A selective emitter passivation contact solar cell and its preparation method
By thinning the polysilicon doped layer and reducing the doping concentration, combined with selective emitter passivation contact structure and laser doping technology, the problem of insufficient short-circuit current of TOPCon solar cells is solved, and the conversion efficiency and open circuit voltage are improved, which is suitable for industrialization Production.
Patent Information
- Application Number
- CN202011245563.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-11-10
AI Technical Summary
The existing TOPCon solar cells have shortcomings in short-circuit current increase, and the long-band reflectivity of the polysilicon layer on the back is poor, resulting in carrier absorption loss and affecting conversion efficiency.
By thinning the thickness of the N+ polysilicon doped layer and reducing the overall doping concentration, a selective emitter passivation contact structure is adopted, including preparing a tunneling oxide layer and an intrinsic amorphous silicon layer on the back, and forming an N++ heavy by laser doping Doping regions reduces the free carrier absorption effect.
It effectively improves the short-circuit current, improves the conversion efficiency of solar cells, and maintains high open circuit voltage and fill factor, making it suitable for industrial production.
Smart Images

Figure CN112331742B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a selective emitter passivation contact solar cell and a preparation method thereof. Background Art
[0002] Tunnel Oxide Passivated Contact (Topcon) technology is a passivation contact structure based on ultra-thin silicon oxide and doped polycrystalline silicon (poly-Si). This passivation structure allows majority carriers to tunnel through the oxide layer, blocking minority carriers, achieving selective carrier passage and greatly reducing the recombination rate of minority carriers, thus avoiding the high recombination risk of metal electrode contact. Therefore, Topcon cells have a higher open circuit voltage and are one of the important directions of research and development on the surface passivation of industrialized high-efficiency solar cells.
[0003] However, although the open-circuit voltage and fill factor have been greatly improved in the current TOPCon battery industrialization, which has brought about a significant improvement in conversion efficiency, the improvement in short-circuit current has remained the same, or even slightly decreased (compared with the N-PERT baseline).
[0004] The applicant found in the study that the thickness and doping concentration of the back polysilicon layer are important factors that hinder the improvement of its short-circuit current. Through optical testing of the passivation contact structure, it was found that the reflectivity of the back surface passivation contact area is poor in the long-wave band, that is, absorption loss occurs in the long-wave band (800-1200nm). The fundamental reason is that the high polysilicon doping layer is mainly a free carrier absorption effect in the infrared band. It exists as a parasitic absorption process and cannot form effective photogenerated carriers. This phenomenon is more obvious in high-doping concentration semiconductors; while the lower doping concentration and thinner polysilicon layer, although it does not affect the overall passivation effect, will cause the back electrode contact resistance to be too large, thereby affecting the improvement of the fill factor FF. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a selective emitter passivation contact solar cell and a preparation method thereof, which can reduce the thickness of the N+ polysilicon doping layer and reduce the overall doping concentration, that is, minimize the free carrier absorption effect, increase the short-circuit current, and thus improve the solar cell conversion efficiency.
[0006] The technical solution adopted by the present invention to solve the above technical problems is: a method for preparing a selective emitter passivation contact solar cell, the method comprising:
[0007] S1, N-type silicon wafer pretreatment and double-sided texturing;
[0008] S2. Front side processing of N-type silicon wafer:
[0009] Prepare a P+ doped layer on the front side of an N-type silicon wafer;
[0010] S3, Back side processing of N-type silicon wafer:
[0011] A tunnel oxide layer and an intrinsic amorphous silicon layer of a certain thickness are sequentially prepared on the back of an N-type silicon wafer, and then the intrinsic amorphous silicon layer is converted into a polysilicon layer, and an N+ polysilicon doping layer is formed on the back of the silicon wafer;
[0012] S4, back selective heavy doping:
[0013] Performing selective heavy doping on the N+ polysilicon doping layer to form an N++ heavily doped region;
[0014] S5. Remove other unnecessary layers caused by the process;
[0015] S6, forming a front passivation anti-reflection layer on the front side of the N-type silicon wafer, and forming a back passivation anti-reflection layer on the back side of the N-type silicon wafer;
[0016] S7. Electrode metallization is performed on the front and back sides of the N-type silicon wafer respectively to obtain a front electrode and a back electrode; wherein the back electrode is overprinted on the N++ heavily doped region.
[0017] According to the above method, the S2 is specifically:
[0018] A PN junction is formed through a front boron diffusion process; etching is performed to remove the back and edge boron emitter junctions on one side, and the front borosilicate glass layer is retained as a mask layer for the next process.
