A processing technology for force-limiting rod assembly
The cold heading die and surface treatment process for force limiting rod assemblies address inefficiencies in traditional methods by enhancing production efficiency and quality through streamlined processing.
Patent Information
- Application Number
- CN202010781349.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-08-06
AI Technical Summary
Traditional force limiter assemblies are costly, time-consuming, and inefficient, requiring multiple equipment and processes, with high scrap rates and labor intensity, failing to meet customer demands.
A force limiting rod assembly processing technology utilizing cold heading dies and surface treatment processes, including rough drawing, annealing, cold forging, and electroplating, to streamline production and enhance efficiency.
The new process significantly improves production efficiency by replacing traditional complex methods, reducing costs and manpower requirements while ensuring high-quality output.
Smart Images

Figure CN111940652B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of force-limiting rod processing, in particular to a force-limiting rod assembly processing technology. Background Art
[0002] Traditional force limiter assemblies are completed through stamping dies and machining, which require multiple equipment and multiple processes to complete production and processing. The entire process is very costly and takes a certain amount of time. There is a very high scrap rate, the process is complicated, and it requires a lot of manpower, material resources and time. In addition, the production efficiency is slow and cannot keep up with customer needs and production rhythm. Summary of the invention
[0003] In order to overcome the deficiencies of the prior art, the present invention provides a force limiting rod assembly processing technology, which can complete the processing of the force limiting rod assembly by using a cold heading die and a surface treatment process, replacing the traditional complex processing technology and greatly improving the production efficiency.
[0004] In order to achieve the above purpose, a force limiting rod assembly processing technology is designed, which is characterized by: the specific process flow is as follows:
[0005] (1) The raw material is subjected to the first rough drawing process, and the diameter of the raw material is controlled to be φ = 11.5 mm;
[0006] (2) subjecting the raw material after the first rough drawing to the first spheroidizing annealing process, the annealing temperature is 710°C, and the temperature is kept for 7 hours;
[0007] (3) The raw material after the first spheroidizing annealing is subjected to a second rough drawing process, and the diameter of the raw material is controlled to be φ = 10.5 mm;
[0008] (4) subjecting the raw material after the second rough drawing to a second spheroidizing annealing process at a temperature of 710°C and keeping the temperature for 7 hours;
[0009] (5) The raw material after the second spheroidizing annealing is subjected to a fine drawing process, and the diameter of the finished wire is controlled to be φ = 10.15 mm;
[0010] (6) Cutting the finished wire after fine drawing into force-limiting rod assembly raw material segments of specified sizes;
[0011] (7) The raw material section of the force limiting rod assembly is pressed into a finished product of the force limiting rod assembly through four sets of cold forging dies;
[0012] (8) Performing surface treatment on the finished product of the force limiting rod assembly;
[0013] (9) The finished force limiter assembly after surface treatment is subjected to appearance inspection. If qualified, it is packaged and put into storage; if unqualified, it is scrapped.
[0014] The outer diameter of the tooth of the finished product of the force limiting rod assembly is Ф15.35±0.15; the surface profile is 0.15; the tooth width is 2×(5±0.3); the total length is 45.9±0.3; the roughness is Rz15 size 2×(≥2.75); the diameter is Ф6.6±0.05; the tooth profile direction tolerance is ±1°; the torque is 69.6±5N.m (360°); and the torque requirement is ≥5 turns (1800°).
[0015] The surface treatment process is an electroplating process, wherein the coating thickness is ≥8 μm; the electroplating solution is DIPSOL NT-200, zinc (ZN): 8-14 g / L, sodium hydroxide: 110-140 g / L; the passivation solution is Finidip 124, with a concentration of 35±5 ml / L; the electroplating temperature is 23±5°C; the time is 25±5s; the sealing temperature is 25±5°C; the specific gravity is 0.80-0.90; and the centrifuge is performed once.
[0016] The cold heading die comprises a first-station cold heading die, a second-station cold heading die, a third-station cold heading die and a fourth-station cold heading die. The first-station cold heading die comprises a first upper die and a first lower die. The first upper die consists of a first upper die punch shell and a first upper die punch carbide. A T-shaped through hole is arranged in the first upper die punch shell, and the first upper die punch carbide is embedded at the bottom of the first upper die punch shell; the first lower die consists of a first lower die shell, a first lower die upper middle sleeve, a first lower die upper carbide, a first lower die lower middle sleeve, a first lower die lower carbide, a first lower die first rear pad, a first lower die second rear pad, a first lower die third rear pad, a first lower die core and a first lower die lock nut. The first lower die is provided with a first lower die upper middle sleeve, a first lower die lower middle sleeve, a first lower die first rear pad, a first lower die second rear pad and a first lower die third rear pad from top to bottom. The first lower die upper middle sleeve has a A first lower die upper hard alloy is embedded, a first lower die lower hard alloy is embedded in the first lower die lower middle sleeve, and the height of the first lower die upper hard alloy and the first lower die lower hard alloy is consistent with the height of the first lower die upper middle sleeve and the first lower die lower middle sleeve, a first lower die core is arranged in the first lower die upper hard alloy, and one end of the first lower die core is flush with the upper end surfaces of the first lower die upper middle sleeve and the first lower die upper hard alloy, and the other end of the first lower die core passes through the first lower die upper hard alloy, the first lower die lower hard alloy, the first lower die first rear pad, the first lower die second rear pad and the first lower die third rear pad from top to bottom and is located at the lower part outside the first lower die third rear pad; a first lower die lock nut is arranged on the outer side of the lower part of the first lower die second rear pad, and the first lower die outer shell is arranged on the outer side of the first lower die lock nut, the first lower die second rear pad, the first lower die first rear pad, the first lower die lower middle sleeve and the first lower die upper middle sleeve.
