New composite air-cooled durable silicon-manganese furnace

By setting iron outlet holes higher than the bottom of the furnace in the smelting electric furnace and using structures such as refractory brick layer and carbon brick layer, the furnace body problem is solved, extending the service life and improving high temperature resistance, achieving higher safety Sexual and economical.

CN111424133BActive Publication Date: 2024-11-15ZHENGZHOU LIANSHENG KILN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010411198.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-15
Publication Date
2024-11-15
Estimated Expiration
2040-05-15

AI Technical Summary

Technical Problem

The existing smelting electric furnace body is prone to furnace penetration after a long period of use, resulting in a short service life and high cost.

Method used

A new composite air-cooled durable silicon manganese furnace was designed. By setting iron outlet holes higher than the upper surface of the furnace bottom, the reserved constant temperature molten iron increases the reduction temperature and blocks the impact of electrode insertion too deep on the furnace bottom, and at the furnace bottom and The furnace wall is equipped with refractory brick layer, carbon brick layer, clay brick protective layer, air-cooled pipe and seam paste core layer to improve high temperature resistance and prevent passing through the furnace.

Benefits of technology

It effectively avoids the phenomenon of furnace penetration, extends the service life of the furnace body, and improves the high temperature resistance and leakage resistance of the furnace bottom and furnace wall, and enhances structural strength and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111424133B_ABST
    Figure CN111424133B_ABST
Patent Text Reader

Abstract

The present invention relates to a novel composite air-cooled durable silicon-manganese furnace, comprising a furnace wall and a furnace bottom, wherein an iron tapping hole is arranged on the furnace wall, and the position of the iron tapping hole is higher than the upper surface of the furnace bottom. The present invention breaks the traditional setting of the position of the iron tapping hole, and can block the influence of the electrode inserted too deeply on the furnace bottom while increasing the reduction temperature by using the reserved constant temperature molten iron below the iron tapping hole, thereby protecting the furnace bottom; by arranging clay bricks, carbon bricks are avoided from being damaged when the furnace is baked; carbon bricks and novel composite caulking paste are arranged alternately, and a caulking paste core layer is arranged in the furnace wall, and the high temperature resistance and high strength performance of the caulking paste are utilized to improve the high temperature resistance of the furnace wall and the furnace bottom, thereby comprehensively improving the structural strength and anti-leakage performance of the furnace wall and the furnace bottom, thereby extending the service life of the furnace body, and having a high safety factor; it can be used in any furnace type with different parameters, especially for calcium carbide furnaces and ferrosilicon furnaces with relatively small furnace type parameters to transform silicon-manganese alloy furnace types, which can effectively increase the furnace chamber and process size, and improve economic indicators.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of smelting electric furnaces, and in particular to a novel composite air-cooled and durable silicon-manganese furnace. Background Art

[0002] The smelting electric furnace is a steelmaking equipment that uses electricity as energy. Due to its high efficiency in dephosphorization and desulfurization, it is increasingly used in production.

[0003] However, due to the high temperature of molten iron in the furnace, the requirements for the furnace body are very high, resulting in a short service life of the currently commonly used furnace body. The furnace body structure in the prior art is prone to furnace penetration after long-term use, resulting in the furnace body being scrapped, causing huge losses to the company. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a novel composite air-cooled and durable silicon-manganese furnace, which avoids the occurrence of furnace penetration and greatly prolongs the service life.

[0005] The present invention is achieved through the following technical scheme, providing a novel composite air-cooled durable silicon manganese furnace, comprising a furnace wall and a furnace bottom, wherein an iron tapping hole is arranged on the furnace wall, and the position of the iron tapping hole is higher than the upper surface of the furnace bottom.

[0006] In the prior art, in order to minimize waste and reduce the residual molten iron in the furnace as much as possible, the tap hole is set below the furnace bottom or at the same height as the furnace bottom. However, the present solution sets the tap hole to be higher than the upper surface of the furnace bottom, so that a portion of molten iron is retained in the furnace. The reserved constant temperature molten iron below the tap hole is used to increase the reduction temperature and block the influence of the electrode inserted too deeply on the furnace bottom, thereby protecting the furnace bottom.

[0007] As an optimization, the furnace bottom includes a refractory brick layer and a carbon brick layer located above the refractory brick layer, the upper surface of the carbon brick layer is lower than the iron tapping hole, and a clay brick protective layer is laid on the upper surface of the carbon brick layer. This optimization scheme improves the high temperature resistance of the furnace bottom by setting the carbon brick layer and the refractory brick layer to prevent the furnace from being penetrated, and by setting the clay brick protective layer on the carbon brick layer, the carbon brick layer is protected by the clay brick protective layer when the furnace is baked to avoid the high temperature flame during the baking of the furnace from damaging the carbon brick layer. When the first furnace of molten iron is smelted, the clay bricks melt in the molten iron, thereby forming a height difference between the upper surface of the furnace bottom and the iron tapping hole.

