Semiconductor device and method for forming the same

By forming a sloped first gate oxide layer and a second gate oxide layer with a thickness smaller than the first gate oxide layer in the semiconductor device, combined with the formation of a stepped gate oxide layer with different thicknesses, the problem of the contradiction between the on-resistance and breakdown voltage of the LDMOS device is solved. , realizing high-performance semiconductor device design.

CN112242355BActive Publication Date: 2024-10-22SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201910645338.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-17
Publication Date
2024-10-22
Estimated Expiration
2039-07-17

AI Technical Summary

Technical Problem

When the on-resistance of LDMOS devices is increased, the breakdown voltage may decrease, and vice versa. It is difficult to obtain the lowest possible on-resistance to reduce conduction losses under certain breakdown voltage conditions.

Method used

By forming a sloped first gate oxide layer and a second gate oxide layer with a thickness smaller than the first gate oxide layer on the semiconductor substrate, combined to form a stepped gate oxide layer with different thicknesses, the on-resistance is reduced and the breakdown voltage is increased. .

Benefits of technology

It achieves high breakdown voltage while maintaining low on-resistance, improves the performance of semiconductor devices, and avoids the problems of slow response speed and poor voltage resistance caused by excessive thickness of the gate oxide layer in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112242355B_ABST
    Figure CN112242355B_ABST
Patent Text Reader

Abstract

A semiconductor device and a method for forming the same, wherein the method comprises: providing a substrate; forming an oxide layer on the substrate; etching the oxide layer to form a first gate oxide layer, wherein the sidewall of the first gate oxide layer is inclined; forming a second gate oxide layer between adjacent first gate oxide layers, wherein the thickness of the second gate oxide layer is less than that of the first gate oxide layer; forming a polysilicon layer on the first gate oxide layer and the second gate oxide layer; etching the first gate oxide layer, the polysilicon layer and the second gate oxide layer until the substrate is exposed to form a gate structure. The present invention forms the first gate oxide layer with an inclined sidewall and the second gate oxide layer with a thickness less than that of the first gate oxide layer, wherein the thickness is thicker at a high voltage of the semiconductor device and thinner at a low voltage, and can maintain a smaller on-resistance while increasing the breakdown voltage of the semiconductor device, thereby improving the performance of the semiconductor device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor device and a method for forming the same. Background Art

[0002] With the development of semiconductor technology, power integrated circuits (PIC) are continuously used in many fields. Laterally double-diffused metal oxide semiconductor transistors (LDMOS) have the characteristics of high operating voltage, simple process, and easy process compatibility with complementary metal oxide semiconductors (CMOS). Therefore, they are widely used in power integrated circuits as power devices.

[0003] The source-drain breakdown voltage (BVdss) and on-resistance (Ron) characteristics of power devices are crucial for efficient power circuit design. Generally speaking, LDMOS devices require higher source-drain breakdown voltage and lower on-resistance in use to improve device performance. However, the on-resistance and breakdown voltage of LDMOS devices are contradictory indicators. If the on-resistance decreases, the breakdown voltage may decrease, and vice versa.

[0004] Therefore, how to obtain the lowest possible on-resistance to reduce conduction loss through reasonable design while meeting a certain breakdown voltage is an urgent problem to be solved. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a semiconductor device and a method for forming the same, so that the semiconductor device has a higher breakdown voltage while maintaining a lower on-resistance.

[0006] To solve the above technical problems, an embodiment of the present invention provides a method for forming a semiconductor device, comprising: providing a substrate; forming an oxide layer on the substrate; etching the oxide layer to form a first gate oxide layer, wherein the side wall of the first gate oxide layer is inclined; forming a second gate oxide layer between adjacent first gate oxide layers, wherein the thickness of the second gate oxide layer is less than that of the first gate oxide layer; forming a polysilicon layer on the first gate oxide layer and the second gate oxide layer; etching the first gate oxide layer, the polysilicon layer and the second gate oxide layer until the substrate is exposed to form a gate structure.

[0007] Optionally, the step of etching the oxide layer includes: etching the oxide layer using a dry etching process to form an inclined side wall, with a certain thickness of the oxide layer remaining on the substrate on both sides of the side wall; and removing the remaining certain thickness of the oxide layer using a wet etching process to form a first gate oxide layer.