[0017] The second station cold heading die comprises a second upper die and a second lower die, the second upper die is composed of a second upper die die shell, a second upper die die hard alloy, the second upper die is composed of a second upper die die back pad, and a second upper die die core, the second upper die die shell has a groove, the groove is embedded with a second upper die die back pad, the lower end of the second upper die die back pad abuts against one end of the second upper die die core, and the other end of the second upper die die core is sleeved with a second upper die die hard alloy on the outer side, the second upper die die shell has a groove, the groove is embedded with a second upper die die back pad, the lower end of the second upper die die back pad abuts against one end of the second upper die die core, and the other end of the second upper die die core is sleeved with a second upper die die hard alloy on the outer side, The second upper die punch carbide is embedded in the bottom of the second upper die punch shell; the second lower die is composed of the second lower die shell, the second lower die upper middle sleeve, the second lower die upper carbide, the second lower die lower middle sleeve, the second lower die lower carbide, the second lower die first rear pad, the second lower die second rear pad, the second lower die third rear pad, the second lower die core, and the second lower die lock nut. The second lower die is respectively provided with the second lower die upper middle sleeve, the second lower die lower middle sleeve, the second lower die first rear pad, the second lower die third rear pad, the second lower die core, and the second lower die lock nut from top to bottom. The second rear pad of the second lower mold and the third rear pad of the second lower mold, the second lower mold upper hard alloy is embedded in the second lower mold upper middle sleeve, the second lower mold lower hard alloy is embedded in the second lower mold lower middle sleeve, and the height of the second lower mold upper hard alloy and the second lower mold lower hard alloy is consistent with the height of the second lower mold upper middle sleeve and the second lower mold lower middle sleeve, the second lower mold upper hard alloy is provided with a second lower mold core, and one end of the second lower mold core is flush with the upper end surface of the second lower mold upper middle sleeve and the second lower mold upper hard alloy The other end of the second lower die core passes through the second lower die upper carbide, the second lower die lower carbide, the second lower die first rear pad, the second lower die second rear pad and the second lower die third rear pad from top to bottom and is located at the lower part outside the second lower die third rear pad; the second lower die lock nut is sleeved on the outer side of the lower part of the second rear pad of the second lower die, and the second lower die outer shell is sleeved on the outer side of the second lower die lock nut, the second lower die second rear pad, the second lower die first rear pad, the second lower die lower middle sleeve and the second lower die upper middle sleeve.
[0018] The third upper die and the third lower die of the third station cold heading die, the third upper die is composed of a third upper die outer rear pad, a third upper die inner rear pad, a third upper die three-needle core, a third upper die three-needle cushion block, a third upper die outer shell, a third upper die sleeve, and a third upper die punch rod. The third upper die outer rear pad, the third upper die three-needle cushion block, and the third upper die sleeve are respectively embedded in the third upper die outer shell from top to bottom. The third upper die inner rear pad is embedded in the third upper die outer rear pad, and one end of the third upper die inner rear pad is flush with the upper end of the third upper die outer rear pad. One end of the third upper die three-needle core is provided below the other end of the inner rear pad of the third upper die, the other end of the third upper die three-needle core penetrates the third upper die three-needle cushion block and abuts against the upper end of the third upper die sleeve, one end of the third upper die punch rod is embedded on the inner side of the lower part of the third upper die three-needle cushion block, the other end of the third upper die punch rod penetrates the third upper die three-needle cushion block and the third upper die sleeve respectively and is located at the lower part outside the third upper die sleeve; the third lower die is composed of a third lower die outer shell, a third lower die upper middle sleeve, a third lower die first hard alloy, and a third lower die second hard alloy. The third lower die is composed of a third lower die third hard alloy, a third lower die first rear pad, a third lower die second rear pad, a third lower die third rear pad, a third lower die core, and a third lower die lock nut. The third lower die is respectively provided with a third lower die upper middle sleeve, a third lower die lower middle sleeve, a third lower die first rear pad, a third lower die second rear pad, and a third lower die third rear pad from top to bottom. The upper part of the third lower die upper middle sleeve is embedded with the third lower die first hard alloy, the lower part of the third lower die upper middle sleeve is embedded with the third lower die second hard alloy, the third lower die lower middle sleeve is embedded with the third lower die third hard alloy, and the third lower die second hard alloy is located at the third lower die second hard alloy. One end of a third lower die core is arranged inside, and one end of the third lower die core is flush with the bottom surface of the first hard alloy of the third lower die, and the other end of the third lower die core respectively passes through the second hard alloy of the third lower die, the third hard alloy of the third lower die, the first rear pad of the third lower die, the second rear pad of the third lower die and the third rear pad of the third lower die, and is located at the lower part outside the third rear pad of the third lower die; the third lower die lock nut is sleeved on the outer side of the lower part of the second rear pad of the third lower die, and the outer side of the third lower die lock nut, the second rear pad of the third lower die, the first rear pad of the third lower die, the lower middle sleeve of the third lower die and the upper middle sleeve of the third lower die are sleeved with the third lower die outer shell.