[0008] As an optimization, a refractory aggregate layer and a refractory board located below the refractory aggregate layer are provided below the refractory brick layer. This optimization scheme further improves the refractory performance of the furnace bottom by providing the refractory board, and facilitates the laying of refractory aggregates. By laying refractory aggregates, not only the refractory performance of the furnace bottom is improved, but also leveling is facilitated, which is convenient for the laying of the refractory brick layer.

[0009] As an optimization, the carbon brick layer includes several layers of carbon bricks and a new composite caulking paste layer between two adjacent layers of carbon bricks, and the new composite caulking paste is filled between the carbon bricks in the same layer. This optimization scheme uses the new composite caulking paste between the brick joints to bond the carbon bricks as a whole, and the new composite caulking paste layer is set to greatly improve the high temperature resistance of the furnace bottom and avoid furnace penetration.

[0010] As an optimization, an air cooling pipe is provided in the furnace bottom, and one end of the air cooling pipe is connected to the cold air supply device. This optimization scheme uses cold air to cool the furnace bottom by providing an air cooling pipe to avoid high temperature penetrating the furnace. At the same time, compared with the water cooling of the prior art, it avoids pipeline corrosion, prolongs the service life of the air cooling pipe, and further prolongs the service life of the furnace body.

[0011] As an optimization, a thermocouple is also provided in the furnace bottom above the air cooling pipe. This optimization scheme facilitates the detection of the temperature of the furnace bottom by providing a thermocouple so as to adjust the cold air.

[0012] As an optimization, the furnace wall includes an inner refractory brick layer and an outer refractory brick layer, and a caulking paste core layer located between the inner refractory brick layer and the outer refractory brick layer and fixing the inner refractory brick layer and the outer refractory brick layer together. This optimization scheme uses caulking paste to firmly fix the inner refractory brick layer and the outer refractory brick layer together, and through the high strength and high temperature resistance of the caulking paste core layer, high-temperature penetration of the furnace is avoided. Due to the setting of the caulking paste core layer, the thickness of the inner refractory brick layer can be reduced, thereby increasing the volume inside the furnace.

[0013] As an optimization, the outer surface of the outer refractory brick layer is provided with a refractory aggregate layer and a refractory layer in sequence from the inside to the outside. This optimization scheme further improves the fire resistance of the furnace wall and prevents leakage through the furnace by providing a refractory aggregate layer and a refractory layer on the outer wall of the outer refractory brick layer.

[0014] As an optimization, the tap hole bricks are cast and fixed on the furnace wall through the anaerobic casting layer, and the part of the tap hole bricks extending out of the furnace wall is covered by the anaerobic casting layer, and the tap hole is opened on the tap hole and the anaerobic casting layer. This optimization scheme uses the anaerobic casting layer to protect the tap hole bricks from oxidation and prolong their service life.

[0015] As an optimization, the tapping end of the tapping hole is fixedly connected with a tapping pipe. This optimization scheme arranges the tapping pipe so that the molten iron outflow position is a certain distance from the furnace body, thereby preventing the molten iron from flowing down the furnace wall, thereby avoiding damage to the furnace wall and extending the service life.

[0016] The beneficial effects of the present invention are as follows: it breaks the traditional setting of the position of the iron tapping hole, and utilizes the reserved constant temperature molten iron below the iron tapping hole to increase the reduction temperature while blocking the influence of the electrode inserted too deeply on the furnace bottom, thereby protecting the furnace bottom; by arranging clay bricks, it avoids damage to carbon bricks during furnace baking; carbon bricks and new composite caulking paste are alternately arranged, and a caulking paste core layer is arranged in the furnace wall. The high temperature resistance and high strength properties of the caulking paste are utilized to improve the high temperature resistance of the furnace wall and the furnace bottom, thereby comprehensively improving the structural strength and leakage-proof performance of the furnace wall and the furnace bottom, thereby extending the service life of the furnace body, and the safety factor is relatively high; the present invention can be used in any furnace type with different parameters, especially for calcium carbide furnaces and ferrosilicon furnaces with smaller furnace parameters to transform silicon-manganese alloy furnaces, which can effectively increase the furnace chamber and process dimensions, and improve economic indicators. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the structure of the present invention;

[0018] Figure 2 This is a schematic diagram of the distribution of the tapholes of the present invention;

[0019] As shown in the figure:

[0020] 1. Outer refractory brick layer, 2. Refractory layer, 3. Refractory aggregate layer, 4. Electrode paste core layer, 5. Inner refractory brick layer, 6. Clay brick protective layer, 7. Carbon brick, 8. Electrode paste layer, 9. Tap hole, 10. Tap hole brick, 11. Anaerobic casting layer, 12. Tap pipe, 13. Second refractory brick layer, 14. First refractory brick layer. DETAILED DESCRIPTION

[0021] In order to clearly illustrate the technical features of this solution, this solution is described below through a specific implementation method.

