A durable heating wire and its preparation process

By using a conductive core made of carbon powder, glass powder, and chrome yellow, combined with a chromium-nickel alloy heating shell, the problem of poor durability of electronic cigarette heating wires has been solved, and the resistance to dirt and the service life of the heating wires have been improved.

CN112189904BActive Publication Date: 2024-11-15SHENZHEN MISTWOOD TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011209960.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-03
Publication Date
2024-11-15
Estimated Expiration
2040-11-03

AI Technical Summary

Technical Problem

The existing heating wires for electronic cigarettes have poor durability, mainly due to their insufficient resistance to dirt and grime, which makes the surface of the heating wire easily corroded and damaged.

Method used

The conductive core is made of carbon powder, glass powder and chrome yellow as raw materials, and the heating shell is made of chromium-nickel alloy. The conductive core is filled by ultrasonic vibration and heated and shaped in an oxygen-free environment. Combined with the melting of glass powder and the carburizing effect of chrome yellow, the strength and dirt resistance of the heating shell are improved.

Benefits of technology

It significantly improves the service life and surface cleanliness of the heating wire, preventing it from being contaminated and corroded during long-term use, and maintaining a better level of cleanliness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a durable heating wire and a preparation process thereof. The heating wire comprises a conductive core and a heating shell. The heating shell is a hollow tubular structure. The conductive core is located in the hollow structure of the heating shell. The wall thickness of the heating shell is 0.2-0.4 mm. The invention overcomes the shortcomings of the prior art. By using a conductive core made of carbon powder, melamine, glass powder and chrome yellow, the service life and dirt resistance of the heating wire are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heating wires for electronic cigarettes, and in particular to a durable heating wire and a preparation process thereof. Background Art

[0002] The biggest harm of traditional cigarettes lies in the way they are used - burning. The harmful gases produced by burning tobacco leaves are actually similar to those produced by burning lettuce. In other words, apart from the factor of nicotine, the biggest harm of traditional cigarettes comes from the backward way of use. When a single cigarette is burned, more than 6,000 compounds will be produced, many of which are confirmed carcinogens. At present, the world has clearly known the harm of traditional cigarettes and the harm of secondhand smoke unique to traditional cigarettes. The ideal solution is that traditional cigarettes disappear from the world. However, such a utopian fantasy is impossible to achieve. The birth of electronic cigarettes appeared in this context. The main principle is to remove the harmful substances produced by the combustion of traditional cigarettes on the basis of ensuring the safe intake of nicotine. Make the way to obtain nicotine safer.

[0003] The working principle of electronic cigarettes is to convert electrical energy into heat energy, and use the heat-like energy to vaporize the oil. Then inhale the vaporized oil mist. Thus, the purpose of nicotine intake is achieved. It is similar to a humidifier, except that the humidifier vaporizes water. Electronic cigarettes vaporize the oil. The biggest advantage of vaporization is that it is a physical change and no new substances will be produced. Therefore, electronic cigarettes are less harmful than traditional cigarettes. The existing electronic cigarette heating wire has a short service life. The main reason is that it has poor dirt resistance, which makes the surface of the heating wire easily corroded and damaged. Summary of the invention

[0004] The purpose of the present invention is to provide a durable heating wire and a preparation process thereof, which overcomes the problem of poor durability of the heating wire used in electronic cigarettes in the prior art.

[0005] To solve the above problems, the technical solutions adopted by the present invention are as follows:

[0006] A durable heating wire comprises a conductive core and a heating shell, wherein the heating shell is a hollow tubular structure, the conductive core is located in the hollow structure of the heating shell, and the wall thickness of the heating shell is 0.2-0.4 mm.

[0007] Preferably, the heating shell is made of chromium-nickel alloy material.

[0008] Preferably, the conductive core is made of raw materials including carbon powder, glass powder, melamine and chrome yellow.

[0009] Preferably, the preparation method of the conductive core is to mix carbon powder, glass powder and chrome yellow evenly, then add them into melamine solution, stir and mix evenly, and then dry and crush to obtain a powdered conductive core.