[0019] The first hard alloy of the third lower die is provided with a flower-tooth-shaped through hole.
[0020] The fourth upper die and the fourth lower die of the fourth station cold heading die, the fourth upper die is composed of a fourth upper die outer rear pad, a fourth upper die inner rear pad, a fourth upper die inner lower rear pad, a fourth upper die core, a fourth upper die shell, a fourth upper die middle sleeve, and a fourth upper die hard alloy. The fourth upper die outer rear pad and the fourth upper die middle sleeve are respectively embedded in the fourth upper die shell from top to bottom, and the fourth upper die inner rear pad and the fourth upper die inner lower rear pad are sequentially embedded in the fourth upper die outer rear pad from top to bottom. , and the lower part of the lower rear pad in the fourth upper die is embedded in the fourth upper die middle sleeve, the bottom of the lower rear pad in the fourth upper die is against one end of the fourth upper die core, and the other end of the fourth upper die core is sleeved with a fourth upper die hard alloy, and the fourth upper die hard alloy is embedded in the bottom of the fourth upper die middle sleeve; the fourth lower die is composed of a fourth lower die shell, a fourth lower die clamp, a fourth lower die hard alloy, a fourth lower die alloy middle sleeve, a fourth lower die punch rod, a fourth lower die outer spring, a fourth lower die inner spring, and the fourth lower die outer spring. The fourth lower mold upper rear pad, the fourth lower mold lower rear pad, the fourth lower mold core, and the fourth lower mold lock nut are composed. The fourth lower mold is respectively provided with a fourth lower mold clamping die, a fourth lower mold alloy middle sleeve and a fourth lower mold lower rear pad from top to bottom. The fourth lower mold alloy middle sleeve and the fourth lower mold lower rear pad are sleeved on the outer side with a fourth lower mold outer spring, and the lower outer side of the fourth lower mold lower rear pad is sleeved with a fourth lower mold lock nut. The fourth lower mold clamping die, the fourth lower mold outer spring, the fourth lower mold lower rear pad and the fourth lower mold lock nut are sleeved on the outer side with a fourth lower mold shell; the upper part of the fourth lower mold alloy middle sleeve is sleeved with a fourth lower mold outer spring, the fourth lower mold lower rear pad and the fourth lower mold lock nut. A fourth lower die hard alloy is embedded, a fourth lower die upper rear pad is embedded in the lower part of the fourth lower die alloy middle sleeve, and a fourth lower die punch is provided between the fourth lower die upper rear pad and the inner top surface of the fourth lower die alloy middle sleeve, one end of a fourth lower die core is provided in the fourth lower die hard alloy, and the other end of the fourth lower die core respectively penetrates the fourth lower die hard alloy, the fourth lower die punch, the fourth lower die upper rear pad and the fourth lower die lower rear pad, and is located at the lower part outside the fourth lower die lower rear pad; the lower outer side of the fourth lower die upper rear pad is provided with a fourth lower die inner spring.
[0021] The lower part of the inner side of the fourth upper die hard alloy is provided with a flower tooth-shaped through hole.
[0022] The upper part and the lower part of the inner side of the fourth lower die hard alloy are respectively provided with flower tooth-shaped through holes.
[0023] Compared with the prior art, the present invention provides a force limiting rod assembly processing technology, which can complete the processing of the force limiting rod assembly by using a cold heading die and a surface treatment process, replacing the traditional complex processing technology and greatly improving the production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of the force limiting rod assembly.
[0025] Figure 2 It is a schematic diagram of the first upper mold structure.
[0026] Figure 3 It is a schematic diagram of the first lower mold structure.
[0027] Figure 4 Schematic diagram of the second upper mold structure.
[0028] Figure 5 It is a schematic diagram of the second lower mold structure.
[0029] Figure 6 Schematic diagram of the third upper die structure.
[0030] Figure 7 It is a schematic diagram of the third lower mold structure.
[0031] Figure 8 Schematic diagram of the fourth upper mold structure.
[0032] Fig. 9 It is a schematic diagram of the fourth lower mold structure. DETAILED DESCRIPTION
[0033] The present invention will be further described below with reference to the accompanying drawings.
[0034] A force limiting rod assembly processing technology, the specific process flow is as follows:
[0035] (1) The raw material is subjected to the first rough drawing process, and the diameter of the raw material is controlled to be φ = 11.5 mm;
[0036] (2) The raw material after the first rough drawing is subjected to the first spheroidizing annealing process at a temperature of 710°C and kept at this temperature for 7 hours;
[0037] (3) The raw material after the first spheroidizing annealing is subjected to a second rough drawing process, and the diameter of the raw material is controlled to be φ = 10.5 mm;
[0038] (4) subjecting the raw material after the second rough drawing to a second spheroidizing annealing process at a temperature of 710°C and keeping the temperature for 7 hours;
[0039] (5) The raw material after the second spheroidizing annealing is subjected to a fine drawing process, and the diameter of the finished wire is controlled to be φ = 10.15 mm;
[0040] (6) Cutting the finished wire after fine drawing into force-limiting rod assembly raw material segments of specified sizes;
[0041] (7) The raw material section of the force limiting rod assembly is pressed into a finished product of the force limiting rod assembly through four sets of cold forging dies;
[0042] (8) Performing surface treatment on the finished product of the force limiting rod assembly;
[0043] (9) The finished force limiter assembly after surface treatment is subjected to appearance inspection. If qualified, it is packaged and put into storage; if unqualified, it is scrapped.
