Method for manufacturing glass device and glass device
By forming through holes on the glass substrate and thinning them, combined with the use of laser modification part and hydrogen fluoride etching liquid, the problem of reducing the mechanical strength of the glass substrate and long etching time is solved, and a stable production of glass thickness of less than 300 μm is achieved. Glass installation.
Patent Information
- Application Number
- CN201980036910.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-08
- Filing Date
- 2019-06-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-06-07
AI Technical Summary
When the through holes are formed in the glass substrate, the mechanical strength is reduced, especially the glass substrate with a thickness of 300 μm or less is prone to breakage when processing the conductive portion of the circuit, and the conventional dry etching method takes a long time, making it difficult to achieve practicality.
By forming through holes on the glass substrate and thinning them, the through holes and connection wiring are formed simultaneously by using a laser modification part and a hydrogen fluoride etching liquid to ensure that the thickness of the glass substrate is more than 50 μm and less than 300 μm, and the design of conical holes is adopted to improve the Mechanical strength.
A glass device having a glass thickness of 300 μm or less is easily manufactured to ensure that the glass substrate is processed stably when forming a circuit conductive portion, thereby improving the mechanical strength and reducing the manufacturing time.
Smart Images

Figure CN112335037B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a glass device having a glass substrate using a through hole, and the glass device. Background Art
[0002] In the past, for example, as a packaging technology for LSI (Large-Scale Integration), a packaging technology using through silicon vias (TSV) is known. Silicon substrates with through electrodes are widely used as (for example) interposers. Interposers are substrates that connect substrates with different distances between terminals (for example, ICs (Integrated Circuits) and printed circuit boards with different wiring design rules).
[0003] As described in Non-Patent Document 1, when forming TSVs on a silicon substrate, there is known a method of forming TSVs before, after, or during a step of forming an element such as a transistor or a circuit such as an electrode.
[0004] Here, not only is the silicon substrate expensive, but silicon is also a semiconductor. Therefore, in TSV technology, it is necessary to form a through hole on the silicon substrate and then perform insulation treatment, which increases the cost of the substrate. Therefore, for example, in order to reduce the cost of the interposer, a glass substrate with a through electrode formed in a cheap and large-area glass substrate (TSV: Through Silicon Via) has attracted attention.
[0005] When a glass substrate with a through electrode is used, a through hole needs to be formed in the glass substrate in the TGV technology. As a technology for forming a through hole in a glass substrate, for example, as described in Patent Document 1, a technology for forming a through hole by irradiation with a pulsed YAG laser is known.
[0006] In addition, Patent Document 2 describes a method for forming micro-holes in a photosensitive glass substrate. In the method described in Patent Document 2, a photomask is placed at a predetermined position on a photosensitive glass substrate and irradiated with ultraviolet light to form a latent image. Next, the photosensitive glass substrate is heat-treated to crystallize the latent image. Subsequently, a processing hole smaller than the latent image is formed at the center of the portion where the latent image is formed by laser. Next, etching is performed using hydrogen fluoride to selectively etch away the crystallized portion, thereby forming a hole.
[0007] Furthermore, Patent Document 3 describes a method of forming a hole in a flat glass by a pair of upper and lower core drills on the same axis facing each other on both sides of the flat glass.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2000-61667
[0011] Patent Document 2: Japanese Patent Application Publication No. 2001-105398
[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 54-126215
[0013] Non-patent literature
[0014] Non-patent document 1: Koji Yoshinaga, Tsuki Nomura, "Trends in research and development of TSV technology for 3-dimensional LSI packaging" (Progress in research and development of TSV technology for 3-dimensional LSI packaging), Science and Technology Trends, Institute of Science, Technology and Academic Policy, April 2010, No. 10 Summary of the invention
[0015] Problems to be solved by the invention
[0016] Since through holes are formed in the glass substrate, the mechanical strength of the glass substrate may be reduced. In particular, when glass with a thickness of less than 300 μm is used, due to the influence of reduced mechanical strength, when forming a conductive part such as a circuit, the glass may break during transportation, making it difficult to handle the glass substrate.