[0008] Optionally, the etching gas for the dry etching is a mixed gas of C4F8, CF4 and CHF3, and the volume ratio of the mixed gas is 2:1:3.

[0009] Optionally, an angle between the sidewall of the first gate oxide layer and the substrate is 30° to 60°.

[0010] Optionally, the oxide layer is formed by chemical vapor deposition.

[0011] Optionally, the step of etching the first gate oxide layer includes: using a dry etching process to make the side wall on one side of the first gate oxide layer vertical, retaining the inclined side wall on the other side, and leaving a certain thickness of the first gate oxide layer on the substrate on the side of the vertical side wall; using a wet etching process to remove the remaining certain thickness of the first gate oxide layer.

[0012] Optionally, the etching gas for the dry etching is a mixed gas of CF4 and CHF3.

[0013] Optionally, the wet etching solution is hydrofluoric acid.

[0014] Optionally, the step of etching the polysilicon layer and the second gate oxide layer includes: etching the polysilicon layer using a dry etching process until the second gate oxide layer is exposed; and etching the second gate oxide layer using a dry etching process until the substrate is exposed.

[0015] Optionally, the etching gas for dry etching the polysilicon layer is hydrogen bromide and chlorine.

[0016] Optionally, the etching gas for dry etching the second gate oxide layer is hydrogen bromide and helium.

[0017] Optionally, after forming the gate structure, a source region and a drain region are formed in the substrate on both sides of the gate structure, the source region is close to the inclined sidewall of the first gate oxide layer, and the drain region is close to the vertical sidewall of the first gate oxide layer.

[0018] A semiconductor device formed by the above method comprises: a substrate; a gate structure located on the substrate, the gate structure comprising a first gate oxide layer, a second gate oxide layer and a polysilicon layer, wherein: the first gate oxide layer is located on the substrate, and the side wall on one side of the first gate oxide layer is inclined, and the side wall on the other side is vertical; the second gate oxide layer is located on the substrate on the side of the inclined side wall of the first gate oxide layer, and the thickness of the second gate oxide layer is less than that of the first gate oxide layer; the polysilicon layer is located on the surfaces of the first gate oxide layer and the second gate oxide layer.

[0019] Optionally, the semiconductor device further includes: a source region and a drain region, wherein the source region and the drain region are located in the substrate on both sides of the gate structure, the source region is close to an inclined side wall of the first gate oxide layer, and the drain region is close to a vertical side wall of the first gate oxide layer.

[0020] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:

[0021] The side wall of the first gate oxide layer is inclined, and the thickness of the first gate oxide layer gradually decreases from the middle to the inclined part, and the thickness of the formed second gate oxide layer is smaller than that of the first gate oxide layer. The first gate oxide layer and the second gate oxide layer are combined to form a stepped gate oxide layer with different thicknesses. If the first gate oxide layer is fully adopted, the withstand voltage requirement can be met. However, when the semiconductor device forms an inversion layer during subsequent operation, the capacitance of the overly thick gate oxide layer is small, which will make it relatively difficult to turn on the device and the response speed is slow. If the second gate oxide layer is fully adopted, the withstand voltage requirement cannot be met due to the insufficient thickness of the gate oxide layer. The combination of the first gate oxide layer and the second gate oxide layer can both increase the breakdown voltage and reduce the on-resistance.

[0022] Furthermore, the source region and the drain region are formed, and the source region has an inclined sidewall near the first gate oxide layer, and the drain region has a vertical sidewall near the first gate oxide layer. When the semiconductor device is in subsequent operation, the electric field strength is the largest near the drain region, and gradually decreases from the drain region to the source region. Therefore, when the semiconductor device is in subsequent operation, the thickness of the gate oxide layer does not need to be too thick near the source region, and the thickness is reduced by making the sidewall of the first gate oxide layer inclined and the second gate oxide layer. When the semiconductor device is in subsequent operation, when an inversion layer is formed on the surface of the substrate at the inclined part of the first gate oxide layer and below the second gate oxide layer, the device is easier to turn on due to the reduced thickness of the gate oxide layer, thereby improving the response speed. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figures 1 to 8 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor device of the present invention. DETAILED DESCRIPTION

[0024] As can be seen from the background technology, LDMOS devices require higher source-drain breakdown voltage and lower on-resistance in use to improve device performance. However, the on-resistance and breakdown voltage of LDMOS devices are contradictory indicators. If the on-resistance decreases, the breakdown voltage may decrease, and vice versa.