[0019] According to the above method, the S5 includes: removing the front-side plated polysilicon layer; removing the front-side mask layer and the residual doping source on the back side.
[0020] According to the above method, it also includes the step of front selective heavy doping, performing front selective heavy doping on the P+ doping layer to form a P++ heavily doped area;
[0021] The step of selectively heavily doping the front side is performed after removing the polysilicon coated around the front side and before removing the mask layer on the front side and the residual doping source on the back side;
[0022] The front electrode is overprinted on the P++ heavily doped region.
[0023] According to the above method, the back side selective heavy doping and / or the front side selective heavy doping are performed by laser doping.
[0024] According to the above method, during laser doping, the laser mode is a pulse nanosecond mode, a continuous mode or a quasi-continuous mode, and the laser wavelength is 200nm to 1100nm.
[0025] According to the above method, during laser doping, the laser energy distribution is Gaussian distribution or flat-top distribution.
[0026] According to the above method, during laser doping, the laser processing method is a galvanometer scanning method, or the XY module drives the laser module or the N-type silicon wafer to move relative to each other for processing.
[0027] According to the above method, the thickness of the intrinsic amorphous silicon layer in S3 is 40-120nm, the thickness of the obtained N+ polysilicon doped layer is 40-120nm, the square resistance of the N+ polysilicon doped layer in S3 is 100-300Ω / □, and the square resistance of the N++ heavily doped area is 40-70Ω / □.
[0028] According to the above method, the square resistance of the P+ doped layer is 120-200Ω / □, and the square resistance of the P++ heavily doped region is 70-90Ω / □.
[0029] According to the above method, the front side coated polysilicon layer is removed by chemical etching or laser scanning processing.
[0030] A selective emitter passivation contact solar cell is prepared by adopting the method.
[0031] The beneficial effects of the present invention are:
[0032] 1. By preparing a selective emitter on the back side, the contact resistance between the electrode and the N++ heavily doped area can be effectively reduced, while reducing the metal contact recombination rate of the N++ heavily doped area under the metal gate line. Under the premise of ensuring the passivation effect and high fill factor, the thickness of the N+ polysilicon doping layer can be reduced as much as possible and the overall doping concentration can be reduced, that is, the free carrier absorption effect can be minimized, the short-circuit current can be increased, and the conversion efficiency of the solar cell can be improved.
[0033] 2. The configuration of the front and back double-sided heavy doping of the present invention reduces the contact resistance between the silver aluminum paste and the P++ heavily doped area due to the introduction of heavy doping on the front side, and at the same time reduces the recombination rate of the P++ heavily doped area under the metal gate line, further improving the open circuit voltage of the battery; the diffusion square resistance of the P+ doped layer is increased, which also increases the open circuit voltage and short-circuit current of the battery to a certain extent, thereby further improving the conversion efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a flow chart of a method according to Embodiment 1 of the present invention.
[0035] Figure 2This is a schematic diagram of the battery structure of Example 1 of the present invention.
[0036] Figure 3 This is a schematic diagram of the battery structure of Example 3 of the present invention.
[0037] In the figure: 201-N-type silicon substrate, 202-tunneling oxide layer, 203-N+ polysilicon doped layer, 204-N++ heavily doped region, 205-back passivation anti-reflection layer, 206-P+ doped layer, 207-front passivation anti-reflection layer, 208-back electrode, 209-front electrode, 210-P++ layer. DETAILED DESCRIPTION
[0038] The present invention is further described below in conjunction with specific examples and drawings.
[0039] Embodiment 1:
[0040] like Figure 1 As shown, the present invention provides a method for preparing a selective emitter passivation contact solar cell, the method comprising:
[0041] 1. N-type silicon wafer pretreatment and double-sided texturing.
[0042] 2. Front side processing of N-type silicon wafer:
[0043] A P+ doping layer is arranged on the front side of the N-type silicon wafer. Specifically, the silicon wafer enters a diffusion furnace tube to undergo a front boron diffusion process to form a PN junction.
[0044] 3. Etching: remove the back and edge boron emitter junctions on one side, while retaining the front BSG (borosilicate glass) as a mask layer for the next process to protect the front PN junction.
[0045] 4. Preparation of tunnel oxide layer on the back of N-type silicon wafer:
[0046] Specifically, a tunneling oxide layer is grown on the back side of the N-type silicon wafer.
