Method for manufacturing metal wiring of semiconductor device
By performing plasma treatment on the silicon nitride layer SiN of the semiconductor device, the compressive stress is increased, the problem of cobalt loss in nodes of 7nm and below is solved, the bonding density of tungsten and sidewall silicon oxide dielectric layer is improved, and cobalt metal is avoided Corrosion enhances the reliability of the device.
Patent Information
- Application Number
- CN202011477780.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-12-15
AI Technical Summary
In semiconductor device manufacturing at nodes of 7 nm and below, the cobalt loss problem in the via layer causes the device to be broken, and the existing bondless layer-free selective tungsten deposition process has poor bonding in the cobalt metal connection, resulting in corrosion of the cobalt metal.
By performing plasma treatment on the silicon nitride layer SiN, the compressive stress between the dielectric layer and the side wall of the tungsten plug is increased, the infiltration of the abrasive liquid and the cleaning liquid is reduced, and the bonding density of the tungsten and the side wall silicon oxide dielectric layer is improved. Avoid corrosion of cobalt metal.
It effectively reduces the problem of cobalt loss, enhances the bonding density of metal tungsten and sidewall silicon oxide dielectric layer, prevents cobalt metal from being corroded during chemical mechanical grinding, and improves the reliability of the device.
Smart Images

Figure CN112582339B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor integrated circuit technology, and in particular to a method for manufacturing metal wiring of a semiconductor device, which is used to solve the cobalt deficiency of an interconnection layer in a manufacturing process of a 7nm or lower node. Background Art
[0002] As the size of semiconductor devices shrinks, the CD of contact holes or contact grooves shrinks, RS (sheet resistance, also known as film resistance) increases, and the contribution of the bonding layer (Ti / TiN) to RS becomes more and more obvious. At present, many international research institutions have carried out research on the selective tungsten deposition process (selective W deposition) technology without the need for a bonding layer, especially in the filling of the via layer Via 0 (V0) at technology nodes of 10nm and below, and have achieved certain results. Since 7nm has begun to have higher requirements for the RS of the contact groove in the interconnect layer (M0), it is usually necessary to use cobalt metal with lower RS to replace the traditional tungsten metal.
[0003] For the metal connection interconnection of the node M0 / layer below 10nm, there are currently multiple solutions in the industry, such as Co / Co, Co / W, and W / W. In the most common Co / W solution, the manufacturing method of metal connections of semiconductor devices in the prior art uses a selective metal tungsten deposition process without an adhesive layer for the through-hole layer.
[0004] However, those skilled in the art know that if the through-hole layer adopts a selective metal tungsten deposition process without a bonding layer, the through-hole layer and the silicon oxide / silicon nitride dielectric layer on the sidewall will not be well bonded, which will cause the tungsten in the subsequent through-hole layer to corrode the active cobalt in the lower layer (interconnection line layer) through this interface during the chemical mechanical polishing (W CMP) manufacturing process, resulting in a cobalt missing (Co missing) problem, causing the device to short-circuit. Summary of the invention
[0005] The purpose of the present invention is to provide a method for manufacturing metal connections of semiconductor devices, which is used to solve the problem of cobalt missing in nodes of 7nm and below. The method utilizes the stress effect on silicon nitride SiN to significantly shorten the time of exposure of the interface between the upper SiN / W layer and the middle oxide / SelW layer to the W polishing liquid and the cleaning liquid during CMP polishing, thereby reducing the contact of the polishing liquid with metal cobalt (cobalt), thereby alleviating the cobalt missing problem in the lower layer.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] A method for manufacturing a metal connection of a semiconductor device comprises the following steps:
[0008] Step S1: providing a substrate including an interconnect layer structure, and forming a dielectric layer on the substrate, wherein the interconnect material in the interconnect layer structure includes metal cobalt, and the dielectric layer includes a contact hole etch stop layer, a silicon oxide layer SiO2, and a silicon nitride layer SiN grown sequentially on the substrate;
[0009] Step S2: performing a standard photolithography and etching process on the dielectric layer to form a patterned through-hole layer; wherein the through-holes in the through-hole layer penetrate the dielectric layer;
[0010] Step S3: depositing tungsten on the via layer by a selective tungsten deposition process to form a via tungsten plug in the via layer; wherein at least one of the via tungsten plugs is in contact with the interconnect layer structure;
[0011] Step S4: performing a plasma treatment process on the surface of the through-hole layer to generate compressive stress in the silicon nitride layer SiN to increase the squeezing force between the dielectric in the dielectric layer and the side wall of the through-hole tungsten plug;
[0012] Step S5: depositing a TiN adhesion layer and a metal tungsten layer in sequence to form a through-hole tungsten plug covering layer on the through-hole layer;
[0013] Step S6: performing a tungsten chemical mechanical planarization process on the through-hole tungsten plug capping layer to form a planarized through-hole layer.