[0044] The outer diameter of the tooth of the finished force limiting rod assembly is Ф15.35±0.15; the surface profile is 0.15; the tooth width is 2× (5±0.3); the total length is 45.9±0.3; the roughness is Rz15 size 2× (≥2.75); the diameter is Ф6.6±0.05; the tooth profile direction tolerance is ±1°; the torque is 69.6±5N.m (360°); the torque requirement is ≥5 turns (1800°).
[0045] The surface treatment process is an electroplating process, in which the coating thickness is ≥8μm; electroplating solution: DIPSOL NT-200, zinc (ZN): 8-14g / L, sodium hydroxide: 110-140g / L; passivation solution: Finidip 124, its concentration is 35±5ml / L; electroplating temperature: 23±5℃; time: 25±5s; sealing temperature: 25±5℃; specific gravity: 0.80-0.90; centrifugation once.
[0046] like Figures 2 to 9As shown, the cold heading die includes a first-station cold heading die, a second-station cold heading die, a third-station cold heading die, and a fourth-station cold heading die. The first-station cold heading die includes a first upper die and a first lower die. The first upper die is composed of a first upper die die shell and a first upper die hard alloy. A T-shaped through hole is provided in the first upper die die shell 1-1, and a first upper die hard alloy 1-2 is embedded at the bottom of the first upper die die shell 1-1; the first lower die is composed of a first lower die shell, a first lower die upper middle sleeve, and a first lower die upper hard alloy. The first lower die is composed of a first lower die upper middle sleeve 1-4, a first lower die lower middle sleeve 1-6, a first lower die first rear pad 1-8, a first lower die second rear pad 1-9 and a first lower die third rear pad 1-11. The first lower die upper middle sleeve 1-4 is embedded with a first lower die upper hard alloy 1-5. The first lower die lower middle sleeve 1-6 is embedded with a first lower die upper hard alloy 1-5. The first lower die lower carbide 1-7, and the height of the first lower die upper carbide 1-5 and the first lower die lower carbide 1-7 are consistent with the height of the first lower die upper middle sleeve 1-4 and the first lower die lower middle sleeve 1-6, the first lower die upper carbide 1-5 is provided with a first lower die core 1-12, and one end of the first lower die core 1-12 is flush with the upper end surface of the first lower die upper middle sleeve 1-4 and the first lower die upper carbide 1-5, and the other end of the first lower die core 1-12 passes through the first lower die upper carbide 1-5 from top to bottom. -5, the first lower die lower carbide 1-7, the first lower die first rear pad 1-8, the first lower die second rear pad 1-9 and the first lower die third rear pad 1-11 are located at the lower part outside the first lower die third rear pad 1-11; the first lower die lock nut 1-10 is sleeved on the outer side of the lower part of the first lower die second rear pad 1-9, and the first lower die lock nut 1-10, the first lower die second rear pad 1-9, the first lower die first rear pad 1-8, the first lower die lower middle sleeve 1-6 and the first lower die upper middle sleeve 1-4 are sleeved on the outer side thereof.
[0047] The second station cold heading die includes a second upper die and a second lower die. The second upper die is composed of a second upper die die shell, a second upper die die carbide, and the second upper die is composed of a second upper die die back pad and a second upper die die core. The second upper die die shell 2-2 has an inner groove, and a second upper die die back pad 2-1 is embedded in the groove. The lower end of the second upper die die back pad 2-1 abuts against one end of the second upper die die core 2-3, and the other end of the second upper die die core 2-3 is sleeved with a second upper die die carbide 2-4 on the outer side. The second upper die die carbide 2-4 is embedded in the first The bottom of the second upper die punch shell 2-2; the second lower die is composed of a second lower die shell, a second lower die upper middle sleeve, a second lower die upper carbide, a second lower die lower middle sleeve, a second lower die lower carbide, a second lower die first rear pad, a second lower die second rear pad, a second lower die third rear pad, a second lower die core, and a second lower die lock nut. The second lower die is respectively provided with a second lower die upper middle sleeve 2-6, a second lower die lower middle sleeve 2-8, a second lower die first rear pad 2-10, a second lower die second rear pad 2-11 and a second lower die third rear pad 2-13 from top to bottom. The second lower die upper middle sleeve 2-6 is embedded with There is a second lower die upper carbide 2-7, a second lower die lower middle sleeve 2-8 is embedded with a second lower die lower carbide 2-9, and the height of the second lower die upper carbide 2-7 and the second lower die lower carbide 2-9 is consistent with the height of the second lower die upper middle sleeve 2-6 and the second lower die lower middle sleeve 2-8, a second lower die core 2-14 is arranged in the second lower die upper carbide 2-7, and one end of the second lower die core 2-14 is flush with the upper end surface of the second lower die upper middle sleeve 2-6 and the second lower die upper carbide 2-7, and the other end of the second lower die core 2-14 is respectively It penetrates the second lower die upper hard alloy 2-7, the second lower die lower hard alloy 2-9, the second lower die first rear pad 2-10, the second lower die second rear pad 2-11 and the second lower die third rear pad 2-13 and is located at the lower part outside the second lower die third rear pad 2-13; the second lower die lock nut 2-12 is sleeved on the outer side of the lower part of the second lower die second rear pad 2-11, and the second lower die outer shell 2-5 is sleeved on the outer side of the second lower die lock nut 2-12, the second lower die second rear pad 2-11, the second lower die first rear pad 2-10, the second lower die lower middle sleeve 2-8 and the second lower die upper middle sleeve 2-6.
