On the other hand, the upper limit is preferably less than 178° C. If the heat treatment temperature is lower than 150° C., a long time is required for the crosslinking reaction to occur, thereby increasing the processing cost. If the heat treatment temperature is higher than 178° C., deformation becomes large due to melting of nylon 12, etc., which is not preferred.
[0046] The heat treatment time is not particularly limited, but the upper limit is preferably 100 hours or less, more preferably 10 hours or less. Since the treatment cost increases as the treatment time increases, it is not preferred if the heat treatment time exceeds 100 hours.
[0047] Example
[0048] Hereinafter, examples will be described. It should be noted that, unless otherwise specified, "%" is based on mass.
[0049] Example 1
[0050] Production of bonded magnet composition
[0051] 7.7% by mass of nylon 12 resin powder and 0.3% by mass of phenolic antioxidant powder were added to 92% by mass of samarium iron nitrogen magnetic powder (average particle size of 3 μm), mixed in a mixer, and then the mixed powder was put into a double-screw mixer and kneaded at 210° C. to obtain a kneaded product. The obtained kneaded product was cooled and cut to obtain a bonded magnet composition.
[0052] Molding process
[0053] The obtained bonded magnet composition was dissolved in a cylinder at 250° C., and injection molded in a mold adjusted to 90° C. while applying an orientation magnetic field of 9 kOe, thereby obtaining a bonded magnet (B).
[0054] Amorphization / heat treatment process
[0055] NP-221 (an alcohol solution of a mixture of dihydroxybenzene derivatives, manufactured by Keizen Co., Ltd.) as an amorphization agent was applied to all surfaces of the obtained bonded magnet (B). Then, the alcohol solvent was evaporated by natural drying, and heat-treated by placing in an oven adjusted to 150°C for 1 hour and exposing to the atmosphere to obtain a bonded magnet (A). Table 1 shows the conditions of the heat treatment time of each example.
[0056] Embodiments 2 to 4
[0057] A bonded magnet (A) was produced by the method described in Example 1 except that the heat treatment time was changed.
[0058] Table 1 shows the conditions of the heat treatment time in each example.
[0059] Example 5
[0060] A bonded magnet was produced by the method described in Example 2 except that a mixed powder of SmFeN powder and NdFeB powder having an average particle size of 200 μm in a mass ratio of 5:95 was used instead of the SmFeN magnetic powder.
[0061] Example 6
[0062] A bonded magnet was produced by the method described in Example 2 except that a mixed powder of SmFeN powder and NdFeB powder having an average particle size of 200 μm in a mass ratio of 50:50 was used instead of the SmFeN magnetic powder.
[0063] Example 7
[0064] A bonded magnet was prepared by the method described in Example 2 except that a mixed powder of SmFeN powder and anisotropic ferrite powder having an average particle size of 1 μm in a mass ratio of 5:95 was used instead of the SmFeN magnetic powder.
[0065] Example 8
[0066] A bonded magnet was produced according to the method described in Example 2 except that a mixed powder of SmFeN powder and anisotropic ferrite powder having an average particle size of 1 μm in a mass ratio of 50:50 was used instead of the SmFeN magnetic powder.
[0067] Comparative Example 1
[0068] A bonded magnet was produced in the same manner as in Example 1 except that the treatment with the amorphizing agent and the heat treatment were not performed.
[0069] Comparative Example 2
[0070] A bonded magnet was produced by the method described in Example 2 except that 91.5 mass % of NdFeB powder having an average particle size of 200 μm and 8.2 mass % of nylon 12 resin powder were used instead of the SmFeN magnetic powder.
[0071] Comparative Example 3
[0072] A bonded magnet was produced by the method described in Example 2 except that 88% by mass of anisotropic ferrite powder having an average particle size of 1 μm and 11.7% by mass of nylon 12 resin powder were used instead of the samarium iron nitrogen magnetic powder.
[0073] Comparative Example 4
[0074] <Mixing and molding process of nylon 12 resin>
[0075] After mixing 0.3% by mass of a phenolic antioxidant with 99.7% by mass of nylon 12 resin powder containing no magnetic powder by a mixer, the mixed powder is added to a twin-shaft kneader and kneaded at 190° C. to obtain a kneaded product. After the obtained kneaded product is cooled, it is cut into appropriate sizes to obtain a nylon 12 resin composition, which is then placed in the hopper of an injection molding machine, dissolved in a barrel at 200° C., and injection molded in a mold adjusted to 40° C. to obtain a bonded magnet.
[0076] The bonded magnets obtained in Examples and Comparative Examples were evaluated by the following methods.
