Mounting structure and nanoparticle mounting material
By using nanoparticle mounting material of the second metal solid solution in the first metal, the problem of bonding SiC and GaN components at high temperatures is solved, the sintering time is shortened and the generation of intermetallic compounds is suppressed, and high-efficiency and low-damage bonding is achieved. Effect.
Patent Information
- Application Number
- CN201980003873.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-04-12
- Filing Date
- 2019-02-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-02-14
AI Technical Summary
When using SiC elements and GaN elements in the prior art, the solder material has insufficient heat resistance, making it difficult to effectively bond the element electrode and the lead frame electrode at high temperatures, and the nanoparticles are sintered for a long time, making it difficult to shorten the bonding time and suppress the surroundings. Thermal damage to the component.
Using a nanoparticle mounting material containing the first metal and a second metal solid solution in the first metal, the diffusion coefficient of the second metal is greater than the self-diffusion coefficient of the first metal, and short-term sintering is used to shorten the bonding time and suppress the metal. The formation of inter-compounds ensures the conductivity and heat resistance of the metal.
It realizes effective bonding of component electrodes and lead frame electrodes in a short time at low temperatures, reduces thermal damage to peripheral components, and maintains the conductivity and heat resistance of nanoparticles, improving production efficiency and product quality.
Smart Images

Figure CN111033703B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a mounting structure having a structure in which two members are joined by a metal material and used in equipment such as a power plant, and a nanoparticle mounting material used in the production of the mounting structure. Background Art
[0002] Devices such as power units that have semiconductor elements that generate heat sometimes have a mounting structure in which two components, a substrate and a heat dissipation portion, are joined in order to transfer heat from a substrate on which the semiconductor elements are mounted to a heat dissipation portion in order to dissipate the heat generated by the semiconductor elements.
[0003] In recent years, as a power device, from the perspective of energy saving, the use of next-generation power device elements such as SiC elements and GaN elements, which have the advantage of being able to efficiently control electric power, has been increasing from existing Si elements. These next-generation power device elements have the advantage of being able to operate even at high temperatures, and can withstand greater heat than existing Si elements, so sometimes they can control the flow of larger currents. However, if a larger current flows, the heat generated from the semiconductor element increases, and the semiconductor element is further heated. As a result, the temperature Tj of the joint between the electrode of the lead frame, etc., which is used to pass the current controlled by the semiconductor element, and the element electrode also increases. For example, when using existing Si elements, the temperature Tj of the above-mentioned joint is about 125°C, but when using SiC elements and GaN elements, it reaches 200-250°C.
[0004] Therefore, the joint portion between the element electrode and the lead frame electrode requires thermal conductivity for efficiently dissipating the generated heat to the lead frame and heat resistance corresponding to a higher temperature Tj of the joint portion.
[0005] In the past, solder materials were widely used in the joints used in the joints of the mounting structure that uses a conductor to join the element electrode and the lead frame electrode, because they can be joined at low temperatures. However, the temperature Tj of the joint when using SiC elements and GaN elements, that is, 200 to 250°C, is a very harsh temperature because it is near or above the melting point for the solder materials that are mainly composed of Sn and Pb, etc. Therefore, it is difficult to ensure heat resistance when using SiC elements and GaN elements in the mounting structure that uses these solder materials for the joints.
[0006] In response to such a problem, expectations for mounting structures obtained by sintering metals such as Ag and Cu to join component electrodes to lead frame electrodes are increasing. Metals such as Ag and Cu have excellent thermal conductivity, and their respective melting points are sufficiently high relative to the temperature Tj of the above-mentioned joint, that is, 200 to 250°C, so they also have excellent heat resistance. However, since metals such as Ag and Cu have high melting points, in order to melt the above-mentioned metals and join them through solid-liquid diffusion between the component electrode and the lead frame electrode as in the existing joining using solder materials, heating at 1000 to 1200°C is required, making practical use difficult.