[0010] The process for preparing a durable heating wire comprises the following steps:

[0011] S1, immersing the heating shell in an ethanol solution, cleaning it, and then taking it out and drying it to obtain a clean heating shell;

[0012] S2, sealing one end of the clean heating shell, and then filling the heating shell with a conductive core, with ultrasonic vibration during the filling process;

[0013] S3, after filling the conductive core, bend the heating shell into the desired shape, then place the heating shell in an oxygen-free environment at 700-900°C for heating, and then cool it to room temperature to set the shape;

[0014] S4, closing the other end of the shaped heating shell to obtain a heating wire blank, and then connecting the two ends of the heating wire blank to a power source to raise the temperature of the heating wire to 500-700° C., and then cooling it to room temperature to obtain a heating wire.

[0015] Compared with the prior art, the implementation effects of the present invention are as follows:

[0016] 1. The present invention uses carbon powder as a matrix and fully mixes it with glass powder, melamine and chrome yellow, so that the conductive core generates conductivity under the conduction effect of carbon. The heating shell of the heating wire can heat the carbon inside during the electrothermal process. Under the action of current and heat, the carbon atoms in the carbon powder penetrate into the heating shell to improve the strength of the heating shell. At the same time, due to the thin thickness of the heating shell, the carbon atoms on the surface of the outer surface of the heating shell that contacts the air are oxidized by the air to form carbon dioxide, so that carbon dioxide gas is continuously generated on the outer surface of the heating shell. At the same time, the carbon atoms inside the heating shell penetrate outward and continuously replenish the carbon on the outer surface of the heating shell, so that the heating wire is not easily contaminated when used in electronic cigarettes, and can still maintain a good cleanliness after long-term use.

[0017] 2. The present invention uses glass powder as the filler of the conductive core. During the heating process of the conductive core, the glass powder can melt and play a bonding role with the carbon powder and chrome yellow, so that the conductive core inside the heating wire blank after heat treatment can be hardened and the heating wire can be shaped. At the same time, the added glass powder also plays an insulating role to prevent the excellent conductivity of the carbon powder from causing the heating shell of the heating wire to not generate sufficient heat. At the same time, during the actual use of the heating wire, the glass powder re-melts and softens, releasing the carbon powder bonded to it, which can effectively replenish carbon on the heating shell.

[0018] 3. The present invention uses chrome yellow and melamine as additives for the conductive core. Chrome yellow can slow down carburization, thereby preventing the heating shell from becoming brittle and easy to break due to excessive carburization. Meanwhile, melamine decomposes to produce nitrogen-containing substances during the preparation of the heating wire, so that the conductive core of the heating wire finally manufactured contains nitrogen, so that the heating wire can be properly nitrided during use, thereby improving the structural strength of the heating shell and avoiding the problem of the heating wire strength decreasing rapidly at high temperature, thereby shortening its service life. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example 1

[0021] The carbon powder is crushed to less than 200 mesh, and then mixed with glass powder with a particle size less than 200 mesh and chrome yellow in a mass ratio of 8:3:2. Then, 2 kg of the mixed carbon powder, glass powder and chrome yellow are added to 3 kg of a methanol solution containing 2 wt% of melamine, heated to 50°C, stirred and mixed until the methanol is evaporated, and then the mixture is crushed and passed through a 200-mesh sieve to obtain a powdered conductive core.

[0022] The tubular heating shell with a hollow structure is immersed in an ethanol solution for cleaning, the wall thickness of the heating shell is 0.2 mm, and then taken out and dried to obtain a clean heating shell, and then one end of the clean heating shell is sealed, and then a powdered conductive core is filled into the heating shell, and ultrasonic vibration is used during the filling process to make the conductive core in the heating shell tightly filled; after filling the conductive core, the heating shell is bent into a desired shape, and then the heating shell is placed in an oxygen-free environment at 800°C for heating, and then cooled to room temperature and shaped, and the other end of the shaped heating shell is sealed to obtain a heating wire blank; finally, both ends of the heating wire blank are connected to a power supply to raise the temperature of the heating wire to 600°C, and after cooling to room temperature, a heating wire is obtained.