[0025] The traditional method to increase the breakdown voltage of LDMOS is to form a field oxide layer. The field oxide layer is usually formed by local oxidation of silicon, using nitride as a mask layer, and thermally oxidizing silicon to form an oxide layer. Since the oxide layer is thicker than the consumed silicon, the oxidation growth under the nitride mask will raise the edge of the nitride, resulting in a "bird's beak effect" and forming a leakage channel, which is not conducive to the voltage resistance of semiconductor devices. In addition, if the breakdown voltage is increased by increasing the thickness of the gate oxide layer, the on-resistance of the device will increase and the response speed will slow down.

[0026] In order to solve the above technical problems, the inventors have provided a method for forming a semiconductor device after research, wherein an oxide layer is first formed on a semiconductor substrate, and then the oxide layer is etched to form a first gate oxide layer, wherein the sidewall of the first gate oxide layer is inclined, and a second gate oxide layer is formed between adjacent first gate oxide layers, and the thickness of the second gate oxide layer is less than that of the first gate oxide layer. Due to the inclination of the sidewall, the thickness of the first gate oxide layer gradually decreases from the middle to the sidewall, and is combined with the second gate oxide layer to form a stepped gate oxide layer. On the one hand, the oxide layer is not grown by consuming silicon, but is directly formed on the substrate to avoid the "bird's beak effect"; on the other hand, during the subsequent operation of the semiconductor device, the voltage value gradually decreases from the inclined corner of the first gate oxide layer to the inclined sidewall direction, so the thickness of the first gate oxide layer from the middle to the inclined corner is relatively thick and is not easily broken down, which can improve the breakdown voltage of the semiconductor device, and the gate oxide layer does not need to be too thick in places where the voltage value is small, so the thickness of the gate oxide layer is reduced from the middle of the first gate oxide layer to the sidewall and the second gate oxide layer, so that the device can maintain a low on-resistance.

[0027] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0028] Figures 1 to 8 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor device of the present invention.

[0029] refer to Figure 1 , providing a substrate 10.

[0030] In this embodiment, the substrate 10 is a silicon substrate; in other embodiments, the substrate 10 can also be at least one of the following materials: germanium (Ge), silicon germanium (GeSi), silicon carbide (SiC), silicon on insulator (SOI), stacked silicon on insulator (SSOI), silicon germanium on insulator (SiGeOI) and germanium on insulator (GeOI), etc.

[0031] It should be noted that the step of providing the substrate 10 further includes: forming a shallow trench isolation structure 11 in the substrate 10 .

[0032] Continue to refer Figure 1 , an oxide layer 20 is formed on the substrate 10. The material of the oxide layer 20 is silicon oxide.

[0033] In this embodiment, the method for forming the oxide layer 20 is chemical vapor deposition. The process parameters of the chemical vapor deposition method include: using tetraethyl orthosilicate gas as the reaction gas, the reaction pressure is 0.3-0.5 Torr, and the temperature is 600-700°C.

[0034] The oxide layer 20 is directly formed on the surface of the substrate 10 by chemical vapor deposition, rather than by a method that consumes the substrate, so that the "bird's beak effect" can be avoided, which is beneficial to the voltage resistance of the semiconductor device.

[0035] After the oxide layer 20 is formed, a high temperature heat treatment is performed to densify the oxide layer 20. Densification is beneficial to improving the quality of the oxide layer 20 and facilitating subsequent processes.

[0036] refer to Figure 2 , the oxide layer 20 is etched to form an inclined side wall 201 of the oxide layer 20.

[0037] In this embodiment, the process of etching the oxide layer 20 to form the inclined sidewall 201 is anisotropic dry etching. The process parameters of the dry etching include: the etching gas is a mixed gas of C4F8, CF4 and CHF3, wherein the volume ratio of the mixed gas is 2:1:3, and the etching pressure is 0.05-0.15 Torr.

[0038] The etching gas uses a gas with a high fluorine-carbon ratio such as C4F8 and CF4. During the etching process, by-products will be formed on the side wall 201. The by-products cover the side wall 201 and can play a protective role, resulting in a slower etching rate closer to the surface of the substrate 10, thereby making the side wall 201 inclined.