[0007] In order to facilitate the above-mentioned joining when using high melting point metals such as Ag and Cu, the use of these particles with an average particle size of several nm to several hundred nm as nanoparticle mounting materials has been studied. Compared with metal particles with an average particle size of micrometers or more, the ratio of the surface area occupied by the nano-sized metal particles to the surface area of the particles, that is, the specific surface area, is very large. At this time, the surface of the metal particles is in an unstable state compared to the bulk metal and has a large surface energy. Therefore, nano-sized metal particles can be joined by the above-mentioned sintering at a low temperature (e.g., 150 to 400°C) far below their melting point.
[0008] However, when the above-mentioned joining is performed by sintering of nanoparticle mounting materials such as Ag and Cu, the time required for the heating process for diffusing these metals between solid phases is 30 minutes to 60 minutes or more. This time is particularly large compared to the 5 minutes or so of the existing solder material. If you want to shorten the time required for the above-mentioned heating process, you need to sinter the vapor nanoparticle mounting material at a higher temperature. However, if the temperature during the above-mentioned sintering is increased, thermal damage will occur to the peripheral components exposed to the high temperature during sintering. On the other hand, if the holding temperature during joining is low in order to suppress the thermal damage to the peripheral components, the time required for the above-mentioned heating process increases exponentially, and the cost will increase especially during mass production. In this way, if you want to join the component electrode with the lead frame electrode by sintering the above-mentioned nanoparticle mounting material, it is difficult to take into account both the suppression of thermal damage to the peripheral components to improve the quality of the product and the shortening of the preparation time (lead time) during mass production to suppress the cost. Therefore, it is necessary to shorten the time required for the above-mentioned joining and the nanoparticle mounting material that will not increase the thermal damage to the peripheral components.
[0009] Patent document 1 discloses a bonding material, which contains: first metal particles having an organic film that can be detached by heating arranged on the surface thereof; and second metal particles containing a metal having a liquid phase generation temperature lower than the detachment start temperature of the organic film and capable of forming an intermetallic compound by reacting with the first metal particles. Regarding the bonding material described in Patent document 1, Patent document 1 states that first, the second metal particles are heated at a temperature (below 250°C) at which the liquid phase is generated, and then, the organic film is heated at a temperature (about 250°C to 350°C) at which the organic film is detached from the surface of the first metal particles, thereby generating an intermetallic compound. Patent document 1 states that if the bonding layer is formed by the above method, the formation of the intermetallic compound will be uniformly induced in the bonding material, and a bonding layer with excellent bonding strength will be formed.
[0010] Prior Art Literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2017-101313 Summary of the invention
[0013] According to the bonding material described in Patent Document 1, it is expected that bonding at a lower temperature can be performed, thereby shortening the time required for conventional bonding without increasing thermal damage to surrounding components. However, as described in Patent Document 1, there is a problem that when an intermetallic compound with first metal particles is formed by melting the second metal particles, brittleness unique to the intermetallic compound is found, and thus the heat resistance of the first metal changes.
[0014] The present invention is made in view of the above-mentioned problems, and its purpose is to provide a mounting structure and a nanoparticle mounting material used in the manufacture of the mounting structure. The mounting structure is a mounting structure obtained by joining an element electrode to a metal component by sintering metal nanoparticles. The mounting structure shortens the time required for joining based on the above-mentioned sintering, reduces thermal damage to surrounding components during sintering, and inhibits the generation of intermetallic compounds based on the above-mentioned sintering, making it difficult to reduce the physical properties of the metal constituting the nanoparticles.
[0015] In order to achieve the above-mentioned problem, a mounting structure is used, which includes: a semiconductor element having an element electrode; a metal component; and a sintered body, which joins the semiconductor element and the metal component, the sintered body including: a first metal, and a second metal solid-dissolved in the first metal, the second metal being a metal whose diffusion coefficient in the first metal is greater than the self-diffusion coefficient of the first metal, and the content of the second metal relative to the total mass of the first metal and the second metal in the sintered body is below the solid solubility limit of the second metal in the first metal.