[0047] 5. Preparation of intrinsic amorphous silicon layer on the back:
[0048] Specifically, a certain thickness of intrinsic amorphous silicon layer is deposited on the tunnel oxide layer. In this embodiment, the thickness of the intrinsic amorphous silicon layer is 40-120nm. At present, the thickness of amorphous silicon on the back of conventional topcon cells is about 150-200nm, but in the present invention, since selective heavy doping is performed on the back later, it can be reduced to 40-120nm.
[0049] 6. Crystallization and phosphorus diffusion
[0050] Specifically, the silicon wafer enters the diffusion furnace tube for crystallization treatment, converts the intrinsic amorphous silicon layer into a polycrystalline silicon layer, and forms an N+ polycrystalline silicon doped layer on the back of the silicon wafer. The thickness of the N+ polycrystalline silicon doped layer is 40-120nm, and its square resistance is 100-200Ω / □, preferably 140Ω / □.
[0051] 7. Selective heavy doping on the back side:
[0052] The N+ polysilicon doping layer is selectively heavily doped to form an N++ heavily doped area. The selective heavy doping is to form an N++ heavily doped area corresponding to the back electrode (also called gate line) prepared subsequently, that is, the N++ heavily doped area is directly below the gate line (the back of the N-type silicon wafer is facing upward at this time). In this embodiment, laser doping is adopted to dope the back gate line area with laser to form an N++ heavily doped area. The laser mode is a pulsed ns (nanosecond) mode, a continuous (CW) mode or a quasi-continuous (QCW) mode; the laser energy distribution is a Gaussian distribution or a flat-top distribution; the laser wavelength is 200nm to 1100nm; the laser spot is circular or square; the laser processing method is a galvanometer scanning method or an XY module drives the laser module and the product to move relative to each other for processing. The square resistance of the obtained N++ heavily doped area is 40 to 70Ω / □.
[0053] 8. Removal of the front-side polysilicon layer In this embodiment, chemical etching can be used: acid system solution (HF / HNO3+additive mixture), alkaline system solution (NaOH, KOH, TMAH and other solutions), or laser scanning processing.
[0054] 9. Remove the mask layer on the front side and the residual doping source on the back side. In this embodiment, since the front side adopts the boron diffusion process, the mask layer on the front side is BSG (borosilicate glass); the back side adopts the laser doping method, so the residual doping source on the back side is PSG (phosphorus silicon glass).
[0055] 10. A front passivation anti-reflection layer is formed on the front side of the N-type silicon wafer, and a back passivation anti-reflection layer is formed on the back side of the N-type silicon wafer.
[0056] Specifically, a double-sided deposition method is adopted. The back passivation anti-reflection layer is a SiNx film or a SiOx / SiNx double-layer film from the inside to the outside, or a SiOx / SiNx / SiONx triple-layer film from the inside to the outside, the front passivation anti-reflection layer is a SiNx film or an AlOx / SiNx double-layer film from the inside to the outside, or a different combination of AlOx / SiNx / SiONx triple-layer film, and the tunneling passivation layer is a tunneling oxide layer.
[0057] 11. Electrode metallization is performed on the front and back sides of the N-type silicon wafer to obtain a front electrode and a back electrode; wherein the back electrode is overprinted on the N++ heavily doped region.
[0058] The present invention also provides a selective emitter passivation contact solar cell, which is prepared by the method described above. Figure 2 As shown, the cell includes an N-type silicon substrate 201, a P+ doped layer 206 and a front passivation anti-reflection layer 207 arranged sequentially from bottom to top on the front side; a tunneling oxide layer 202, an N+ polysilicon doped layer 203, and a back passivation anti-reflection layer 205 arranged sequentially on the back side, and the position corresponding to the N+ polysilicon doped layer 203 and the back electrode 208 is an N++ heavily doped region 204. It also includes a front electrode 209, which is in contact with the P+ doped layer; the back electrode 208 is in contact with the N++ heavily doped region 204 of the N+ polysilicon doped layer 203, forming a selective emitter.
[0059] The battery selective emitter of the present invention can technically reduce the deposition thickness and doping concentration of the polysilicon layer while ensuring the open circuit voltage enhancement effect, which can effectively reduce the free carrier absorption effect (FCA), increase the short circuit current, and thus improve the conversion efficiency of the Topcon battery. Reducing the deposition thickness of the polysilicon layer makes the polysilicon layer plated on the front side thinner, which is more convenient to remove.
[0060] The phosphosilicate glass or phosphorus source formed in the back-side doping process is used as a laser doping source to form local heavy doping (N++ layer) in the gate line contact area, reducing the contact resistance between Ag and the N++ layer and ensuring the advantage of the fill factor (FF).