[0048] The third station cold heading die is a third upper die and a third lower die. The third upper die is composed of a third upper die outer rear pad, a third upper die inner rear pad, a third upper die three-needle core, a third upper die three-needle cushion block, a third upper die shell, a third upper die sleeve, and a third upper die punch rod. The third upper die shell 3-5 is respectively embedded with a third upper die outer rear pad 3-2, a third upper die three-needle cushion block 3-4 and a third upper die sleeve 3-7 from top to bottom. The third upper die outer rear pad 3-2 is embedded with a third upper die inner rear pad 3-1, and one end of the third upper die inner rear pad 3-1 is flush with the upper end of the third upper die outer rear pad 3-2, and the other end of the third upper die inner rear pad 3-1 is provided below the third One end of the upper die three-needle core 3-3, the other end of the third upper die three-needle core 3-3 penetrates the third upper die three-needle cushion block 3-4 and abuts against the upper end of the third upper die sleeve 3-7, one end of the third upper die punch rod 3-6 is embedded on the inner side of the lower part of the third upper die three-needle cushion block 3-4, the other end of the third upper die punch rod 3-6 penetrates the third upper die three-needle cushion block 3-4 and the third upper die sleeve 3-7 respectively and is located at the lower part outside the third upper die sleeve 3-7; the third lower die is composed of a third lower die outer shell, a third lower die upper middle sleeve, a third lower die lower middle sleeve, a third lower die first hard alloy, a third lower die second hard alloy, a third lower die third hard alloy, a third lower die first rear pad, a third lower die second rear pad, a third The third lower die is composed of a third rear pad, a third lower die core, and a third lower die lock nut. The third lower die is respectively provided with a third lower die upper middle sleeve 3-10, a third lower die lower middle sleeve 3-12, a third lower die first rear pad 3-14, a third lower die second rear pad 3-15 and a third lower die third rear pad 3-17 from top to bottom. The upper part of the third lower die upper middle sleeve 3-10 is embedded with a third lower die first hard alloy 3-8, the lower part of the third lower die upper middle sleeve 3-10 is embedded with a third lower die second hard alloy 3-11, the third lower die lower middle sleeve 3-12 is embedded with a third lower die third hard alloy 3-13, and one end of the third lower die core 3-18 is located inside the second hard alloy 3-11 of the third lower die, and the third lower die core 3- One end of 18 is flush with the bottom surface of the first cemented carbide 3-8 of the third lower die, and the other end of the third lower die core 3-18 respectively penetrates the third lower die second cemented carbide 3-11, the third lower die third cemented carbide 3-13, the third lower die first rear pad 3-14, the third lower die second rear pad 3-15 and the third lower die third rear pad 3-17, and is located at the lower part outside the third lower die third rear pad 3-17; the third lower die lock nut 3-16 is provided on the outer side of the lower part of the third lower die second rear pad 3-15, and the third lower die outer shell 3-9 is provided on the outer side of the third lower die lock nut 3-16, the third lower die second rear pad 3-15, the third lower die first rear pad 3-14, the third lower die lower middle sleeve 3-12 and the third lower die upper middle sleeve 3-10.
[0049] A flower-tooth-shaped through hole is arranged in the first hard alloy 3-8 of the third lower die.