[0016] In addition, a nanoparticle mounting material is used, which contains at least: nanoparticles of a first metal, and nanoparticles of a second metal solid-dissolved in the above-mentioned first metal, the ratio of the nanoparticles of the above-mentioned first metal with a particle size of less than 100nm relative to the total number of the nanoparticles of the above-mentioned first metal is more than 50%, the average particle size of the nanoparticles of the above-mentioned second metal is less than 100nm, the above-mentioned second metal is a metal whose diffusion coefficient in the above-mentioned first metal is greater than the self-diffusion coefficient of the above-mentioned first metal, and the mass ratio of the above-mentioned second metal relative to the total mass of the above-mentioned first metal and the above-mentioned second metal is below the solid solubility limit of the above-mentioned first metal.
[0017] According to the present invention, a mounting structure and a nanoparticle mounting material used in the manufacture of the mounting structure can be provided, wherein the mounting structure reduces the physical properties of the metal constituting the nanoparticles by shortening the time required for sintering-based joining, reducing thermal damage to surrounding components during sintering, and inhibiting the generation of intermetallic compounds based on the above-mentioned sintering. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a cross-sectional view of a bonding portion from a semiconductor element to a lead frame of the mounting structure in the present embodiment, taken along a direction parallel to the thickness direction.
[0019] Figure 2 This is a cross-sectional SEM image of the sintered body in the mounting structure of Example 1-4 in the present embodiment.
[0020] Figure 3 This is a cross-sectional SEM image of the sintered body in the mounting structure of Comparative Example 1-1. DETAILED DESCRIPTION
[0021] Hereinafter, a mounting structure according to an embodiment of the present invention, a nanoparticle mounting material used for producing the mounting structure, and a method for producing the mounting structure will be described in detail.
[0022] <Structure>
[0023] Figure 1 It is a cross-sectional view of a bonding portion from a semiconductor element to a lead frame of the mounting structure in the present embodiment, taken along a direction parallel to the thickness direction.
[0024] The mounting structure 108 in the present embodiment is a mounting structure in which a semiconductor element 101 having an element electrode 102 and a lead frame 105 having a lead frame electrode 104 are bonded to each other via a sintered body 103 .
[0025] The mounting structure 108 has a structure in which a semiconductor element 101 such as a transistor is supported by a lead frame 105 and connected to external wiring through the lead frame 105. The semiconductor element 101 and the lead frame 105 are electrically and mechanically connected by bonding an element electrode 102 of the semiconductor element 101 and a lead frame electrode 104 of the lead frame 105 via a sintered body 103.
[0026] In the present embodiment, the sintered body 103 is a structure formed by sintering nano-sized metal particles, and is a sintered body containing a first metal and a second metal.
[0027] In addition, regarding the size of the nano-sized metal particles, an average particle diameter of 50 nm to 100 nm is preferred.
[0028] The average particle size is calculated using a laser particle size distribution analyzer. The average particle size is the value of the median particle size d50% (μm, volume conversion). The same applies to the following.
[0029] The first metal is a metal having electrical conductivity, high thermal conductivity, and heat resistance that can withstand the temperature Tj of the junction portion, which is the temperature Tj of the junction portion (sintered body 103) of the semiconductor element 101 and the lead frame 105 when using SiC elements and GaN elements, i.e., 200 to 250° C. Examples of the first metal include Ag and Cu.
[0030] Here, the temperature Tj of the junction portion refers to the highest temperature reached at the junction interface when the semiconductor element is operating.
[0031] The second metal is a metal that can be dissolved in the first metal, and at least a part of it is dissolved in the first metal in the sintered body 103. In addition, the second metal is an element whose diffusion coefficient in the first metal is greater than the self-diffusion coefficient of the first metal. Here, the so-called self-diffusion coefficient refers to the coefficient of diffusion of metal atoms in the metal.
[0032] Examples of the second metal include Sn, Cu, Pb, and Ge when the first metal is Ag, and Ge when the first metal is Cu.