[0061] The process flow of the invention is simple and suitable for application in large-scale production of existing production lines.
[0062] Embodiment 2:
[0063] The scheme and principle of this embodiment are basically the same as those of the first embodiment, except that:
[0064] The selected N-type silicon wafer has a resistivity of 0.3-10 ohm·cm and a thickness of 90-200 μm. The N-type silicon wafer is pre-processed and textured using existing technology to form a pyramid structure.
[0065] The silicon wafer is loaded into a tubular diffusion furnace using existing technology to form a PN junction through front diffusion. The boron source is boron tribromide, the diffusion temperature is 900-1100°C, and the square resistance of the P+ doped layer after boron diffusion is 70-110Ω / □, and the surface concentration is greater than 1E19cm -3The conventional boron diffusion process specifically adopted in this embodiment has a diffusion temperature of 920°C and a time of 35 minutes. After the boron diffusion, the square resistance of the P+ doped layer is 90Ω / □ and the surface concentration is 3E19cm -3 .
[0066] In this embodiment, a single-sided etching and polishing process is performed on the back and edge of the silicon wafer using a HF / HNO3 mixed solution to remove the P+ doped layer that spreads to the back during boron diffusion, and the edge is etched to insulate the front and back surfaces; at the same time, the front BSG is retained as a barrier layer, i.e., a mask layer.
[0067] A tunneling oxide layer with a thickness of 1 to 3 nm is prepared on the back of the silicon wafer by high-temperature thermal oxidation, nitric acid oxidation or ozone oxidation, wherein the thickness is preferably 1.5 nm. Specifically, in this embodiment, a tunneling oxide layer with a thickness of 1.5 nm is prepared on the back of the silicon wafer by high-temperature thermal oxidation.
[0068] By using LPCVD or PECVD, an amorphous silicon layer with a thickness of 40 to 120 nm is deposited on the back of the silicon wafer, wherein the preferred thickness is 70 nm. At this time, a circle of coating will be generated on the front. In this embodiment, an amorphous silicon layer with a thickness of 70 nm is deposited on the back of the silicon wafer by using LPCVD.
[0069] The intrinsic amorphous silicon layer is crystallized and doped, and the amorphous silicon layer is converted into a polycrystalline silicon layer. At the same time, a polycrystalline silicon doped layer (N+ layer) is formed on the back of the silicon wafer. Specifically, the silicon wafer enters the diffusion furnace tube for crystallization, the doping method is tubular diffusion, the phosphorus source is phosphorus oxychloride, the temperature is 800-865°C, the time is 10-20min, the small nitrogen flow rate is 50-150sccm; the polycrystalline silicon layer has a square resistance of 70-90Ω / □. In this embodiment, the temperature is 825°C, the time is 15min, the small nitrogen flow rate is 100sccm; the polycrystalline silicon layer has a square resistance of 120Ω / □.
[0070] Selective doping on the back side, after selective doping, the square resistance of the heavily doped area is 40 to 70Ω / □. Preferably, laser is used for selective doping. The laser pulse width is ns (nanoseconds), CW mode or QCW mode; the laser energy distribution is Gaussian distribution or uniform distribution; the laser wavelength is 200nm to 1100nm; the laser spot is circular or square; the laser processing method is galvanometer scanning or XY module reciprocating processing. In this embodiment, a 532nm laser is used, with a power of 28W, a scanning speed of 26m / s, and a spot size of 120um*120um. The metal grid line area on the back side is scanned by a galvanometer for local doping advancement, and the square resistance after the laser is 45Ω / □.
[0071] The polysilicon layer on the front side is removed by using HNO3 / HF mixed solution. The borosilicate glass on the front side and the phosphorus silicon glass on the back side are removed by using HF solution.
[0072] In order to increase the passivation characteristics of the front and back surfaces and the absorption of light, a layer of SiNx film or a double-layer film of AlOx / SiNx or a triple-layer film of AlOx / SiNx / SiONx is deposited on the front surface as the front passivation anti-reflection layer 207, and a layer of SiNx film or a double-layer film of SiOx / SiNx or a triple-layer film of SiOx / SiNx / SiONx is deposited on the back surface as the back passivation anti-reflection layer 205. In this embodiment, a double-layer film of AlOx / SiNx is deposited on the front surface, and the thicknesses thereof are 5nm and 75nm respectively; a layer of SiNx film is deposited on the back surface, and the thickness thereof is 80nm.