[0050] The fourth station cold heading die is a fourth upper die and a fourth lower die. The fourth upper die is composed of a fourth upper die outer rear pad, a fourth upper die inner upper rear pad, a fourth upper die inner lower rear pad, a fourth upper die core, a fourth upper die shell, a fourth upper die middle sleeve, and a fourth upper die carbide alloy. The fourth upper die shell 4-4 is respectively embedded with a fourth upper die outer rear pad 4-1 and a fourth upper die middle sleeve 4-5 from top to bottom, the fourth upper die outer rear pad 4-1 is sequentially embedded with a fourth upper die inner upper rear pad 4-2 and a fourth upper die inner lower rear pad 4-3 from top to bottom, and the lower part of the fourth upper die inner lower rear pad 4-3 is embedded in the fourth upper die outer rear pad 4-1. The fourth upper die punch sleeve 4-5 is located in the bottom of the lower rear pad 4-3 in the fourth upper die punch, which abuts against one end of the fourth upper die punch core 4-6. The other end of the fourth upper die punch core 4-6 is sleeved on the outer side with a fourth upper die punch carbide 4-7. The fourth upper die punch carbide 4-7 is embedded in the bottom of the fourth upper die punch sleeve 4-5. The fourth lower die is composed of a fourth lower die shell, a fourth lower die clamping die, a fourth lower die carbide, a fourth lower die alloy sleeve, a fourth lower die punch rod, a fourth lower die outer spring, a fourth lower die inner spring, a fourth lower die upper rear pad, a fourth lower die lower rear pad, a fourth lower die core, and a fourth lower die lock nut. The fourth lower die is composed of a fourth lower die shell, a fourth lower die clamping die, a fourth lower die carbide, a fourth lower die alloy sleeve, a fourth lower die punch rod, a fourth lower die outer spring, a fourth lower die inner spring, a fourth lower die upper rear pad, a fourth lower die lower rear pad, a fourth lower die core, and a fourth lower die lock nut. A fourth lower die clamping die 4-9, a fourth lower die alloy middle sleeve 4-11 and a fourth lower die lower rear pad 4-16 are respectively provided, and a fourth lower die outer spring 4-13 is sleeved on the outer side of the fourth lower die alloy middle sleeve 4-11 and the fourth lower die lower rear pad 4-16, and a fourth lower die locking nut 4-17 is sleeved on the lower outer side of the fourth lower die clamping die 4-9, the fourth lower die outer spring 4-13, the fourth lower die lower rear pad 4-16 and the fourth lower die locking nut 4-17 are sleeved on the outer side of the fourth lower die housing 4-8; a fourth lower die hard alloy 4-10 is embedded in the upper part of the fourth lower die alloy middle sleeve 4-11, and the fourth lower die alloy middle sleeve 4 -11 is embedded with the fourth lower die upper rear pad 4-15 in the lower part, and the fourth lower die punch rod 4-12 is provided between the fourth lower die upper rear pad 4-15 and the inner top surface of the fourth lower die alloy middle sleeve 4-11, and one end of the fourth lower die core 4-18 is provided in the fourth lower die carbide 4-10, and the other end of the fourth lower die core 4-18 respectively penetrates the fourth lower die carbide 4-10, the fourth lower die punch rod 4-12, the fourth lower die upper rear pad 4-15 and the fourth lower die lower rear pad 4-16, and is located at the lower part outside the fourth lower die lower rear pad 4-16; the lower outer side of the fourth lower die upper rear pad 4-15 is sleeved with the fourth lower die inner spring 4-14.
[0051] A tooth-shaped through hole is provided at the lower part of the inner side of the fourth upper die hard alloy 4-7.
[0052] The upper and lower parts of the inner side of the fourth lower die carbide 4-10 are respectively provided with flower-tooth-shaped through holes.
[0053] The force limiting rod assembly can be processed by using cold heading dies and surface treatment technology, replacing the traditional complex processing technology and greatly improving production efficiency.
Claims
1. A process for processing a force-limiting rod assembly, characterized in that: The specific process is as follows: (1) The raw material is subjected to the first rough drawing process, and the diameter of the raw material is controlled to be φ=11.5 mm; (2) subjecting the raw material after the first rough drawing to the first spheroidizing annealing process, the annealing temperature is 710° C., and the temperature is kept for 7 hours; (3) The raw material after the first spheroidizing annealing is subjected to a second rough drawing process, and the diameter of the raw material is controlled to be φ=10.5 mm; (4) subjecting the raw material after the second rough drawing to a second spheroidizing annealing process at a temperature of 710° C. and keeping the temperature for 7 hours; (5) The raw material after the second spheroidizing annealing is subjected to a fine drawing process, and the diameter of the finished wire is controlled to be φ=10.15 mm; (6) Cutting the finished wire after fine drawing into force-limiting rod assembly raw material segments of specified sizes; (7) Pressing the raw material section of the force limiting rod assembly into a finished product of the force limiting rod assembly through four sets of cold heading dies; (8) performing a surface treatment process on the finished product of the force limiting rod assembly; (9) Conduct appearance inspection on the finished force-limiting rod assembly after surface treatment. If qualified, it will be packaged and put into storage; if unqualified, it will be scrapped; The four sets of cold heading dies include a first-station cold heading die, a second-station cold heading die, a third-station cold heading die, and a fourth-station cold heading die. The first-station cold heading die includes a first upper die and a first lower die. The first upper die is composed of a first upper die die shell and a first upper die die hard alloy. A T-shaped through hole is provided in the first