[0039] Continue to refer Figure 2After the inclined side wall 201 is formed, the dry etching is stopped, and a certain thickness of the oxide layer 20 is retained on the substrate on both sides of the side wall 201.

[0040] The reason for doing so is that the dry etching rate is relatively fast. If the oxide layer 20 of a certain thickness is not retained first and is directly removed by dry etching, it is easy to cause damage to the surface of the substrate 10, which is not conducive to the performance of the semiconductor device.

[0041] refer to Figure 3 The oxide layer 20 on the substrate 10 at both sides of the sidewall 201 is removed by a wet etching process to form a first gate oxide layer 30 , wherein the sidewalls of the first gate oxide layer 30 are inclined.

[0042] Specifically, the first gate oxide layer 30 is in a regular trapezoidal shape. For the convenience of subsequent description, the first gate oxide layer 30 is divided into a rectangular region 301 and inclined regions 302 and 303 . The two corners of the rectangular region 301 and the inclined regions 302 and 303 are respectively at A and A′.

[0043] The angle between the sidewall 201 of the first gate oxide layer 30 and the surface of the substrate 10 is 30° to 60°. If the angle is less than 30°, the thickness of the first gate oxide layer 30 changes slowly, resulting in a large turn-on voltage and slow response speed of the semiconductor device; if the angle is greater than 60°, the thickness of the first gate oxide layer 30 decreases suddenly, which easily causes the first gate oxide layer 30 to be broken down.

[0044] In this embodiment, two first gate oxide layers 30 are formed simultaneously, and two gate structures are directly formed on the basis of the two first gate oxide layers 30 in the subsequent process, and a common source region is formed between the two gate structures. On the one hand, the process steps can be reduced, and on the other hand, the common source region can reduce the area required for the device.

[0045] In other embodiments, only one first gate oxide layer 30 or more than two first gate oxide layers 30 may be formed.

[0046] It should be noted that the two first gate oxide layers 30 are formed on the substrate 10 between the shallow trench isolation structures 11. The inclined region 303 of the first gate oxide layer 30 is close to the shallow trench isolation structure 11, and the inclined region 302 of the first gate oxide layer 30 is far from the shallow trench isolation structure 11.

[0047] In this embodiment, the process parameters of the wet etching include: the etching solution is hydrofluoric acid, and the concentration of the hydrofluoric acid is 1:100.

[0048] It should be noted that, before the step of dry etching the oxide layer 20, a photoresist layer (not shown) needs to be formed on the oxide layer 20, the photoresist layer is etched to form a photoresist pattern, and the oxide layer 20 is etched using the photoresist pattern as a mask. After the oxide layer 20 is wet-etched to form the first gate oxide layer 30, the photoresist pattern is removed.

[0049] refer to Figure 4 After forming the first gate oxide layer 30, a drift region 12 is formed in the substrate 10. During the subsequent operation of the semiconductor device, the drift region 12 is used for voltage reduction.

[0050] In this embodiment, one side of the drift region 12 is connected to the shallow trench isolation structure 11 , and the other side does not exceed the corner A of the first gate oxide layer 30 .

[0051] In this embodiment, the formed LDMOS is an N-type LDMOS, the substrate 10 is a P-type substrate, and the drift region 12 is doped with N-type impurity ions, and the N-type impurity ions are one or more of phosphorus ions, arsenic ions, and antimony ions; in other embodiments, when the formed LDMOS is a P-type LDMOS, the substrate 10 is an N-type substrate, and the drift region 12 is doped with P-type impurity ions, and the P-type impurity ions are one or more of boron ions, indium ions, and gallium ions.

[0052] Continue to refer Figure 4 , a second gate oxide layer 40 is formed between adjacent first gate oxide layers 30 , and a thickness of the second gate oxide layer 40 is smaller than that of the first gate oxide layer 30 .

[0053] The ratio of the thickness of the first gate oxide layer 30 to the thickness of the second gate oxide layer 40 is in a range of 4:1 to 5:1.

[0054] During the subsequent operation of the semiconductor device, the voltage value gradually decreases from the corner A of the first gate oxide layer 30 to the second gate oxide layer 40. Therefore, the thickness of the second gate oxide layer 40 does not need to be too thick and is smaller than the thickness of the first gate oxide layer 30, thereby reducing the on-resistance of the semiconductor device.