[0017] In addition, in TSV technology, as a method for forming through holes in silicon substrates, methods such as the Bosch process using dry etching have been established. However, it takes a long time to form through holes in glass substrates by dry etching, and it is difficult to be considered practical. In particular, the formation of through holes with a glass thickness of less than 300 μm and the application in electronic device substrates represented by interposers have very high technical difficulties and are difficult to be considered practical.
[0018] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a glass device having a glass substrate having a glass thickness of 300 μm or less in a simpler manner.
[0019] Means for solving problems
[0020] In order to solve the problem, a manufacturing method of a glass device according to one aspect of the present invention is a method for manufacturing a glass device obtained by forming one or more through holes in a glass substrate, and connecting a first wiring on a first surface of the glass substrate and a second wiring on a second surface which is a surface opposite to the first surface via the through holes, wherein after forming the first wiring, the through hole is formed by etching and the glass substrate is thinned, and then the wiring in the through hole and the second wiring are formed, and the first wiring and the second wiring are connected via the wiring in the through hole, the thickness of the glass substrate after the thinning is not less than 50 μm and not more than 300 μm, the shape of the through hole is a truncated cone shape with the opening of the second surface as the bottom, and the relationship between the opening diameter of the first surface and the opening diameter of the second surface of the through hole, that is, the second surface opening diameter / the first surface opening diameter is not less than 1.8 and not more than 2.2.
[0021] A method for manufacturing a glass device according to another aspect of the present invention includes: a step of forming a first wiring on a first surface of a glass substrate; a step of supporting the first wiring side of the glass substrate on which the first wiring is formed by a support; a step of irradiating the glass substrate from a surface opposite to the first surface with a laser to form a laser-modified portion extending from the first surface toward a surface opposite to the first surface, which serves as a starting point for forming a through hole; a step of forming a through hole by etching from the surface opposite to the first surface of the glass substrate toward the first surface using a hydrogen fluoride etching solution after the step of supporting by the support and the step of forming the laser-modified portion, thereby thinning the glass substrate and forming a through hole; a step of forming a through electrode inside the through hole, forming a second wiring on a surface of the glass substrate opposite to the first surface, and connecting the first wiring and the second wiring via the through electrode after the through hole is formed by removing the support from the glass substrate.
[0022] Effects of the Invention
[0023] According to the above aspect of the present invention, after wiring is formed on one surface, through holes are formed while thinning the glass substrate and etching is performed, thereby making it possible to more easily manufacture a glass device having a glass substrate with a glass thickness of 300 μm or less.
[0024] At this time, when the glass substrate is supported by a support body such as a glass carrier and etching is used to thin the glass and simultaneously form through holes, it can be ensured that the glass substrate is easy to handle when forming conductive parts such as circuits, and a glass device with a through electrode having a glass substrate thickness of less than 300 μm can be stably formed.
[0025] BRIEF DESCRIPTION OF THE DRAWINGS
[0026] [ Figure 1 ] is a cross-sectional view showing the steps of a method for manufacturing a glass device according to a first embodiment of the present invention.
[0027] [ Figure 2 ] is a cross-sectional view showing the steps of a method for manufacturing a glass device according to a second embodiment of the present invention.
[0028] [ Figure 3 ] is a diagram showing the relationship between the thickness T1 of the glass substrate before the thickness becomes thinner (thinned) and the length M1 of the laser modified portion.
[0029] [ Figure 4 ] is a diagram showing the relationship between the diameter D1 of the through hole and the glass substrate T2 after the hydrofluoric acid treatment.
[0030] [ Figure 5 ] is an example of a glass device using RF applications of the present invention.