[0014] Furthermore, the gas source used in the plasma treatment process in step S4 includes argon Ar, hydrogen H2 or nitrogen N2.
[0015] Further, the interconnection line layer structure is an interconnection line layer structure M0; and the through hole layer is a through hole layer V0.
[0016] Furthermore, the material of the contact hole etch stop layer is silicon nitride or nitrogen-doped silicon carbide.
[0017] Furthermore, the step S4 further comprises performing a compressive stress process on the surface of the through-hole layer to increase the compressive stress between the dielectric in the dielectric layer and the metal tungsten and the side wall in the through-hole.
[0018] Furthermore, the compressive stress process is a plasma bias bombardment process.
[0019] Furthermore, the plasma bias bombardment process is a heavy ion plasma bias bombardment process.
[0020] Furthermore, the heavy ions are Ar ions.
[0021] Furthermore, the dielectric layer includes, from bottom to top, a contact hole etch stop layer and a flow chemical vapor deposited silicon oxide layer, and step S4 also includes performing a water vapor annealing process on the flow chemical vapor deposited silicon oxide layer to further increase the compressive stress between the dielectric in the dielectric layer and the side wall of the through-hole tungsten plug.
[0022] It can be seen from the above technical scheme that the present invention provides a method for manufacturing metal wiring of a semiconductor device, wherein the dielectric layer structure of SiN / SiO2 (N / O) originally used in the through-hole layer is replaced with a SiN / SiO / SIN (N / O / N) structure, and after the through-hole layer is etched (Etch) to form through holes and grooves, selective tungsten is filled in, and then the upper layer of SiN is subjected to plasma treatment, including but not limited to Ar / H2 / N2 gas source; after the plasma treatment, the upper layer of SiN on the surface generates a compressive stress; under the action of the compressive stress, the infiltration of the grinding liquid and the cleaning liquid can be effectively prevented, Co corrosion can be reduced or even eliminated, and the number of Co missing defects can be reduced; thereby, the tightness of the bonding between the metal tungsten and the silicon oxide dielectric layer of the side wall is enhanced to prevent the grinding liquid of the subsequent tungsten CMP in the through-hole layer from corroding the cobalt metal in the lower layer (metal interconnection layer M0) through this interface, thereby solving the cobalt missing problem, and from the perspective of process integration, it is not complicated. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The flowchart of the method for manufacturing metal wiring of a semiconductor device according to an embodiment of the present invention is shown.
[0024] Figure 2-Figure 11 FIG. 1 is a schematic diagram showing a process for forming metal wiring of a semiconductor device in a preferred embodiment (Embodiment 1) of the present invention. DETAILED DESCRIPTION
[0025] The following is combined with Figure 1-11 , the specific implementation modes of the present invention are further described in detail.