[0055] In this embodiment, the second gate oxide layer 40 is formed by furnace thermal oxidation. The material of the second gate oxide layer 40 is silicon oxide.

[0056] refer to Figure 5 , a polysilicon layer 50 is formed on the first gate oxide layer 30 and the second gate oxide layer 40 .

[0057] In this embodiment, the polysilicon layer 50 is formed by chemical vapor deposition.

[0058] In this embodiment, the polysilicon layer 50 covers all or part of the rectangular region 301 and the inclined region 302 of the first gate oxide layer 30 , and the second gate oxide layer 40 .

[0059] It should be noted that the method for forming the polysilicon layer 50 also includes: forming a mask layer (not shown) on the polysilicon layer 50, etching the polysilicon layer 50 using the mask layer as a mask, and removing the polysilicon layer 50 above the inclined region 303 or above the inclined region 303 and above part of the rectangular region 301.

[0060] The reason for doing so is that the polysilicon layer 50 is used to form a gate structure later, and removing the polysilicon layer 50 above the inclined region 303 reserves space for subsequently forming a drain region between the gate structure and the shallow trench isolation structure.

[0061] In this embodiment, the process of etching the polysilicon layer 50 is dry etching.

[0062] refer to Figure 6 , etching the first gate oxide layer 30 to remove the inclined region 303 of the first gate oxide layer 30 close to the shallow trench isolation structure 11.

[0063] The reason for doing so is to reserve space for the subsequent formation of the drain region, which is between the shallow trench isolation structure 11 and the gate structure formed later. Therefore, when electrons are transmitted from the drain region to the subsequently formed source region, they do not need to bypass the shallow trench isolation structure, and the electron migration path is short, which reduces the on-resistance of the semiconductor and improves the response speed.

[0064] In this embodiment, the step of etching the first gate oxide layer 30 includes: removing the inclined region 303 by dry etching to form a vertical sidewall, and stopping dry etching when a small amount of the first gate oxide layer 30 remains on the substrate 10 in the inclined region 303 .

[0065] Stopping the dry etching when a small amount of the first gate oxide layer 30 remains on the substrate 10 can prevent the substrate 10 from being damaged by too high a dry etching rate, which is beneficial to subsequent processes.

[0066] In this embodiment, the process parameters of the dry etching include: the etching gas is a mixed gas of CF4 and CHF3, wherein the ratio of the mixed gas is 1:1-1:2, and the etching pressure is 0.05-0.15 Torr.

[0067] After dry etching, a wet etching process is used to remove the remaining small amount of the first gate oxide layer 30 to form a first gate oxide layer 30'. The sidewall of the first gate oxide layer 30' away from the shallow trench isolation structure 11 is inclined, and the sidewall close to the shallow trench isolation structure 11 is vertical, and the vertical sidewall is aligned with the sidewall of the polysilicon layer 50 in the vertical direction.

[0068] In this embodiment, the process parameters of the wet etching include: the etching solution is hydrofluoric acid, and the concentration of the hydrofluoric acid is 1:100.

[0069] refer to Figure 7 , the polysilicon layer 50 is etched until the second gate oxide layer 40 is exposed. Specifically, the polysilicon layer 50 between adjacent first gate oxide layers 30' is etched.

[0070] In this embodiment, the method for etching the polysilicon layer 50 is dry etching, and the etching gas used for the dry etching is hydrogen bromide and chlorine.

[0071] refer to Figure 8 , the second gate oxide layer 40 is etched until the substrate 10 is exposed to form a gate structure 60 .

[0072] In this embodiment, the method for etching the second gate oxide layer 40 is dry etching, and the etching gas used for the dry etching is hydrogen bromide and helium.

[0073] When etching the second gate oxide layer 40 , the etching gas is replaced with hydrogen bromide and helium, which can reduce the etching rate and avoid damaging the substrate 10 due to too high an etching speed.

[0074] Continue to refer Figure 8 After forming the gate structure 60, a source region 101 and a drain region 102 are formed in the substrate 10 on both sides of the gate structure 60. The source region 101 is located between two adjacent gate structures 60, close to the inclined sidewall of the first gate oxide layer 30'. Two adjacent gate structures 60 share one source region 101, which can reduce the area and is conducive to the integration of semiconductor devices. The drain region 102 is located in the drift region 12, and the drain region 102 is located between the shallow trench isolation structure 11 and the gate structure 60, close to the vertical sidewall of the first gate oxide layer 30'.