[0031] [ Figure 6 ] is a glass interposer as an example of a glass device using the present invention. DETAILED DESCRIPTION
[0032] Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0033] It should be noted that the following description relates to examples of the present invention, and the present invention is not limited thereto.
[0034] <First Embodiment>
[0035] In the method for manufacturing a glass device according to the first embodiment, Figure 1 to explain.
[0036] (Step 1)
[0037] First, if Figure 1 As shown in (a), laser light is irradiated from the first surface 10a side toward the glass substrate 10 to form a laser modified portion 20 as a starting point of the through hole 40. The laser modified portion 20 is formed so as to extend downward (e.g., in a vertical direction) from the first surface 10a and to have its lower end rest in the glass substrate 10.
[0038] (Step 2)
[0039] Next, if Figure 1As shown in (b), a hydrofluoric acid-resistant metal film 11 is formed on the first surface 10a of the glass substrate 10 in a manner having a thickness in a range of 10 nm to 500 nm. Subsequently, a copper layer 111 is formed on the hydrofluoric acid-resistant metal film 11 in a manner having a thickness in a range of 100 nm to 500 nm. Through this step 2, a seed layer 112 is formed on the first surface 10a of the glass substrate 10. The material of the hydrofluoric acid-resistant metal film 11 is appropriately selected from (for example) chromium, nickel, and nickel-chromium.
[0040] (Step 3)
[0041] Next, if Figure 1 As shown in (c), a photoresist of a target pattern is formed. Although dry photoresist is usually used, in this step, a photosensitive film such as RD-1225 manufactured by Hitachi Chemical Co., Ltd. of direct imaging type is used to laminate the first surface 10a side, and then the set pattern is imaged and developed to expose the seed layer 112 formed in step 2. Power is supplied to the exposed seed layer to perform electrolytic copper plating with a thickness of 2 μm to 10 μm. After electroplating, the unnecessary dry film resist is dissolved and peeled off, and the seed layer is etched to form wiring.
[0042] (Step 4)
[0043] Next, if Figure 1 As shown in (d), insulating resin 12 is used for lamination, and blind holes are formed on the insulating resin 12 by laser. Subsequently, a dry film resist is laminated thereon, and after imaging a predetermined pattern, it is developed. Then, the unnecessary dry film resist is dissolved and peeled off to form wiring. After forming the wiring, a solder resist layer 13 is formed to form the wiring on the first surface 10a side, that is, the first surface wiring layer 14.
[0044] (Step 5)
[0045] Next, if Figure 1 As shown in (e), the glass carrier 30 constituting the support is bonded to the first surface wiring layer 14 via an adhesive 35 for temporary bonding. Considering the transportability after thinning, the thickness of the glass carrier 30 is expected to be in the range of 0.7 mm to 1.5 mm. The thickness of the glass carrier 30 can be appropriately set according to the thickness of the glass substrate. In addition, although the glass carrier 30 is exemplified as the support, the support does not have to be made of glass, and can also be made of metal, resin, etc.
[0046] (Step 6)
[0047] Next, if Figure 1As shown in (f), a wiring substrate formed by bonding a glass carrier 30 to a glass substrate 10 via an adhesive 35 is etched using a hydrogen fluoride solution from the surface of the glass substrate 10 opposite to the first surface 10a (the lower surface in the figure). The glass of the portion where the laser modified portion 20 is not formed is etched away by the hydrogen fluoride solution, and the thickness is reduced in a manner parallel to the first surface 10a of the glass substrate 10. When the hydrogen fluoride solution contacts the laser modified portion 20, the laser modified portion 20 is preferentially dissolved, thereby forming a through hole 40. As a result, the glass substrate 10 is thinned and the through hole 40 is formed. That is, the thickness thinning and the formation of the through hole 40 are achieved through a single etching process. The lower surface of the thinned glass substrate 10 becomes the second surface 10b on which the second surface wiring layer 15 is formed.