[0026] The present invention discloses a method for manufacturing metal wiring of a semiconductor device, which enhances the adhesion between tungsten and the silicon oxide dielectric layer of the side wall by increasing the compressive stress of the silicon oxide film. Specifically, the present invention is to replace the conventional SiN / SiO2 (N / O) dielectric layer structure of the through hole layer in the prior art with a SiN / SiO / SiN (N / O / N) dielectric layer structure, and after completing the through hole layer etching (Etch) to form through holes and grooves, fill in selective tungsten, and then perform plasma treatment on the upper SiN layer, including but not limited to Ar / H2 / N2 gas source; after the plasma treatment, the upper SiN layer on the surface generates a compressive stress, which enhances the adhesion between tungsten and the silicon oxide dielectric layer of the side wall, and can effectively prevent the infiltration of grinding liquid and cleaning liquid, thereby avoiding the problem of cobalt deficiency caused by the CMP grinding liquid corroding the cobalt in the lower layer (interconnection line layer) in the subsequent through hole layer during the chemical mechanical polishing (W CMP) manufacturing process.
[0027] See also Figure 1 , Figure 1 The flowchart of the method for manufacturing the metal wiring of the semiconductor device in the embodiment of the present invention is shown. In the embodiment of the present invention, the method for manufacturing the metal wiring of the semiconductor device specifically includes the following steps:
[0028] Step S1: providing a substrate including an interconnect layer structure, and forming a dielectric layer on the substrate, wherein the interconnect material in the interconnect layer structure includes metal cobalt, and the dielectric layer includes a contact hole etch stop layer, a silicon oxide layer SiO2, and a silicon nitride layer SiN grown sequentially on the substrate;
[0029] Step S2: performing a standard photolithography and etching process on the dielectric layer to form a patterned through-hole layer; wherein the through-holes in the through-hole layer penetrate the dielectric layer;
[0030] Step S3: depositing tungsten on the via layer by a selective tungsten deposition process to form a via tungsten plug in the via layer; wherein at least one of the via tungsten plugs is in contact with the interconnect layer structure;
[0031] Step S4: performing a plasma treatment process on the surface of the through-hole layer to generate compressive stress in the silicon nitride layer SiN to increase the squeezing force between the dielectric in the dielectric layer and the side wall of the through-hole tungsten plug;
[0032] Step S5: depositing a TiN adhesion layer and a metal tungsten layer in sequence to form a through-hole tungsten plug covering layer on the through-hole layer;
[0033] Step S6: performing a tungsten chemical mechanical planarization process on the through-hole tungsten plug capping layer to form a planarized through-hole layer.
[0034] Preferably, the gas source used in the plasma treatment process in step S4 includes argon Ar, hydrogen H2 or nitrogen N2; and the material of the contact hole etch stop layer is silicon nitride (SiN) or nitrogen-doped silicon carbide (NDC).
[0035] Further, the interconnection line layer structure is an interconnection line layer structure M0; and the through hole layer is a through hole layer V0.
[0036] The technical solution of the present invention is illustrated below by a specific embodiment.
[0037] Example 1
[0038] See also Figures 2 to 5 ,like Figure 2 As shown, a substrate (not shown) containing an interconnect layer structure 1 is provided, and the structure of the interconnect layer structure 1 is an S / D / G metal wiring structure, wherein the interconnect layer structure 1 includes Co metal interconnect material and dielectric material (for example, SiO2 as shown in the figure), and the device below the interconnect layer structure 1 is omitted and not shown.
[0039] In the embodiment of the present invention, a dielectric layer 2 is formed on a substrate 1, and the dielectric layer 2 includes, from bottom to top, a contact hole etch stop layer 21 (CESL), a silicon oxide layer (SiO2) 22, and a silicon nitride layer (SiN) 23. The contact hole etch stop layer 21 (CESL) Figure 3 , Figure 4 and Figure 4 The material of the silicon nitride layer 22 (shown in FIG. 1 ) may be silicon nitride (SiN) or nitrogen doped silicon carbide (NDC). The silicon nitride layer SiN serves as an etching stop layer for the silicon oxide layer 22 (SiO2).