[0075] After the source region 101 and the drain region 102 are formed, electrodes are drawn out on the source region 101 and the drain region 102 to form a source electrode and a drain electrode.

[0076] When a forward voltage is applied between the gate and the source of the semiconductor device formed by the method of the embodiment of the present invention, an inversion layer (not shown) will be formed on the surface of the substrate 10 near the gate structure 60. Specifically, the inversion layer is on the surface of the substrate 10 from the inclined region 302 to below the second gate oxide layer 40. Therefore, in the inclined region 302, the thickness of the first gate oxide layer 30' is gradually reduced, which can make the semiconductor device easy to turn on and improve the response speed. In addition, during the operation of the semiconductor device, the electric field strength gradually decreases from near the drain region 102 to the source region 101, and the voltage is reduced through the drift region. Therefore, near the drain region 102, where the surface electric field is the largest, the gate oxide layer is most likely to break down, and a thicker gate oxide layer needs to be provided. However, relatively speaking, the thicker the gate oxide layer, the greater the on-resistance. A too thick gate oxide layer is not required near the source region 101. In order to maintain a low on-resistance, the thickness of the gate oxide layer can be gradually reduced. Therefore, the method of the embodiment of the present invention forms the first gate oxide layer 30' with an inclined sidewall, and the thickness gradually decreases from the corner A to the inclined sidewall. The thickness of the formed second gate oxide layer 40 is much smaller than the first gate oxide layer 30, and no additional shallow trench isolation structure is required between the source and drain, which can make the semiconductor device have a higher voltage resistance and maintain a smaller on-resistance.

[0077] In addition, there is no shallow trench isolation structure 11 between the source region 101 and the drain region 102, so electrons can be directly transmitted from the drain to the source with a short transmission path, which can further reduce the on-resistance and improve the response speed of the semiconductor device.

[0078] The present invention also provides a semiconductor device formed by the method.

[0079] refer to Figure 8 The semiconductor device comprises: a substrate 10; a gate structure 60, which is located on the substrate 10, and the gate structure 60 comprises a first gate oxide layer 30', a second gate oxide layer 40 and a polysilicon layer 50, wherein: the first gate oxide layer 30' is located on the substrate 10, and the side wall of one side of the first gate oxide layer 30' is inclined, and the side wall of the other side is vertical; the second gate oxide layer 40 is located on the substrate 10 on the side of the inclined side wall of the first gate oxide layer 30', and the thickness of the second gate oxide layer 40 is less than the first gate oxide layer 30'; the polysilicon layer 50 is located on the surfaces of the first gate oxide layer 30' and the second gate oxide layer 40.

[0080] The ratio of the thickness of the first gate oxide layer 30 ′ to the thickness of the second gate oxide layer 40 is in a range of 4:1 to 5:1.

[0081] In this embodiment, the substrate 10 further has a shallow trench isolation structure 11 and a drift region 12 , and the drift region 12 is located on one side of the shallow trench isolation structure 11 .

[0082] In this embodiment, the semiconductor device further includes: a source region 101 and a drain region 102 , and the source region 101 and the drain region 102 are located in the substrate 10 on both sides of the gate structure 60 .

[0083] In this embodiment, the source region 101 is located between adjacent gate structures 60, close to the inclined sidewall of the first gate oxide layer 30', and the adjacent gate structures 60 share a source electrode, which can improve the integration of the semiconductor device; the drain region 102 is located in the drift region 12, close to the vertical sidewall of the first gate oxide layer 30'.

[0084] When the semiconductor device is working in the subsequent operation, the surface electric field is the largest near the drain region 102, and gradually decreases from the drain region 102 to the source region 101, and the voltage is reduced through the drift region 12. The thickness of the second gate oxide layer 40 is much smaller than that of the first gate oxide layer 30'. On the one hand, no additional isolation structure is required between the drain region 102 and the source region 101, and electrons can flow directly from the drain region 102 to the source region 101 without bypassing the isolation structure, thereby reducing the electron transmission path, thereby reducing the on-resistance and improving the response speed of the semiconductor device; on the other hand, the thickness of the first gate oxide layer 30' is larger at a higher voltage, and the first gate oxide layer 30' is inclined at a lower voltage, and the second gate oxide layer 40 is arranged, and the thickness gradually decreases, which can improve both the breakdown voltage of the semiconductor device and the response speed of the semiconductor device.