[0077] <Evaluation of Mechanical Heat Resistance>
[0078] The obtained bonded magnet was left at room temperature in an air-conditioned room for one night, and then its short-term heat resistance was evaluated by measuring its load deflection temperature (HDT) (conditions: horizontal placement, test load: 1.80 MPa, heating rate: 120°C / hr).
[0079] It was confirmed that Examples 1 to 8 had higher HDT temperatures than Comparative Examples 1 to 4, and that the heat resistance was improved.
[0080] <Evaluation of long-term heat resistance>
[0081] The obtained bonded magnet was placed in an air-conditioned room at room temperature for one night, then placed in an oven at 150°C and exposed to the atmosphere. The molded product after 1000 hours was placed in an air-conditioned room at room temperature for one night, and the bending strength was measured using a multi-purpose strength tester. The ratio of the bending strength of the molded product after 1000 hours to the bending strength of the bonded magnet before being placed in the oven was evaluated as the bending strength maintenance rate.
[0082] Since Examples 1 to 8 had higher flexural strength retention rates than Comparative Examples 1 to 4, it was confirmed that the long-term heat resistance was improved.
[0083] <Evaluation of unextracted ingredients>
[0084] Figure 1 The figure shows the residue after Soxhlet extraction using hexafluoroisopropanol on the bonded magnet obtained in Example 1. It can be confirmed that a thin layer of about 100 μm is formed on the surface. In addition, Soxhlet extraction was also performed on Examples 2 to 8 and Comparative Examples 1 to 4. As a result, a surface layer of about 100 μm can be confirmed for Examples 2 to 8, but no surface layer can be confirmed for Comparative Examples 1 to 4.
[0085] For Example 1, the Fe concentration from the magnetic powder contained in the surface layer of the extraction residue was measured by X-ray fluorescence analysis (XRF), and the C concentration was measured by TOC analysis (combustion method). The results showed that the Fe concentration was 72.1% by mass and the C concentration was 2.2% by mass. In addition, the central part of the extraction residue was also analyzed for Fe and C, and the results were 72.1% by mass and 0.36% by mass, respectively. The ratio of the unextracted components contained in the extraction residue defined by the formula: C / Fe×100 is 3.1% in the surface layer and 0.5% in the central part, which can confirm that the unextracted components are more contained in the surface layer. It can be confirmed from Table 1 that in Examples 2 to 8, the unextracted components are also more contained in the surface layer.
[0086] In addition, the mass of the unextracted components that can be calculated by subtracting the content of the magnetic powder component from the mass of the remaining extraction residue and dividing it by the mass of the bonded magnet before Soxhlet extraction, the content of the unextracted components of each embodiment and comparative example was calculated. It should be noted that the content of the magnetic powder component is calculated based on the content of the metal component from the magnetic powder obtained by ICP-AES analysis after the extraction residue is completely dissolved.
[0087] Table 1
[0088]
[0089] Industrial Applicability
[0090] The bonded magnet of the present invention has high heat resistance and can therefore be suitably used in applications such as engines.
Claims
1. A bonded magnet comprising SmFeN-based magnetic powder, nylon 12, and unextracted components relative to hexafluoroisopropanol, The bonded magnet is obtained by contacting a bonded magnet containing SmFeN-based magnetic powder and nylon 12 with an amorphizing agent selected from divalent or higher phenols, fluoroalcohols and benzenesulfonamides, and heat-treating the bonded magnet in contact with the amorphizing agent. The unextracted components relative to hexafluoroisopropanol refer to the materials obtained by subjecting the bonded magnet to Soxhlet extraction for 24 hours and removing the magnetic powder components from the remaining extraction residue. The unextracted components are contained more in the surface layer than in the central portion of the bonded magnet.
2. The bonded magnet according to claim 1, wherein: The content of the unextracted components contained in the bonded magnet exceeds 0.1 mass % and is 5 mass % or less.
3. The bonded magnet according to claim 1, wherein: The content of the unextracted components contained in the bonded magnet is more than 0.15 mass % and less than 1 mass %.
4. The bonded magnet according to claim 1, wherein: The thickness of the surface layer is 10 μm or more and 1 mm or less in a depth direction from the surface of the bonded magnet.
5. The bonded magnet according to any one of claims 1 to 4, wherein: The content of the nylon 12 is 3 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the SmFeN-based magnetic powder.