[0033] As described later, the nanoparticle mounting material containing the nanoparticles of the first metal and the nanoparticles of the second metal is sintered to form a sintered body 103. During the sintering, the nanoparticles of the second metal diffuse faster than the first metal because the diffusion coefficient in the first metal is greater than the self-diffusion coefficient of the first metal, and it is easy to make the nanoparticles of the first metal combine with each other. Therefore, the second metal can shorten the time required for the combination of the nanoparticles of the first metal and shorten the time required for the joining based on sintering. Thus, the thermal damage to the surrounding components during sintering can be reduced. In addition, at this time, since the nanoparticles of the second metal disappear due to the solid solution of the second metal in the first metal through the diffusion, the second metal disappears. Therefore, in the sintered body 103, the phase of the second metal is not formed, and the properties of the first metal such as electrical conductivity, thermal conductivity and heat resistance are difficult to be damaged.
[0034] The diffusion coefficient of the second metal in the first metal and the self-diffusion coefficient of the first metal can use known values, and the temperature for producing the sintered body 103 may be determined based on a value of 200° C., for example.
[0035] Regarding the sintered body 103, the content of the second metal relative to the total mass of the first metal and the second metal is below the solid solubility limit of the second metal in the first metal. Thus, changes in the electrical conductivity, thermal conductivity, heat resistance, and other properties of the first metal caused by the formation of an intermetallic compound between the second metal and the first metal can be suppressed.
[0036] On the other hand, during sintering at low temperature and in a short time, in order to fully combine the nanoparticles of the first metal to suppress the reduction of electrical conductivity, thermal conductivity and heat resistance caused by the residual unsintered nanoparticles, it is preferred to increase the content of the second metal as much as possible below the above-mentioned solid solubility limit. Specifically, the content of the second metal can be set to more than 70% and less than 100% relative to the above-mentioned solid solubility limit. For example, when the first metal is Ag and the second metal is Sn (the solid solubility limit of Sn is 10% by mass), the content of the second metal, i.e., Sn, can be set to more than 7% by mass and less than 10% by mass relative to the total mass of the first metal and the second metal.
[0037] The solid solubility limit of the second metal in the first metal can be obtained from the equilibrium diagram of the first metal and the second metal, and may be set to the solid solubility limit of the temperature for producing the sintered body 103 , for example, 200° C.
[0038] <Nano Particle Mounting Materials>
[0039] The nanoparticle mounted material in the present embodiment is a mounted material containing at least the nanoparticles of the first metal described above and the nanoparticles of the second metal described above.
[0040] In the present embodiment, the first metal is a metal having electrical conductivity, high thermal conductivity, and heat resistance that can withstand the temperature Tj of the junction portion, which is the temperature Tj of the junction portion (sintered body 103) of the semiconductor element 101 and the lead frame 105 when using SiC elements and GaN elements, i.e., 200 to 250° C. Examples of the first metal include Ag and Cu.
[0041] In addition, in the present embodiment, the second metal is a metal that can be dissolved in the first metal, and is an element whose diffusion coefficient in the first metal is greater than the self-diffusion coefficient of the first metal. Examples of the second metal include Sn, Cu, Pb, and Ge when the first metal is Ag, and Ge when the first metal is Cu.
[0042] In addition, in the present embodiment, the mass ratio of the second metal relative to the total mass of the first metal and the second metal is below the solid solubility limit of the first metal. In addition, the content of the second metal can be set to 70% or more and 100% or less relative to the solid solubility limit. When the first metal is Ag and the second metal is Sn (the solid solubility limit of Sn is 10% by mass), the content of the second metal, i.e., Sn, relative to the total mass of the first metal and the second metal, can be set to 7% or more and 10% or less by mass.
[0043] In this embodiment, the proportion of the first metal nanoparticles with a particle size of 100 nm or less is 50% or more relative to the total number of the first metal nanoparticles. The smaller the particle size of the first metal nanoparticles, the larger the specific surface area of the nanoparticles, and the easier it is to sinter even at a lower temperature.