[0048] The etching amount by the hydrogen fluoride solution can be appropriately set according to the thickness of the glass device. For example, when the thickness T1 of the glass substrate 10 used in step 1 is 400 μm, the etching amount is preferably within a range of 100 μm to 350 μm.
[0049] The thickness T2 of the thinned glass substrate 10 is preferably not less than 50 μm and not more than 300 μm.
[0050] (Step 7)
[0051] Next, if Figure 1 (g) shows that the same process as step 1 and step 2 is performed. That is, a seed layer for power supply is formed on the second surface where the through hole 40 is formed, and a pattern is formed by a dry film resist. Subsequently, after power is supplied to the seed layer to perform electrolytic plating with a thickness of 2 μm to 10 μm, the unnecessary dry film resist is dissolved and peeled off to form a through electrode. Then, the unnecessary seed layer is removed and an outer protective film such as an insulating resin or a solder resist is applied.
[0052] Since the hydrogen fluoride solution is no longer used for etching in the subsequent steps, the seed layer for power supply on the second surface can use a material different from the hydrofluoric acid-resistant metal. In this case, a metal layer composed of a material different from the hydrofluoric acid-resistant metal is formed on the side of the through hole 40. Examples of materials different from the hydrofluoric acid-resistant metal include Ti, Cu, chemically plated Ni, etc., and at least one metal layer composed of such a material is formed on the side of the through hole 40. The material and the number of layers are not limited to the present content and can be appropriately set as needed.
[0053] The first wiring and the second wiring are stacked in at least one layer, and the number of stacked layers can be set as necessary.
[0054] In addition, an opening may be provided when an external connection terminal is required. The wiring on the second surface 10b side, that is, the second surface wiring layer 15 is formed by coating an outer protective film such as an insulating resin or a solder resist.
[0055] (Step 8)
[0056] Next, if Figure 1 As shown in (h), the glass carrier 30 temporarily attached in step 5 is removed, thereby completing the glass device.
[0057] <Second Embodiment>
[0058] In the method for manufacturing a glass device according to the second embodiment, Figure 2 to explain.
[0059] (Step 1)
[0060] First, if Figure 2 As shown in (a), a hydrofluoric acid-resistant metal film 11 is formed on the first surface 10a of the glass substrate 10 in a thickness range of 10 nm to 500 nm, and a copper layer 111 is formed on the hydrofluoric acid-resistant metal film 11 in a thickness range of 100 nm to 500 nm, thereby forming a seed layer 112. The material of the hydrofluoric acid-resistant metal film 11 is appropriately selected from (for example) chromium, nickel, and nickel-chromium.
[0061] (Step 2)
[0062] Next, if Figure 2 As shown in (b), a photoresist of a predetermined pattern is formed on the first surface 10a of the glass substrate 10. Although dry photoresist is generally used, in this step, a direct imaging type photosensitive film such as RD-1225 manufactured by Hitachi Chemical Co., Ltd. is used to laminate the first surface 10a side of the glass substrate 10. Then, the predetermined pattern is imaged and then developed to expose the seed layer 112 formed in step 1. Power is supplied to the exposed seed layer to perform electrolytic copper plating with a thickness of not less than 2 μm and not more than 10 μm, and then the dry film resist that is no longer needed is dissolved and peeled off to remove the seed layer, thereby forming wiring.
[0063] (Step 3)
[0064] Next, if Figure 2As shown in (c), the first surface 10a side is laminated with an insulating resin 12, and a blind hole is formed on the insulating resin 12 by laser. Subsequently, a dry film resist is used for lamination, and a predetermined pattern is imaged and then developed. Then, the dry film resist that is no longer needed is dissolved and peeled off to form wiring. After the wiring is formed, a solder resist layer 13 is formed to form the wiring on the first surface 10a side, i.e., the first surface wiring layer 14.