[0022] like Figure 1 The new composite air-cooled durable silicon-manganese furnace shown comprises a steel shell and a furnace lining located in the steel shell. The furnace lining comprises a furnace wall and a furnace bottom. The furnace wall is cylindrical. Two iron tapping holes 9 are arranged along the circumferential direction on the furnace wall. The central angle corresponding to the two iron tapping holes is 120°. The position of the iron tapping holes is higher than the upper surface of the furnace bottom.

[0023] The furnace bottom includes a refractory brick layer and a carbon brick layer located above the refractory brick layer. The upper surface of the carbon brick layer is 150~200mm lower than the iron tapping hole, and a clay brick protective layer 6 is laid on the upper surface of the carbon brick layer. The edge of the carbon brick layer extends upward along the inner wall of the furnace wall to a certain height. When the furnace body is baked, the clay bricks of the clay brick protective layer are used to protect the carbon brick layer and the lower part of the inner wall of the furnace wall. When the first batch of molten iron is smelted after the furnace is opened, the clay bricks are melted by the high-temperature molten iron, so that a height difference of 150~200mm is formed between the iron tapping hole and the furnace bottom for retaining the molten iron.

[0024] The refractory brick layer of this embodiment includes a first refractory brick layer 14 and a second refractory brick layer 13 located above the first refractory brick layer, the first refractory brick layer includes several layers of secondary high-aluminum bricks, the second refractory brick layer includes several layers of primary high-aluminum bricks, and the brick joints between adjacent high-aluminum bricks are filled with refractory clinker powder. A refractory aggregate layer and a refractory board located below the refractory aggregate layer are also provided below the first refractory brick layer, and the refractory board of this embodiment is a double-layer asbestos board.

[0025] The carbon brick layer includes several layers of carbon bricks 7 and a new composite caulking paste layer between two adjacent layers of carbon bricks, the new composite caulking paste layer is an electrode paste layer 8, the carbon bricks and the electrode paste layer are arranged alternately up and down, the upper and lower adjacent layers of carbon bricks are staggered by 35°~45°, and the new composite caulking paste is filled between the carbon bricks of the same layer, the new composite caulking paste is an electrode paste. By arranging the electrode paste layer on the carbon brick layer, the heat resistance of the furnace bottom is improved, the thickness of the refractory brick layer can be reduced, and the furnace volume is increased.

[0026] The furnace bottom is equipped with a coil-type air cooling pipe, which is made of seamless steel pipe. The air cooling pipe is located at 4 to 6 layers of refractory bricks below the bottom of the carbon brick layer. Both ends of the air cooling pipe extend out of the electric furnace, and one end is connected to the cold air supply device. The cold air provided by the cold air supply device enters the air cooling pipe to cool the furnace bottom. A thermocouple is also provided above the air cooling pipe in the furnace bottom to monitor the temperature of the furnace bottom.

[0027] The furnace wall includes an inner refractory brick layer 5, an electrode paste core layer 4, an outer refractory brick layer 1, a refractory aggregate layer 3 and a refractory layer 2 which are arranged in sequence from the inside to the outside. The inner refractory brick layer and the outer refractory brick layer are fixed as a whole by a grouting core layer. The grouting core layer is the electrode paste core layer 4, the grouting paste is the electrode paste, the refractory layer 2 is an asbestos board, and the refractory aggregate layer 3 is a high-alumina aggregate with a radial thickness of 60 mm.

[0028] The tap hole brick 10 is cast and fixed on the furnace wall through the anaerobic casting layer 11, and the part of the tap hole brick extending out of the furnace wall is covered by the anaerobic casting layer. The tap hole and the anaerobic casting layer are provided with tap holes, and the tapping end of the tap hole is fixedly connected with a tapping pipe 12. The tap hole brick of this embodiment is a semi-graphite carbon-silicon carbide tap hole brick, and the anaerobic casting layer is a corundum castable, which not only ensures the structural strength, but also utilizes the oxygen-free property of the corundum castable.