[0044] In addition, in the present embodiment, the average particle size of the nanoparticles of the second metal is less than 100nm. The smaller the average particle size of the nanoparticles of the second metal, the easier it is for the second metal to diffuse into the first metal and dissolve, and the time required for sintering can be shortened. In addition, the smaller the average particle size of the nanoparticles of the second metal, the easier it is for the second metal to dissolve into the first metal, and the changes in the electrical conductivity, thermal conductivity, heat resistance and other characteristics of the first metal caused by the nanoparticles of the second metal that have not dissolved remaining in the sintered body 103 after sintering can be suppressed.
[0045] The nanoparticle mounting material may further contain an organic solvent for imparting coating properties to the electrode and dispersibility to the nanoparticles, a dispersant for preventing aggregation of the nanoparticles during storage, and a reducing agent for removing an oxide film formed on the surface of the nanoparticles.
[0046] <Process>
[0047] The method for manufacturing a mounting structure in the present embodiment includes the step of bonding a device electrode of a semiconductor device and a lead frame electrode of a lead frame by sintering the first metal nanoparticles and the second metal nanoparticles using the nanoparticle mounting material.
[0048] (1) Nanoparticle mounting material preparation process
[0049] First, a nanoparticle mounting material including the nanoparticles of the first metal and the nanoparticles of the second metal is prepared. The nanoparticle mounting material may further include an organic solvent, a dispersant, a reducing agent, and the like.
[0050] (2) Nanoparticle mounting material supply process
[0051] Next, the nanoparticle mounting material is supplied to the lead frame electrode 104 on the lead frame 105 using a metal mask or the like. The lead frame electrode 104 can be formed of Cu or the like.
[0052] (3) Component placement process
[0053] Furthermore, the semiconductor element 101 is placed on the supplied nanoparticle mounting material so that the element electrode 102 is in contact with the nanoparticle mounting material. The element electrode 102 may have an outermost layer formed of Au or the like.
[0054] (4) Joining process
[0055] Finally, the lead frame 105 on which the semiconductor element 101 and the nanoparticle mounting material are mounted is placed in an airflow type heating furnace and heated in the air atmosphere. The heating conditions are not particularly limited, but can be set to, for example, 200° C. for about 20 minutes.
[0056] Thus, the nanoparticles of the first metal and the second metal in the nanoparticle mounting material are sintered to cause particle growth, forming a sintered body 103 composed of a collection of structures of more than 200 nm. At this time, the elements constituting the element electrode 102 diffuse into each other within a range of a thickness of about several nm from the interface between the element constituting the element electrode 102 and the first metal and the second metal, and the elements constituting the lead frame electrode 104 diffuse into each other within a range of a thickness of about several nm from the interface between the element constituting the lead frame electrode 104 and the first metal and the second metal, and the element electrode 102 and the lead frame electrode 104 are bonded to produce a mounting structure 108.
[0057] Example
[0058] The present invention is described in detail based on the examples, but the present invention is not limited to these examples.
[0059] [Example 1]
[0060] 1. Fabrication of the installation structure
[0061] Ag nanoparticles with an average particle size of 100 nm were prepared as nanoparticles of the first metal, and Sn nanoparticles with an average particle size of 100 nm, Sb nanoparticles with an average particle size of 100 nm, and Pd nanoparticles with an average particle size of 100 nm were prepared as nanoparticles of the second metal. When the nanoparticles of the first metal were observed using a scanning electron microscope (SEM), the proportion of nanoparticles with a particle size of 100 nm or less was 50% relative to the number of nanoparticles of the first metal observed.
[0062] The nanoparticles of the first metal and the nanoparticles of the second metal are mixed to prepare a nanoparticle mounting material by making the total amount of the nanoparticles of the first metal and the nanoparticles of the second metal 70% by mass, the amount of polyethylene glycol (average molecular weight of 200) as an organic solvent 29% by mass, and the total amount of the dispersant and the reducing agent 1% by mass. At this time, the nanoparticles of the first metal and the nanoparticles of the second metal are mixed at different ratios so that the total amount is 70% by mass to obtain a plurality of nanoparticle mounting materials.