[0065] (Step 4)
[0066] Next, if Figure 2 As shown in FIG. 5 , the glass carrier 30 is bonded to the first surface wiring layer 14 via a temporary bonding adhesive 35. Considering the transportability after thinning, the thickness of the glass carrier 30 is preferably in the range of 0.7 mm to 1.5 mm. The thickness of the glass carrier 30 can be appropriately set according to the thickness of the glass substrate 10.
[0067] (Step 5)
[0068] Next, if Figure 2 As shown in (e), the glass substrate 10 is irradiated with laser light from the surface of the glass substrate 10 opposite to the first surface 10a (the lower surface in the figure) to form a laser modified portion 20. The laser modified portion 20 is formed in a manner perpendicular to the hydrofluoric acid-resistant metal film 11 formed in step 1 and with the lower end staying inside the glass substrate 10.
[0069] (Step 6)
[0070] Next, if Figure 2 As shown in (f), the glass substrate after the laser modified portion 20 is formed in step 5 is etched from the surface opposite to the first surface 10a (the lower surface in the figure) using a hydrogen fluoride solution. The glass portion where the laser modified portion 20 is not formed is etched away by the hydrogen fluoride solution, and the thickness of the glass substrate 10 is reduced in a manner parallel to the first surface wiring layer 14. When the hydrogen fluoride solution contacts the laser modified portion 20, the laser modified portion 20 is preferentially dissolved, thereby forming a through hole 40. As a result, the glass substrate 10 is thinned and the through hole 40 is formed. The lower surface of the thinned glass substrate 10 becomes the second surface 10b on which the second surface wiring layer 15 is formed.
[0071] The etching amount by the hydrogen fluoride solution can be appropriately set according to the thickness of the glass device. For example, when the thickness T1 of the glass substrate used in step 1 is 400 μm, the etching amount is preferably within a range of 100 μm to 350 μm.
[0072] The thickness T2 of the thinned glass substrate 10 is preferably not less than 50 μm and not more than 300 μm.
[0073] (Step 7)
[0074] Next, if Figure 2 As shown in (g), an electroless nickel plating layer or an electroless copper plating layer is formed on the second surface 10b having a through hole 40 as a seed layer for power supply, and a pattern is formed by a dry film resist, and power is supplied to the seed layer to perform electrolytic plating with a thickness of 2 μm to 10 μm. Subsequently, the dry film resist that is no longer needed is dissolved and peeled off to form a through electrode. Then, the seed layer that is no longer needed is removed and an outer protective film such as an insulating resin or a solder resist layer is coated. In the case where an external connection terminal is required, an opening portion may also be provided. By coating an outer protective film such as an insulating resin or a solder resist layer, wiring on the second surface 10b side, i.e., a second wiring layer, is formed.
[0075] Here, both the first-plane wiring layer 14 and the second-plane wiring layer 15 are in communication with the through-electrode formed in the through-hole 40 via the hydrofluoric acid-resistant metal film 11 .
[0076] (Step 8)
[0077] Next, if Figure 2 As shown in (h), the glass carrier 30 temporarily attached in step 5 is removed, thereby completing the glass device.
[0078] (Regarding the formation of laser modified area)
[0079] The laser modified portion 20 is a linear or rod-shaped region extending downward (e.g., in a direction perpendicular to the first surface 10a) from the first surface 10a of the glass substrate 10. The length of the laser modified portion 20 is set to be shorter than the thickness T1 of the glass substrate 10 in step 1 before thinning. Specifically, the length of the laser modified portion 20 is a length that is adapted to the thickness of the glass substrate 10 in the finally obtained glass device.
[0080] Figure 1 (a) and Figure 2 The wavelength λ of the laser used to form the laser modified portion 20 inside the glass shown in (e) is set to 535nm or less. The wavelength λ is preferably in the range of 355nm to 535nm. If the wavelength λ is less than 355nm, it is difficult to obtain laser output, and it may be difficult to form a stable laser modified portion 20. On the other hand, if the wavelength λ is greater than 535nm, the irradiation point becomes larger, and it is difficult to form the laser modified portion 20. In addition, due to the influence of heat, instead of the modification process, the ablation process is performed, which easily generates microcracks and cracks.