[0029] The masonry method of the durable silicon-manganese furnace of this embodiment includes the following aspects:

[0030] 1. Inspection before masonry: Check the furnace shell before construction. The total horizontal flatness of the furnace shell bottom plate is allowed to have a deviation of ≤5mm in the longitudinal and transverse length. Construction can only be carried out after it meets the design requirements and is accepted in accordance with these regulations.

[0031] 2. Leveling the furnace bottom: Before laying the furnace lining, the refractory aggregate is used to level the furnace bottom. The thickness of the refractory aggregate layer at the furnace bottom is 60~70mm;

[0032] 3. Dry-laid refractory bricks: Lay out the lines on the finished furnace bottom leveling layer to find the center of the furnace body.

[0033] Lines, side lines, etc. are laid radially from the center to the surroundings. Refractory bricks are laid by dry laying. The brick joints are less than 2mm. The brick joints are filled with dry and homogeneous refractory fine powder to ensure flatness. The vertical and horizontal brick joints are staggered by half a brick. After the furnace bottom is dry-laid for one layer, the brick joints are filled with refractory fine powder so that the brick joints are filled with refractory clinker powder. After cleaning, they are laid upward layer by layer. The joints around the furnace bottom and the asbestos board are naturally filled with refractory aggregates without ramming.

[0034] 4. Laying the air cooling pipe at the bottom of the furnace: According to the different sizes of the furnace, the air cooling pipe is laid at 4 to 6 layers of high alumina bricks below the carbon bricks at the bottom of the furnace;

[0035] 5. Masonry of high-alumina bricks for furnace walls: Use phosphate refractory mud to masonry high-alumina bricks. The vertical joints between the upper and lower layers of bricks should be staggered by half a brick, the masonry joints should be less than 2mm, the maximum radius deviation should be less than 5mm, and the vertical deviation should be less than 5mm;

[0036] 6. Carbon brick masonry of furnace bottom electric furnace:

[0037] Laying out the lines: The furnace bottom carbon bricks are two layers. Before laying out the center line of the furnace bottom, the center line coincides with the center line of one of the iron outlets. Use carbon cement to lay out the carbon bricks of the furnace bottom.

[0038] Masonry sequence: Carbon bricks are laid with wide seams. The gaps are filled and compacted with electrode paste. After compaction, a layer of electrode paste with a thickness of 60-100 mm is laid on the top of the carbon bricks. The upper and lower adjacent layers of carbon bricks are laid with a staggered seam of 35-45 degrees.

[0039] 7. Furnace bottom thickness control: double-layer asbestos board thickness is 20mm, refractory aggregate thickness is 40mm, and it is strictly compacted and leveled, and the diameter size deviation is not more than 5mm;

[0040] 8. After the three-layer high thermal conductivity electric furnace carbon bricks are built, the graphite and semi-graphite silicon carbide bricks are laid.

[0041] Close the furnace mouth, find the level before masonry, use carbon cement to build, if the carbon cement is too thin, add graphite powder to adjust, after the furnace mouth combined carbon bricks are built, build the furnace wall electric furnace carbon bricks, the gap is 80mm, the gap is compacted with cold ramming paste, the gap radius size deviation is less than 5mm, and the vertical size deviation is less than 5mm;

[0042] 9. Laying of high-alumina bricks on the furnace wall: After the laying of ring-shaped carbon bricks is completed, lay the ring-shaped high-alumina bricks.

[0043] Pause after laying 6 layers to knot the electrode paste between the ring-laid carbon bricks and the ring-laid high-alumina bricks. Tie knots while laying high-alumina bricks. When the construction is completed to the upper plane of the ring-laid carbon bricks, tie knots of the corundum refractory castables on both sides of the furnace eye. The thickness of each layer of corundum castables shall not exceed 200mm and shall be compacted with a tamping machine.

[0044] 10. When the construction reaches the upper surface of the ring-laid carbon bricks, clean up and prepare to start tamping the new composite grout; the ring-laid carbon bricks and the bottom carbon bricks are connected with carbon cement for leveling;

[0045] 11. Ring-laid high-alumina bricks: When laying the first layer of high-alumina bricks, use carbonaceous mortar for masonry to facilitate durability.