[0063] A lead frame electrode made of Cu is arranged on the lead frame. In addition, the above-mentioned nanoparticle mounting material is poured into a metal mask with a length of 1 mm, a width of 1 mm, and a thickness of 50 μm arranged on the surface of the above-mentioned lead frame electrode. Furthermore, a semiconductor element having an element electrode formed of Au on the outermost layer is placed so that the above-mentioned element electrode is in contact with the above-mentioned nanoparticle mounting material. Afterwards, the lead frame carrying the above-mentioned semiconductor element is placed in an airflow type heating furnace and heated at 200° C. for 20 minutes in an atmospheric atmosphere to obtain a mounting structure.
[0064] In addition, the self-diffusion coefficient of Ag in Ag at 200°C is 10 -24 m 2 / sec, while the diffusion coefficient of Sn in Ag at 200°C is 10 -22 m 2 In addition, the diffusion coefficient of Sb in Ag at 200°C is 10 -25 m 2 / sec, and the diffusion coefficient of Pd in Ag at 200°C is 10 -31 m 2 / sec.
[0065] In addition, the solid solubility limit of Sn in Ag is 10 mass %.
[0066] 2. Evaluation
[0067] After the fabricated mounting structure is embedded in epoxy resin, mirror polishing is performed from the semiconductor element side using grinding paper and a buff to expose a cross section of the sintered body 103 of the nanoparticle mounting material formed by the above heating near the center in the thickness direction. The cross section is observed using SEM to observe the proportion of unsintered nanoparticles, the presence or absence of intermetallic compounds, and the residual state of nanoparticles of the second metal.
[0068] (Proportion of unsintered nanoparticles)
[0069] An image at 100,000 times magnification was taken using an SEM, and the ratio of particles having a particle size of 100 nm or less to the total number of particles observed in the field of view was calculated and defined as the ratio of unsintered nanoparticles.
[0070] When the ratio of the unsintered nanoparticles was smaller than the value when Sn as the second metal was not added, the result was considered as acceptable.
[0071] (Presence or absence of intermetallic compounds)
[0072] When a phase with different brightness is confirmed in the SEM image, energy dispersive X-ray analysis (EDX analysis) of the phase with different brightness is performed. When the phase with different brightness is a phase containing the first metal and the second metal, it is determined that an intermetallic compound is generated.
[0073] The case where no intermetallic compound was present was considered acceptable.
[0074] (Remaining nanoparticles of the second metal)
[0075] When a phase with different brightness is confirmed in the above SEM image, energy dispersive X-ray analysis (EDX analysis) of the phase with different brightness is performed. When the phase with different brightness is a phase consisting of substantially only the second metal, it is determined that nanoparticles of the second metal are not sintered and remain.
[0076] The case where no second metal remained was considered acceptable.
[0077] Table 1 shows the types of the first metal and the second metal in Example 1, the mass ratio (content) of the second metal (Sn) nanoparticles relative to the total mass of the first metal (Ag) nanoparticles and the second metal (Sn) nanoparticles, and the results of the above evaluation.
[0078] [Table 1]
[0079]
[0080] Figure 2 The cross-sectional SEM image of the sintered body 103 in the mounting structure of Example 1-4 is shown in FIG. Figure 3 2 shows a cross-sectional SEM image of the sintered body 103 in the mounting structure of Comparative Example 1-1.
[0081] Figure 2 In the structure after joining, except for the portion indicated by the dotted line, no particles with a particle size of 100 nm or less were found. In the sintered body 103 in the mounting structure of Example 1-4, it was confirmed that the nanoparticle mounting material was sintered well. On the other hand, in Figure 3 In the figure, the proportion of the tissue containing particles with a particle size of 100 nm or less represented by the dotted line is Figure 2 In the sintered body 103 in the mounting structure of Comparative Example 1-1, it was confirmed that the sintering of the nanoparticle mounting material was not so good.