upper die die shell (1-1). The first upper die die hard alloy (1-2) is embedded at the bottom of the first upper die die shell (1-1). The first lower die is composed of a first lower die shell, a first lower die upper middle sleeve, a first lower die upper hard alloy, a first lower die lower middle sleeve, The first lower die is composed of a first lower die lower carbide, a first lower die first rear pad, a first lower die second rear pad, a first lower die third rear pad, a first lower die core, and a first lower die lock nut. The first lower die is respectively provided with a first lower die upper middle sleeve (1-4), a first lower die lower middle sleeve (1-6), a first lower die first rear pad (1-8), a first lower die second rear pad (1-9), and a first lower die third rear pad (1-11) from top to bottom. The first lower die upper middle sleeve (1-4) is embedded with a first lower die upper carbide (1-5), and the first lower die lower middle sleeve (1-6) is embedded with a first lower die lower carbide (1-7 ), and the height of the first lower die upper hard alloy (1-5) and the first lower die lower hard alloy (1-7) is consistent with the height of the first lower die upper middle sleeve (1-4) and the first lower die lower middle sleeve (1-6), a first lower die core (1-12) is provided in the first lower die upper hard alloy (1-5), and one end of the first lower die core (1-12) is flush with the upper end surface of the first lower die upper middle sleeve (1-4) and the first lower die upper hard alloy (1-5), and the other end of the first lower die core (1-12) passes through the first lower die upper hard alloy (1-5), the first lower die upper middle sleeve (1-4), and the first lower die upper hard alloy (1-5) from top to bottom. The lower hard alloy (1-7), the first lower die first rear pad (1-8), the first lower die second rear pad (1-9) and the first lower die third rear pad (1-11) are located at the lower part outside the first lower die third rear pad (1-11); the first lower die lock nut (1-10) is sleeved on the outer side of the lower part of the first lower die second rear pad (1-9); the first lower die lock nut (1-10), the first lower die second rear pad (1-9), the first lower die first rear pad (1-8), the first lower die lower middle sleeve (1-6) and the first lower die upper middle sleeve (1-4) are sleeved on the outer side of the first lower die outer sleeve (1-3);The fourth station cold heading die comprises a fourth upper die and a fourth lower die, wherein the fourth upper die is composed of a fourth upper die outer rear pad, a fourth upper die inner upper rear pad, a fourth upper die inner lower rear pad, a fourth upper die core, a fourth upper die shell, a fourth upper die middle sleeve, and a fourth upper die hard alloy. The fourth upper die shell (4-4) is respectively embedded with a fourth upper die outer rear pad (4-1) and a fourth upper die middle sleeve (4-5) from top to bottom, the fourth upper die outer rear pad (4-1) is sequentially embedded with a fourth upper die inner upper rear pad (4-2) and a fourth upper die inner lower rear pad (4-3) from top to bottom, and the lower part of the fourth upper die inner lower rear pad (4-3) is embedded in the fourth upper die. In the middle sleeve (4-5), the bottom of the lower rear pad (4-3) in the fourth upper die punch abuts against one end of the fourth upper die punch core (4-6), and the outer side of the other end of the fourth upper die punch core (4-6) is sleeved with a fourth upper die punch carbide (4-7), and the fourth upper die punch carbide (4-7) is embedded in the bottom of the fourth upper die punch middle sleeve (4-5); the fourth lower die is composed of a fourth lower die shell, a fourth lower die clamping die, a fourth lower die carbide, a fourth lower die alloy middle sleeve, a fourth lower die punch rod, a fourth lower die outer spring, a fourth lower die inner spring, a fourth lower die upper rear pad, a fourth lower die lower rear pad, a fourth lower die core, and a fourth lower die lock nut, and the fourth lower die is respectively provided with a fourth lower die clamping die (4-9), A fourth lower die alloy middle sleeve (4-11) and a fourth lower die lower rear pad (4-16), a fourth lower die outer spring (4-13) is sleeved on the outer side of the fourth lower die alloy middle sleeve (4-11) and the fourth lower die lower rear pad (4-16), a fourth lower die lock nut (4-17) is sleeved on the lower outer side of the fourth lower die lower rear pad (4-16), and a fourth lower die outer shell (4-8) is sleeved on the outer side of the fourth lower die clamping die (4-9), the fourth lower die outer spring (4-13), the fourth lower die lower rear pad (4-16) and the fourth lower die lock nut (4-17); a fourth lower die hard alloy (4-10) is embedded in the upper part of the fourth lower die alloy middle sleeve (4-11), and a fourth lower die outer spring (4-13) is sleeved on the lower outer side of the fourth lower die lower rear pad (4-16). A fourth lower die upper rear pad (4-15) is embedded therein, and a fourth lower die punch (4-12) is arranged between the fourth lower die upper rear pad (4-15) and the inner top surface of the fourth lower die alloy middle sleeve (4-11); one end of a fourth lower die core (4-18) is arranged in the fourth lower die hard alloy (4-10); the other end of the fourth lower die core (4-18) respectively penetrates the fourth lower die hard alloy (4-10), the fourth lower die punch (4-12), the fourth lower die upper rear pad (4-15) and the fourth lower die lower rear pad (4-16), and is located at the lower part outside the fourth lower die lower rear pad (4-16); the lower outer side of the fourth lower die upper rear pad (4-15) is sleeved with a fourth lower die inner spring (4-14); The lower part of the inner side of the fourth upper die hard alloy (4-7) is provided with a flower tooth-shaped through hole; The upper and lower parts of the inner side of the fourth lower die hard alloy (4-10) are respectively provided with flower tooth-shaped through holes.