[0023] Example 2

[0024] The carbon powder is crushed to less than 200 mesh, and then mixed with glass powder with a particle size less than 200 mesh and chrome yellow in a mass ratio of 8:4:1. Then, 2.6 kg of the mixed carbon powder, glass powder and chrome yellow are added to 3 kg of a methanol solution containing 2 wt% of melamine, heated to 60°C, stirred and mixed until the methanol is evaporated, and then the mixture is crushed and passed through a 200-mesh sieve to obtain a powdered conductive core.

[0025] The tubular heating shell with a hollow structure is immersed in an ethanol solution for cleaning, the wall thickness of the heating shell is 0.25 mm, and then taken out and dried to obtain a clean heating shell, and then one end of the clean heating shell is sealed, and then a powdered conductive core is filled into the heating shell, and ultrasonic vibration is used during the filling process to make the conductive core in the heating shell tightly filled; after filling the conductive core, the heating shell is bent into a desired shape, and then the heating shell is placed in an oxygen-free environment at 850°C for heating, and then cooled to room temperature and shaped, and the other end of the shaped heating shell is sealed to obtain a heating wire blank; finally, both ends of the heating wire blank are connected to a power supply to raise the temperature of the heating wire to 700°C, and after cooling to room temperature, a heating wire is obtained.

[0026] Comparative Example 1

[0027] The difference from Example 1 is that the amount of glass powder added is 0.

[0028] Comparative Example 2

[0029] The difference from Example 1 is that the amount of melamine added is 0.

[0030] Comparative Example 3

[0031] The difference from Example 1 is that the added amount of chrome yellow is 0.

[0032] The heating wires in Examples 1-2 and Comparative Examples 1-3 were tested for rapid life value and elongation at 1200°C according to the test method in GB / T1234-1995, and the surface cleanliness of the electronic cigarette was tested at 600°C after continuous smoking of the e-liquid for 2 hours. The results are shown in the following table:

[0033] Fast life value / h Elongation after break / % Surface cleanliness Example 1 116 24 No dirt on the surface Example 2 123 26 No dirt on the surface Comparative Example 1 112 33 No dirt on the surface Comparative Example 2 96 30 There is a small amount of dirt on the surface Comparative Example 3 101 18 No dirt on the surface

[0034] It can be seen from the above table that the present invention uses a conductive core made of carbon powder, melamine, glass powder and chrome yellow, which greatly improves the service life and dirt resistance of the heating wire.

[0035] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A durable heating wire, characterized in that: It comprises a conductive core and a heating shell, wherein the heating shell is a hollow tubular structure, the conductive core is located in the hollow structure of the heating shell, and the wall thickness of the heating shell is 0.2-0.4mm; the heating shell is made of chromium-nickel alloy; The conductive core is prepared from raw materials including carbon powder, glass powder, melamine and chrome yellow. The preparation method of the conductive core is to mix the carbon powder, glass powder and chrome yellow evenly, then add them into the melamine solution, stir and mix evenly, and then dry and crush to obtain a powdered conductive core. The process of the durable heating wire comprises the following steps: S1, immersing the heating shell in an ethanol solution, cleaning it, and then taking it out and drying it to obtain a clean heating shell; S2, sealing one end of the clean heating shell, and then filling the heating shell with a conductive core, and performing ultrasonic vibration during the filling process; S3, after filling the conductive core, bending the heating shell into a desired shape, and then placing the heating shell in an oxygen-free environment at 700-900°C for heating, and then cooling it to room temperature for shaping; S4, sealing the other end of the shaped heating shell to obtain a heating wire blank, and then connecting both ends of the heating wire blank to a power source to raise the temperature of the heating wire to 500-700°C, and then cooling it to room temperature to obtain the heating wire.