[0082] In addition, as is clear from Table 1, the proportion of unsintered nanoparticles in the mounting structures of Examples 1-1 to 1-4 is lower than that in the mounting structure of Comparative Example 1-1. In addition, no generation of intermetallic compounds (Ag5Sn, etc.) or residual nanoparticles of the second metal (Sn) was found.
[0083] The nanoparticle mounting materials used in the preparation of the mounting structures of Examples 1-1 to 1-4 have the following common features. First, a nanoparticle mounting material containing nanoparticles of a first metal and nanoparticles of a second metal solid-dissolved in the first metal is used. In addition, the second metal is a metal whose diffusion coefficient in the first metal is greater than the self-diffusion coefficient of the first metal. In addition, the mass ratio of the nanoparticles of the second metal relative to the total mass of the first metal and the second metal is below the solid solubility limit of the first metal.
[0084] On the other hand, in Comparative Example 1-2, in which the content of the second metal (Sn) relative to the total mass of the nanoparticles of the first metal (Ag) and the nanoparticles of the second metal (Sn) was 12.5 mass %, which was above the solid solubility limit of Sn in Ag, although no unsintered nanoparticles were observed, the generation of intermetallic compounds, namely Ag5Sn, was discovered in the sintered body 103.
[0085] In addition, in Comparative Examples 1-3 and 1-4, each containing Sb and Pd whose diffusion coefficient in Ag is smaller than the self-diffusion coefficient of Ag in Ag, the proportion of unsintered nanoparticles is greater than that in Comparative Example 1-1. When the unsintered nanoparticles are measured, the residues of Sb and Pd are found.
[0086] [Example 2]
[0087] In Example 2, a mounting structure was produced and evaluated in the same manner as in Example 1 except that the second metal was made Cu, Pb, and Ge.
[0088] In addition, the diffusion coefficient of Cu in Ag at 200°C is 10 -17 m 2 / sec, and the diffusion coefficient of Pb in Ag at 200°C is 10 -22 m 2 / sec, and the diffusion coefficient of Ge in Ag at 200°C is 10 -22 m 2 Each of these diffusion coefficients is larger than the self-diffusion coefficient of Ag in Ag at 200°C.
[0089] Furthermore, the mixing ratio of the nanoparticles of the second metal is adjusted so that the mass of Cu, Pb, and Ge relative to the total mass of Ag becomes half of the solid solubility limit at 200° C. in the equilibrium diagram between Ag and each element.
[0090] Table 2 shows the types of the first metal and the second metal in Example 2, the mass ratio (content) of the nanoparticles of the second metal (Sn) relative to the mass total of the nanoparticles of the first metal (Ag) and the nanoparticles of the second metal (Sn), and the results of the above evaluation. In addition, in order to make comparison easier, the nanoparticle mounting materials used in Example 1-2 and Comparative Example 1-1 and the evaluation results are also listed in Table 2.
[0091] [Table 2]
[0092]
[0093] As is clear from Table 2, even when a metal other than Sn is used as the second metal, the proportion of unsintered nanoparticles in the mounting structures of Examples 2-1 to 2-3 is lower than that of the mounting structure of Comparative Example 1-1. In addition, no generation of intermetallic compounds or residual nanoparticles of the second metal were observed.
[0094] The nanoparticle mounting materials used in the preparation of the mounting structures of Examples 2-1 to 2-3 have the following common features. First, a nanoparticle mounting material containing nanoparticles of a first metal and nanoparticles of a second metal solid-dissolved in the first metal is used. In addition, the second metal is a metal whose diffusion coefficient in the first metal is greater than the self-diffusion coefficient of the first metal. In addition, the mass ratio of the nanoparticles of the second metal relative to the total mass of the first metal and the second metal is below the solid solubility limit of the first metal.
[0095] In Example 2-1 in which Cu was used as the second metal, the proportion of unsintered nanoparticles decreased despite the small weight ratio of the second metal. This is considered to be because the diffusion coefficient of Cu in Ag is considerably larger than that of other elements.