[0073] The electrodes on the front and back sides of the silicon wafer are metallized using existing technology. In this embodiment, gate line electrodes are printed on the front and back sides, wherein the back electrode needs to be overprinted on the laser heavily doped area, and high-temperature sintering is performed to complete the metallization of the front and back sides of the battery.
[0074] The electrical performance data of the TOPCON battery of this embodiment and the prior art are shown in Table 1:
[0075] Table 1
[0076]
[0077] The above-mentioned prior art TOPCON battery used for comparison is also a battery obtained by the method of Example 2 of the present invention, the difference being that it does not undergo back selective doping, and the thickness of its N+ doping layer is 150 nm.
[0078] In the present invention, a selective emitter Topcon solar cell is prepared by reducing the thickness of the back polysilicon layer, the doping concentration, and the local heavy doping method. The efficiency is tested to reach 22.69%, which is 0.24% higher than that of traditional conventional Topcon solar cells. The main reason is the increase in short-circuit current, which shows that the free carrier absorption effect of the back polysilicon causes short-circuit current loss. The present invention adjusts the polysilicon thickness, doping concentration, and local heavy doping to ensure high open circuit voltage and fill factor while improving the short-circuit current, thereby improving the Topcon cell conversion efficiency.
[0079] Embodiment 3
[0080] The scheme and principle of this embodiment are basically the same as those of the first embodiment, except that:
[0081] Step 2 Boron Diffusion
[0082] In step 2, a P+ doped layer is provided on the front side of the N-type silicon wafer. After boron diffusion, the sheet resistance of the P+ doped layer is 120-200Ω / □, and the surface concentration is 3E19-5E19cm -3 .
[0083] Between step eight and step nine, there is also a front selective doping step:
[0084] Specifically, the P+ doping layer is selectively heavily doped to form a P++ heavily doped area. The selective heavy doping is to form a P++ heavily doped area corresponding to the subsequently prepared front electrode (also called gate line), that is, the P++ heavily doped area is directly below the front gate line (the front side of the N-type silicon wafer is facing upward at this time). In this embodiment, laser doping is adopted to dope the front gate line area with laser to form a P++ heavily doped area. The laser mode is a pulsed ns (nanosecond) mode, a continuous (CW) mode or a quasi-continuous (QCW) mode; the laser energy distribution is a Gaussian distribution or a flat-top distribution; the laser wavelength is 200nm to 1100nm; the laser spot is circular or square; the laser processing method is a galvanometer scanning method or an XY module drives the laser module and the product to move relative to each other for processing. The square resistance of the obtained P++ heavily doped area is 70 to 90Ω / □.
[0085] In step eleven, electrode metallization is performed on the front and back sides of the N-type silicon wafer respectively to obtain a front electrode and a back electrode; wherein the back electrode is overprinted on the N++ heavily doped area, and the front electrode is overprinted on the P++ heavily doped area.
[0086] The present invention also provides a selective emitter passivation contact solar cell, which is prepared by the method described above. Figure 3 As shown, the cell includes an N-type silicon substrate 201, a P+ doped layer 206 and a front passivation anti-reflection layer 207 arranged in sequence from bottom to top on the front side; a tunneling oxide layer 202, an N+ polysilicon doped layer 203, and a back passivation anti-reflection layer 205 arranged in sequence on the back side, the position corresponding to the N+ polysilicon doped layer 203 and the back electrode 208 is an N++ heavily doped region 204, and the back electrode 208 is in contact with the N++ heavily doped region 204 of the N+ polysilicon doped layer 203 to form a selective emitter; the position corresponding to the P+ doped layer 206 and the front electrode 209 is a P++ heavily doped region 210, and the front electrode 209 is in contact with the P++ heavily doped region 210 of the P+ doped layer 206 to form a selective emitter.
[0087] The configuration of the front and back double-sided heavy doping of the present invention reduces the contact resistance between the silver aluminum paste and the P++ heavily doped area due to the introduction of heavy doping on the front side, and at the same time reduces the recombination rate of the P++ heavily doped area under the metal grid line, further improving the open circuit voltage of the battery; the diffusion square resistance of the P+ doped layer is improved, which also improves the open circuit voltage and short-circuit current of the battery to a certain extent, thereby further improving the conversion efficiency of the battery.
[0088] Embodiment 4
[0089] The scheme and principle of this embodiment are basically the same as those of the second embodiment and the third embodiment.