[0046] The bonding of refractory materials and carbon materials, the mortar joint is less than 2mm, the high-alumina brick ring is built with 16 layers, except for the first layer, the remaining parts are built with phosphate refractory mud, the mortar joint is less than 2mm, the radius size deviation is less than 5mm, and the vertical size deviation is less than 5mm; after the high-alumina brick ring is completed, clay bricks are used to set back and build the bell mouth, the clay brick mortar joint is less than 2mm, the bell mouth is evenly set back, and refractory aggregates are filled while building until the flat part of the upper mouth of the furnace shell;

[0047] 12. Construction of aluminum silicate board: Before pasting aluminum silicate board, remove the floating rust and debris on the surface of the furnace shell, bond it with refractory mud, and then paste 2 layers of asbestos board on the surface of aluminum silicate board with staggered seams. The adhesive is refractory mud mixed with water glass;

[0048] 13. Install 4 K-type thermocouples above the high-aluminum brick on the air-cooling pipe. The temperature measurement range is

[0049] 0-1200 degrees Celsius, the length of the galvanic couple is determined according to the pre-buried protection tube; the pre-buried galvanic protection tube is made of silicon nitride and can be assembled in sections. The inner diameter of the protection tube is not less than 20mm, and the galvanic couple and the furnace shell are insulated.

[0050] 14. Install three Φ1mm tungsten wires at the joints between the upper part of the high-alumina brick and the carbon brick. The length of the tungsten wire is 4 meters. Measure the voltage of the three electrodes to the ground. The tungsten wire and the furnace shell are insulated.

[0051] Of course, the above description is not limited to the above examples. Technical features not described in the present invention can be achieved by or by using existing technologies, which will not be described here. The above embodiments and drawings are only used to illustrate the technical scheme of the present invention and are not limitations of the present invention. The present invention is described in detail with reference to the preferred implementation methods. Ordinary technicians in this field should understand that changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention do not depart from the purpose of the present invention, and should also fall within the scope of protection of the claims of the present invention.

Claims

1. A novel composite air-cooled durable silicon-manganese furnace, comprising a furnace wall and a furnace bottom, wherein an iron tapping hole (9) is provided on the furnace wall, characterized in that: The position of the tap hole is higher than the upper surface of the furnace bottom, and the reserved constant temperature molten iron below the tap hole is used to increase the reduction temperature while preventing the influence of the electrode inserted too deeply on the furnace bottom; The furnace bottom comprises a refractory brick layer and a carbon brick layer located above the refractory brick layer, the upper surface of the carbon brick layer is lower than the iron outlet, and a clay brick protective layer (6) is laid on the upper surface of the carbon brick layer; when the furnace is baked, the clay brick protective layer is used to protect the carbon brick layer to prevent the high temperature flame during the baking of the furnace from damaging the carbon brick layer. When the first furnace of molten iron is smelted, the clay bricks melt in the molten iron, thereby forming a height difference between the upper surface of the furnace bottom and the iron outlet.

2. The novel composite air-cooled durable silicon-manganese furnace according to claim 1 is characterized in that: A refractory aggregate layer and a refractory board located below the refractory aggregate layer are arranged below the refractory brick layer.

3. The novel composite air-cooled durable silicon-manganese furnace according to claim 1 is characterized in that: The carbon brick layer comprises a plurality of layers of carbon bricks (7) and a new type of composite caulking paste layer located between two adjacent layers of carbon bricks, and the new type of composite caulking paste is filled between the carbon bricks in the same layer.

4. The novel composite air-cooled durable silicon-manganese furnace according to claim 1 is characterized in that: An air cooling pipe is arranged in the furnace bottom, and one end of the air cooling pipe is connected to the cold air supply device.

5. The novel composite air-cooled durable silicon-manganese furnace according to claim 4 is characterized in that: A thermocouple is also provided in the furnace bottom above the air cooling pipe.

6. The novel composite air-cooled durable silicon-manganese furnace according to claim 1 is characterized in that: The furnace wall comprises an inner refractory brick layer (5) and an outer refractory brick layer (1), and a caulking core layer (4) located between the inner refractory brick layer and the outer refractory brick layer and fixing the inner refractory brick layer and the outer refractory brick layer together.

7. The novel composite air-cooled durable silicon-manganese furnace according to claim 6 is characterized in that: The outer surface of the outer refractory brick layer is provided with a refractory aggregate layer (3) and a refractory layer (2) in sequence from the inside to the outside.

8. The novel composite air-cooled durable silicon-manganese furnace according to claim 1 is characterized in that: A tap hole brick (10) is cast and fixedly connected to the furnace wall through an anaerobic casting layer (11), and the portion of the tap hole brick extending out of the furnace wall is covered by the anaerobic casting layer. Tap holes are provided on the tap hole and the anaerobic casting layer.

9. The novel composite air-cooled durable silicon-manganese furnace according to claim 8 is characterized in that: An iron outlet pipe (12) is fixedly connected to the iron outlet end of the iron outlet hole.