[0096] [Example 3]
[0097] In Example 3, a mounting structure was produced and evaluated in the same manner as in Example 1 except that the first metal was Cu and the second element was Ge.
[0098] In addition, the diffusion coefficient of Ge in Cu at 200°C is 10 -23 m 2 / sec, and the self-diffusion coefficient of Cu in Cu at 200°C is 10 -29 m 2 The diffusion coefficient of Ge in Cu at 200°C is larger than the self-diffusion coefficient of Cu in Cu at 200°C.
[0099] Furthermore, the mixing ratio of the nanoparticles of the second metal (Ge) was adjusted so that the mass of Ge relative to the total mass of Cu became half of the solid solubility limit at 200° C. in the equilibrium diagram of Cu and Ge.
[0100] Table 3 shows the types of the first metal and the second metal in Example 3, the mass ratio (content) of the second metal (Ge) nanoparticles relative to the total mass of the first metal (Cu) nanoparticles and the second metal (Ge) nanoparticles, and the results of the above evaluation.
[0101] [Table 3]
[0102]
[0103] As is clear from Table 3, even when a metal other than Ag is used as the first metal, the proportion of unsintered nanoparticles in the mounting structure of Example 3-1 is lower than that of the mounting structure of Comparative Example 3-1. In addition, no generation of intermetallic compounds or residual nanoparticles of the second metal were found.
[0104] The nanoparticle mounting material used in the preparation of the mounting structure of embodiment 3-1 has the following characteristics. First, a nanoparticle mounting material containing nanoparticles of a first metal and nanoparticles of a second metal solid-dissolved in the above-mentioned first metal is used. In addition, the above-mentioned second metal is a metal whose diffusion coefficient in the above-mentioned first metal is greater than the self-diffusion coefficient of the above-mentioned first metal. In addition, the mass ratio of the nanoparticles of the above-mentioned second metal relative to the total mass of the above-mentioned first metal and the above-mentioned second metal is below the solid-dissolution limit of the above-mentioned first metal.
[0105] (as a whole)
[0106] Although the lead frame 105 is used in the above description, a metal member may be used, for example, a heat sink may be used.
[0107] Industrial Applicability
[0108] According to the mounting structure of the present invention, it is possible to provide a mounting structure required in devices accompanied by large heat generation such as power devices, which shortens the time required for bonding, reduces thermal damage to peripheral components, and ensures the physical properties of the metal of the nanoparticles.
[0109] -Description of Reference Numerals-
[0110] 101 Semiconductor Components
[0111] 102 Component Electrode
[0112] 103 Sintered body
[0113] 104 Lead frame electrode
[0114] 105 Lead frame
[0115] 108 Install the structure.
Claims
1. A mounting structure, comprising: A semiconductor element having an element electrode; Metal components; and a sintered body that joins the semiconductor element and the metal member, The sintered body includes: a first metal and a second metal solid-dissolved in the first metal, The second metal is a metal having a diffusion coefficient in the first metal greater than a self-diffusion coefficient of the first metal, The content of the second metal relative to the total mass of the first metal and the second metal in the sintered body is equal to or less than the solid solubility limit of the second metal in the first metal. The first metal is Ag and the second metal is Pb, or the first metal is Cu and the second metal is Ge.
2. The mounting structure according to claim 1, wherein: The metal component is a lead frame or a heat sink.
3. A nanoparticle mounting material, At least comprising: nanoparticles of a first metal and nanoparticles of a second metal solid-dissolved in the first metal, The proportion of the first metal nanoparticles having a particle size of 100 nm or less relative to the total number of the first metal nanoparticles is 50% or more, The average particle size of the nanoparticles of the second metal is less than 100 nm, The second metal is a metal having a diffusion coefficient in the first metal greater than a self-diffusion coefficient of the first metal, The mass ratio of the second metal to the total mass of the first metal and the second metal is below the solid solubility limit of the first metal. The first metal is Ag and the second metal is Pb, or the first metal is Cu and the second metal is Ge.