[0081] Furthermore, the laser pulse width is preferably in the range of picoseconds to femtoseconds. If it is nanoseconds or longer, it is difficult to control the energy per pulse, and microcracks are likely to occur, leading to breakage.
[0082] The energy of the laser pulse is preferably selected according to the material of the glass substrate 10 and the type of laser modified portion 20 to be formed. In one example, it is in the range of 5 μJ to 150 μJ. By increasing the energy of the laser pulse, the length of the laser modified portion 20 can be increased in proportion thereto.
[0083] (Regarding etching by hydrogen fluoride solution)
[0084] for Figure 1 (f) and Figure 2 The etching solution composed of a hydrogen fluoride solution shown in (f) contains one or more inorganic acids selected from the group consisting of nitric acid, hydrochloric acid and sulfuric acid in the hydrogen fluoride solution.
[0085] The concentration of hydrofluoric acid is, for example, not less than 1.0 wt % and not more than 6.0 wt %, and preferably, not less than 2.0 wt % and not more than 5.0 wt %.
[0086] In addition, the inorganic acid concentration is within the range of 1.0 wt % to 20.0 wt %, preferably, within the range of 3.0 wt % to 16.0 wt %. It is desirable that the hydrogen fluoride solution set within the above range is used and the etching rate is 1.0 μm / min or less. The temperature of the etching solution during etching is preferably 10° C. to 40° C.
[0087] In the etching using the hydrogen fluoride solution, the entire surface is uniformly etched starting from the surface on the side opposite to the first surface 10a. At this time, etching is performed toward the first surface 10a side in a manner parallel to the first surface 10a until the laser modified portion 20 is reached, thereby thinning the glass. When the hydrogen fluoride solution reaches the end of the laser modified portion 20, the laser modified portion 20 is preferentially etched, thereby forming a through hole 40 along the position of the laser modified portion 20.
[0088] At this time, since etching is performed from the lower side toward the first surface 10a side, the opening on the second surface side is processed into a truncated cone shape with a larger diameter (bottom surface), and the diameter of the through hole 40 formed therein becomes smaller from the second surface 10b toward the first surface 10a. Processing is performed so that the relationship between the opening diameter on the first surface side and the opening diameter on the second surface side (bottom surface side opening diameter) of the through hole 40 (second surface opening diameter / first surface opening diameter) is (for example) not less than 1.8 and not more than 2.2.
[0089] Here, if Figure 3 and Figure 4 As shown, the length M1 of the laser modified portion 20 can be calculated based on the glass thickness T2 after etching with the hydrogen fluoride solution and the diameter D1 of the through hole on the second surface, and the relationship satisfies "M1 = (D1 / 2) + T2" or approximately satisfies "M1 = (D1 / 2) + T2". Approximately satisfying "M1 = (D1 / 2) + T2" means that "M1" and "(D1 / 2) + T2" are basically equal, for example, "M1" / "(D1 / 2) + T2" is greater than 0.95 and less than 1.05. Therefore, the length M1 of the laser modified portion 20 can be appropriately set according to the desired diameter D1 of the through hole and the glass thickness T2 after etching. In addition, the etching amount generated by the hydrogen fluoride solution can be calculated based on the thinned thickness (i.e., "T1-T2").
[0090] According to the manufacturing method of the glass device of this embodiment, after wiring is performed on the first surface 10a side, the glass substrate is thinned by etching and through holes are formed, thereby making it possible to more easily manufacture a glass device having a glass substrate with a glass thickness of 300 μm or less.
[0091] At this time, while the glass substrate 10 is supported by the glass carrier 30, through holes are formed while the glass is thinned by etching, thereby ensuring that the glass substrate can be easily handled when forming conductive parts such as circuits, and a glass device with through electrodes having a glass substrate thickness of less than 300μm can be stably formed.