6. A method for manufacturing a bonded magnet, comprising: The step of contacting a bonded magnet containing SmFeN-based magnetic powder and nylon 12 with an amorphization agent selected from divalent or higher phenols, fluoroalcohols and benzenesulfonamides, and a step of heat treating the bonded magnet in contact with the amorphization agent, The bonded magnet comprises unextracted components relative to hexafluoroisopropanol, The unextracted components relative to hexafluoroisopropanol refer to the materials obtained by subjecting the bonded magnet to Soxhlet extraction for 24 hours and removing the magnetic powder components from the remaining extraction residue. The unextracted components are contained more in the surface layer than in the central portion of the bonded magnet.
7. The method for manufacturing a bonded magnet according to claim 6, wherein: The heat treatment temperature is 150°C or higher and lower than 178°C.
8. The method for manufacturing a bonded magnet according to claim 7, wherein: The heat treatment temperature is 160°C or higher and lower than 178°C.
9. The method for manufacturing a bonded magnet according to any one of claims 6 to 8, wherein: The content of the nylon 12 is 3 parts by mass or more and 15 parts by mass or less relative to 100 parts by mass of the SmFeN-based magnetic powder.
10. The method for manufacturing a bonded magnet according to any one of claims 6 to 8, wherein: The amorphization agent includes a first component capable of dissolving crystalline nylon 12 to amorphize the nylon 12, and an organic solvent.
11. The method for manufacturing a bonded magnet according to claim 9, wherein: The amorphization agent includes a first component capable of dissolving crystalline nylon 12 to amorphize the nylon 12, and an organic solvent.
12. The method for manufacturing a bonded magnet according to claim 10, wherein: The content of the first component in the amorphizing agent is 10 mass % to 30 mass %, and the content of the organic solvent in the amorphizing agent is 70 mass % to 90 mass %.
13. The method for manufacturing a bonded magnet according to claim 11, wherein: The content of the first component in the amorphizing agent is 10 mass % to 30 mass %, and the content of the organic solvent in the amorphizing agent is 70 mass % to 90 mass %.
14. The method for manufacturing a bonded magnet according to claim 10, wherein: The amorphization agent includes a second component capable of maintaining the broadening of polymer chains caused by the first component.
15. The method for manufacturing a bonded magnet according to claim 11, wherein: The amorphization agent includes a second component capable of maintaining the broadening of polymer chains caused by the first component.
16. The method for manufacturing a bonded magnet according to claim 12, wherein: The amorphization agent includes a second component capable of maintaining the broadening of polymer chains caused by the first component.
17. The method for manufacturing a bonded magnet according to claim 13, wherein: The amorphization agent includes a second component capable of maintaining the broadening of polymer chains caused by the first component.
18. The method for manufacturing a bonded magnet according to claim 14, wherein: The content of the second component in the amorphization agent is 10 mass % to 20 mass %.
19. The method for manufacturing a bonded magnet according to claim 15, wherein: The content of the second component in the amorphization agent is 10 mass % to 20 mass %.
20. The method for manufacturing a bonded magnet according to claim 16, wherein: The content of the second component in the amorphization agent is 10 mass % to 20 mass %.
21. The method for manufacturing a bonded magnet according to claim 17, wherein: The content of the second component in the amorphization agent is 10 mass % to 20 mass %.
22. A method for manufacturing a bonded magnet according to any one of claims 6 to 8, wherein the bonded magnet is brought into contact with the amorphizing agent by immersing the bonded magnet in the amorphizing agent or by coating or spraying the amorphizing agent on the bonded magnet.
23. The method for manufacturing a bonded magnet according to claim 9, wherein the bonded magnet is brought into contact with the amorphizing agent by immersing the bonded magnet in the amorphizing agent or by coating or spraying the amorphizing agent on the bonded magnet.
24. The method for manufacturing a bonded magnet according to claim 10, wherein the bonded magnet is brought into contact with the amorphizing agent by immersing the bonded magnet in the amorphizing agent or by coating or spraying the amorphizing agent on the bonded magnet.
25. The method for manufacturing a bonded magnet according to claim 11, wherein the bonded magnet is brought into contact with the amorphizing agent by immersing the bonded magnet in the amorphizing agent or by coating or spraying the amorphizing agent on the bonded magnet.
26. The method for manufacturing a bonded magnet according to claim 14, wherein the bonded magnet is brought into contact with the amorphizing agent by immersing the bonded magnet in the amorphizing agent or by coating or spraying the amorphizing agent on the bonded magnet.
27. The method for manufacturing a bonded magnet according to claim 15, wherein the bonded magnet is brought into contact with the amorphizing agent by immersing the bonded magnet in the amorphizing agent or by coating or spraying the amorphizing agent on the bonded magnet.