[0085] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for forming a semiconductor device, characterized in that: include: Providing a substrate, wherein a shallow trench isolation structure is formed in the substrate; forming an oxide layer on the substrate; Etching the oxide layer to form a first gate oxide layer, wherein the first gate oxide layer is located on the substrate between the shallow trench isolation structures, the sidewall of the first gate oxide layer is inclined, and the first gate oxide layer includes a rectangular region and inclined regions located on both sides of the rectangular region; forming a second gate oxide layer between adjacent first gate oxide layers, wherein the thickness of the second gate oxide layer is smaller than that of the first gate oxide layer; forming a polysilicon layer on the first gate oxide layer and the second gate oxide layer, wherein the polysilicon layer covers all or part of the rectangular region of the first gate oxide layer, the inclined region away from the shallow trench isolation structure, and the second gate oxide layer; Etching the first gate oxide layer to remove the inclined region of the first gate oxide layer close to the shallow trench isolation structure, so that the side wall of the first gate oxide layer away from the shallow trench isolation structure is inclined, and the side wall of the first gate oxide layer close to the shallow trench isolation structure is vertical; The polysilicon layer and the second gate oxide layer between adjacent first gate oxide layers are etched until the substrate is exposed to form a gate structure.

2. The method for forming a semiconductor device according to claim 1, wherein: The step of etching the oxide layer comprises: Etching the oxide layer by dry etching to form an inclined side wall, with a certain thickness of the oxide layer remaining on the substrate at both sides of the side wall; A wet etching process is used to remove the remaining oxide layer of a certain thickness to form a first gate oxide layer.

3. The method for forming a semiconductor device according to claim 2, wherein: The etching gas for the dry etching is a mixed gas of C4F8, CF4 and CHF3, and the volume ratio of the mixed gas is 2:1:

3.

4. The method for forming a semiconductor device according to claim 1, wherein: The included angle between the sidewall of the first gate oxide layer and the substrate is 30° to 60°.

5. The method for forming a semiconductor device according to claim 1, wherein: The oxide layer is formed by chemical vapor deposition.

6. The method for forming a semiconductor device according to claim 1, wherein: The step of etching the first gate oxide layer comprises: Using a dry etching process, the side wall of one side of the first gate oxide layer is made vertical, and the side wall of the other side is kept in an inclined shape, and a certain thickness of the first gate oxide layer remains on the substrate on the side of the vertical side wall; A wet etching process is used to remove the first gate oxide layer remaining to a certain thickness.

7. The method for forming a semiconductor device according to claim 6, wherein: The etching gas for the dry etching is a mixed gas of CF4 and CHF3.

8. The method for forming a semiconductor device according to claim 2 or 6, wherein: The wet etching solution is hydrofluoric acid.

9. The method for forming a semiconductor device according to claim 1, wherein: The step of etching the polysilicon layer and the second gate oxide layer comprises: Etching the polysilicon layer by dry etching until the second gate oxide layer is exposed; The second gate oxide layer is etched by a dry etching process until the substrate is exposed.

10. The method for forming a semiconductor device according to claim 9, wherein: The etching gases for dry etching the polysilicon layer are hydrogen bromide and chlorine.

11. The method for forming a semiconductor device according to claim 9, wherein: The etching gas used for dry etching the second gate oxide layer is hydrogen bromide and helium.

12. The method for forming a semiconductor device according to claim 6, wherein: After forming the gate structure, a source region and a drain region are formed in the substrate on both sides of the gate structure, wherein the source region is close to the inclined sidewall of the first gate oxide layer, and the drain region is close to the vertical sidewall of the first gate oxide layer.

Citation Information

Patent Citations

  • Semiconductor device and method for fabricating thesame

    KR1020010047658A

  • Semiconductor device and manufacturing method thereof

    US20020072159A1

  • Metal oxide semiconductor field-effect transistor and associated methods

    US20030141559A1

  • Self-aligned complementary ldmos

    US20070228463A1