[0092] It should be noted that the etching process for thinning the glass and forming the through hole does not have to be performed at one time, and can be performed by etching multiple times. In short, it is sufficient to perform the process of thinning the glass and forming the through hole by etching.
[0093] The glass device described above can be used in applications such as Figure 5 The RF device shown, and Figure 6 In addition, the present embodiment can be applied to a glass device including a through electrode by easily adjusting the plate thickness of the glass device and forming a through electrode in the through hole.
[0094] The scope of the present invention is not limited to the exemplary embodiments described in the drawings, but also includes all embodiments that provide the same effect as the purpose of the present invention. In addition, the scope of the present invention is not limited to the combination of the features of the present invention defined by the claims, but can be defined by any desired combination of specific features among all the disclosed features.
[0095] In addition, the entire contents of Japanese Patent Application No. 2018-110668 (filed on June 8, 2018) to which this application claims priority are incorporated by reference into this disclosure.
[0096] Explanation of symbols
[0097] 10: Glass substrate
[0098] 11: Hydrofluoric acid resistant metal film
[0099] 12: Insulating resin
[0100] 13: Solder resist layer
[0101] 14: First surface wiring layer (first wiring)
[0102] 15: Second surface wiring layer (second wiring)
[0103] 20: Laser modification department
[0104] 30: Glass carrier (support)
[0105] 35: Adhesive
[0106] 40: Through hole
[0107] T1: Glass substrate thickness
[0108] T2: Thickness of glass substrate after etching
[0109] M1: Length of the laser modified part
[0110] D1: Diameter of the through hole on the second surface
[0111] RF: RF device
[0112] G-IP: Glass Interposer
Claims
1. A method for manufacturing a glass device, characterized in that: include: forming a first wiring on a first surface of a glass substrate; A step of supporting the first wiring side of the glass substrate on which the first wiring is formed by a support; a step of forming a laser modified portion extending from the first surface toward the surface opposite to the first surface and serving as a starting point for forming a through hole by irradiating the glass substrate with laser light from the surface opposite to the first surface; After the step of supporting by the support body and the step of forming the laser modified portion, etching from the surface of the glass substrate opposite to the first surface toward the first surface using a hydrogen fluoride etching solution to form a through hole while thinning the glass substrate; After the through-hole forming step, a through-electrode is formed inside the through-hole, a second wiring is formed on a surface of the glass substrate opposite to the first surface, and the first wiring and the second wiring are connected via the through-electrode; and a step of removing the support from the glass substrate after forming the second wiring, The through hole is in the shape of a truncated cone with a larger diameter on the surface opposite to the first surface. When the diameter of the through hole on the surface opposite to the first surface is set to D1, the thickness of the glass substrate after hydrogen fluoride etching is set to T2, and the length of the laser modified portion is set to M1, the relationship "M1=(D1 / 2)+T2" is satisfied, or the relationship "M1=(D1 / 2)+T2" is approximately satisfied. 2 . The method for manufacturing a glass device according to claim 1 , wherein the formation of the laser modified portion is performed before forming the first wiring or after forming the first wiring on the glass substrate. 3 . The method for manufacturing a glass device according to claim 1 , wherein the thickness of the glass substrate after the through-hole forming step is not less than 50 μm and not more than 300 μm. 4 . The method for manufacturing a glass device according to claim 1 , wherein the laser used to form the laser-modified portion has a laser pulse width in the range of picoseconds to femtoseconds.
5. The method for manufacturing a glass device according to claim 1 or claim 2, characterized in that, in the formation of the through electrode, a seed layer for allowing the conductive material that becomes the through electrode to adhere is formed on the inner periphery of the through hole, and then the through electrode is formed by plating. 6 . The method for manufacturing a glass device according to claim 1 , wherein the first wiring and the second wiring are each laminated by at least one layer.