2. A force limiting rod assembly processing process according to claim 1, characterized in that: The second station cold heading die comprises a second upper die and a second lower die. The second upper die consists of a second upper die die shell, a second upper die die hard alloy, a second upper die die back pad, and a second upper die die core. The second upper die die shell (2-2) has an inner groove, in which a second upper die die back pad (2-1) is embedded. The lower end of the second upper die die back pad (2-1) abuts against one end of the second upper die die core (2-3). The other end of the second upper die die core (2-3) is sleeved with a second upper die die hard alloy (2-4). The second upper die die hard alloy (2-4) is embedded in the second upper die die shell (2-2). 2); the second lower die is composed of a second lower die shell, a second lower die upper middle sleeve, a second lower die upper hard alloy, a second lower die lower middle sleeve, a second lower die lower hard alloy, a second lower die first rear pad, a second lower die second rear pad, a second lower die third rear pad, a second lower die core, and a second lower die lock nut; the second lower die is provided with a second lower die upper middle sleeve (2-6), a second lower die lower middle sleeve (2-8), a second lower die first rear pad (2-10), a second lower die second rear pad (2-11) and a second lower die third rear pad (2-13) from top to bottom; the second lower die upper middle sleeve (2-6) is embedded with a second lower die upper hard alloy (2-7); A second lower die lower hard alloy (2-9) is embedded in the second lower die lower middle sleeve (2-8), and the heights of the second lower die upper hard alloy (2-7) and the second lower die lower hard alloy (2-9) are consistent with the heights of the second lower die upper middle sleeve (2-6) and the second lower die lower middle sleeve (2-8), a second lower die core (2-14) is disposed in the second lower die upper hard alloy (2-7), and one end of the second lower die core (2-14) is flush with the upper end surfaces of the second lower die upper middle sleeve (2-6) and the second lower die upper hard alloy (2-7), and the other end of the second lower die core (2-14) penetrates the second lower die upper hard alloy from top to bottom. The alloy (2-7), the second lower die lower hard alloy (2-9), the second lower die first rear pad (2-10), the second lower die second rear pad (2-11) and the second lower die third rear pad (2-13) are located at the lower part outside the second lower die third rear pad (2-13); the second lower die lock nut (2-12) is sleeved on the outer side of the lower part of the second lower die second rear pad (2-11), and the second lower die outer shell (2-5) is sleeved on the outer side of the second lower die lock nut (2-12), the second lower die second rear pad (2-11), the second lower die first rear pad (2-10), the second lower die lower middle sleeve (2-8) and the second lower die upper middle sleeve (2-6).
3. A process for processing a force limiting rod assembly according to claim 1, characterized in that: The third station cold heading die comprises a third upper die and a third lower die. The third upper die consists of a third upper die outer rear pad, a third upper die inner rear pad, a third upper die three-needle core, a third upper die three-needle cushion block, a third upper die shell, a third upper die sleeve, and a third upper die punch rod. The third upper die shell (3-5) is respectively embedded with a third upper die outer rear pad (3-2), a third upper die three-needle cushion block (3-4), and a third upper die sleeve (3-7) from top to bottom. The third upper die outer rear pad (3-2) is embedded with a third upper die inner rear pad (3-1), and one end of the third upper die inner rear pad (3-1) is connected to the third upper die outer rear pad (3-2). The upper ends are flush, one end of a third upper die three-needle core (3-3) is arranged below the other end of the third upper die inner rear pad (3-1), the other end of the third upper die three-needle core (3-3) penetrates the third upper die three-needle cushion block (3-4) and abuts against the upper end of the third upper die sleeve (3-7), one end of a third upper die punch rod (3-6) is embedded inside the lower part of the third upper die three-needle cushion block (3-4), the other end of the third upper die punch rod (3-6) respectively penetrates the third upper die three-needle cushion block (3-4) and the third upper die sleeve (3-7) and is located at the lower part outside the third upper die sleeve (3-7); the third lower die is composed of a third lower die outer shell, a third lower die upper middle sleeve, and a third lower die lower The third lower die is composed of a middle sleeve, a first hard alloy of the third lower die, a second hard alloy of the third lower die, a third hard alloy of the third lower die, a first rear pad of the third lower die, a second rear pad of the third lower die, a third rear pad of the third lower die, a third lower die core, and a third lower die lock nut. The third lower die is respectively provided with a third lower die upper middle sleeve (3-10), a third lower die lower middle sleeve (3-12), a third lower die first rear pad (3-14), a third lower die second rear pad (3-15) and a third lower die third rear pad (3-17) from top to bottom. The upper part of the third lower die upper middle sleeve (3-10) is embedded with the first hard alloy of the third lower die (3-8), and the lower part of the third lower die upper middle sleeve (3-10) is embedded with the second hard alloy of the third lower die (3-8). -11), a third lower die third hard alloy (3-13) is embedded in the third lower die lower middle sleeve (3-12), one end of a third lower die core (3-18) is disposed in the third lower die second hard alloy (3-11), and one end of the third lower die core (3-18) is flush with the bottom surface of the third lower die first hard alloy (3-8), and the other end of the third lower die core (3-18) respectively penetrates the third lower die second hard alloy (3-11), the third lower die third hard alloy (3-13), the third lower die first rear pad (3-14), the third lower die second rear pad (3-15) and the third lower die third rear pad (3-17), and is located at the lower part outside the third lower die third rear pad (3-17);A third lower mold lock nut (3-16) is sleeved on the outer side of the lower part of the second rear pad (3-15) of the third lower mold, and a third lower mold outer shell (3-9) is sleeved on the outer side of the third lower mold lock nut (3-16), the second rear pad (3-15) of the third lower mold, the first rear pad (3-14) of the third lower mold, the lower middle sleeve (3-12) of the third lower mold, and the upper middle sleeve (3-10) of the third lower mold. ; 4. A process for processing a force limiting rod assembly according to claim 3, characterized in that: The first hard alloy (3-8) of the third lower die is provided with a flower tooth-shaped through hole.
Citation Information
Patent Citations
Cold heading die for head groove of injection molding part
CN212443057U