[0090] The front boron diffusion is a front selective doping diffusion process, where the diffusion temperature is 910℃ and the time is 25min. After the boron diffusion, the square resistance of the P+ doped layer is 120~200Ω / □, and the surface concentration is 3E19~5E19cm -3 In this embodiment, the doping square resistance of the front P+ layer is 150Ω / □, and the surface concentration is 4E19cm -3 .
[0091] When heavily doping on the front side, a 532nm laser with a power of 32W, a scanning speed of 26m / s, and a spot size of 120um*120um is used to perform galvanometer scanning on the metal grid line area on the back side for local doping advancement. The laser rear resistance is 85Ω / □.
[0092] The electrical performance data of this embodiment, embodiment 2, and the TOPCON battery of the prior art are shown in Table 2:
[0093] Table 2
[0094]
[0095] The above embodiments are only used to illustrate the design ideas and features of the present invention, and their purpose is to enable those skilled in the art to understand the content of the present invention and implement it accordingly. The protection scope of the present invention is not limited to the above embodiments. Therefore, any equivalent changes or modifications made based on the principles and design ideas disclosed by the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing a selective emitter passivation contact solar cell, characterized in that: The method includes: S1, N-type silicon wafer pretreatment and double-sided texturing; S2. Front side processing of N-type silicon wafer: A P+ doped layer is provided on the front side of the N-type silicon wafer; S3, Back side processing of N-type silicon wafer: A tunnel oxide layer and an intrinsic amorphous silicon layer of a certain thickness are sequentially prepared on the back of an N-type silicon wafer, wherein the thickness of the intrinsic amorphous silicon layer is 40 to 120 nm; the intrinsic amorphous silicon layer is then converted into a polycrystalline silicon layer, and an N+ polycrystalline silicon doping layer is formed on the back of the silicon wafer; S4, back selective heavy doping: In the N+ polysilicon doping layer, selective heavy doping is performed by laser doping to form an N++ heavily doped region; S5. Remove other unnecessary layers caused by the process; S6, forming a front passivation anti-reflection layer on the front side of the N-type silicon wafer, and forming a back passivation anti-reflection layer on the back side of the N-type silicon wafer; S7. Electrode metallization is performed on the front and back sides of the N-type silicon wafer respectively to obtain a front electrode and a back electrode; wherein the back electrode is overprinted on the N++ heavily doped region.
2. The preparation method according to claim 1, characterized in that: The S2 is specifically: Forming PN junction through front boron diffusion process; Etching, single-sided removal of the back and edge boron emitter junctions, retaining the front borosilicate glass layer as a mask layer for the next process.
3. The preparation method according to claim 2, characterized in that: The S5 includes: removing the front-side plated polysilicon layer; removing the front-side mask layer and the residual doping source on the back side.
4. The preparation method according to claim 3, characterized in that: It also includes a step of selectively heavily doping on the front side, performing selectively heavily doping on the P+ doping layer on the front side to form a P++ heavily doped area; The step of selectively heavily doping the front side is performed after removing the polysilicon coated around the front side and before removing the mask layer on the front side and the residual doping source on the back side; The front electrode is overprinted on the P++ heavily doped region.
5. The preparation method according to claim 4, characterized in that: The front selective heavy doping is performed by laser doping.
6. The preparation method according to claim 1 or 5, characterized in that: During laser doping, the laser mode is a pulse nanosecond mode, a continuous mode or a quasi-continuous mode, and the laser wavelength is 200nm to 1100nm.
7. The preparation method according to claim 1 or 5, characterized in that: During laser doping, the laser energy distribution is Gaussian distribution or flat-top distribution.
8. The preparation method according to claim 1 or 5, characterized in that: During laser doping, the laser processing method is a galvanometer scanning method, or the XY module drives the laser module or the N-type silicon wafer to move relative to each other for processing.
9. The preparation method according to claim 1, characterized in that: The thickness of the N+ polysilicon doped layer obtained in S3 is 40-120 nm, the square resistance of the N+ polysilicon doped layer in S3 is 100-300Ω / □, and the square resistance of the N++ heavily doped region is 40-70Ω / □.
10. The preparation method according to claim 4, characterized in that: The square resistance of the P+ doped layer is 120-200Ω / □, and the square resistance of the P++ heavily doped region is 70-90Ω / □.
11. The preparation method according to claim 3, characterized in that: The removal of the front-side coated polysilicon layer is carried out by chemical etching or laser scanning processing.
12. A selective emitter passivation contact solar cell, characterized in that: The method is prepared by any one of claims 1 to 11.