[0040] That is to say, the dielectric layer 2 structure in the embodiment of the present invention replaces the SiN / SiO2 (N / O) dielectric layer structure of the through hole layer in the prior art with a SiN / SiO / SIN (N / O / N) dielectric layer structure.
[0041] like Figure 6 As shown in the figure, the result pattern after the dielectric layer is subjected to a standard photolithography and etching process, i.e., a patterned through-hole layer is formed; wherein the through-holes in the through-hole layer penetrate the dielectric layer, that is, the through-holes in the through-hole layer have been etched through the contact etch stop layer (CESL) and stopped on the surface of the interconnection line in the interconnection line layer structure.
[0042] like Figure 7As shown in the figure, tungsten is deposited on the via layer using a selective tungsten deposition process to form a via tungsten plug in the via layer; wherein at least one of the via tungsten plugs is in contact with the interconnect layer structure.
[0043] like Figure 8 and 9 As shown in the figure, the dielectric layer 2 includes a contact hole etching stop layer 21 (silicon nitride layer), a silicon oxide layer 22 and a silicon nitride layer 23 from bottom to top, and a plasma treatment process is performed on the surface of the through hole layer to generate compressive stress in the silicon nitride layer SiN to increase the squeezing force between the dielectric in the dielectric layer 2 and the side wall of the through hole tungsten plug.
[0044] like Fig.10 As shown in the figure, a TiN adhesion layer and a metal tungsten layer are deposited in sequence to form a through-hole tungsten plug covering layer on the through-hole layer.
[0045] like Fig.11 As shown, a tungsten chemical mechanical planarization process is performed on the via tungsten plug capping layer to form a planarized via layer.
[0046] Preferably, the dielectric material in the interconnect layer structure is silicon dioxide SiO2, and the polishing in step S6 stops on the silicon dioxide SiO2 surface of the interconnect layer structure according to the polishing ratio of the contact hole etching stop layer to the silicon dioxide SiO2.
[0047] In summary, the silicon nitride layer SIN layer deposited in the embodiment of the present invention serves as a sacrificial dielectric layer for subsequent W CMP. During W CMP polishing, the silicon nitride layer SIN is completely consumed and stops on the silicon oxide layer under the silicon nitride layer SIN. In this way, the in-plane uniformity after W CMP is optimized.
[0048] Specifically, since the polishing liquid and cleaning liquid used in the W CMP are currently mainly acidic, the acidity can easily penetrate into the lower layer and cause corrosion to the Co metal wire in the lower layer. Therefore, the present invention can achieve a significant effect of reducing Co missing defects for acidic polishing liquid and cleaning liquid.
[0049] The above-described embodiments are only preferred embodiments of the present invention, and the embodiments are not intended to limit the patent protection scope of the present invention. Therefore, any equivalent structural changes made using the description and drawings of the present invention should also be included in the protection scope of the present invention.
Claims
1. A method for manufacturing a metal connection of a semiconductor device, characterized in that: include: Step S1: providing a substrate including an interconnect layer structure, and forming a dielectric layer on the substrate, wherein the interconnect material in the interconnect layer structure includes metal cobalt, and the dielectric layer includes a contact hole etch stop layer, a silicon oxide layer SiO2, and a silicon nitride layer SiN grown sequentially on the substrate; Step S2: performing a standard photolithography and etching process on the dielectric layer to form a patterned through-hole layer; wherein the through-holes in the through-hole layer penetrate the dielectric layer; Step S3: depositing tungsten on the through-hole layer by a selective tungsten deposition process to form a through-hole tungsten plug in the through-hole layer; wherein the lower portion of the through-hole tungsten plug contacts the interconnection line of the interconnection line layer structure; and the upper portion of the through-hole tungsten plug is higher than the silicon nitride layer SiN in the dielectric layer; Step S4: performing a plasma treatment process on the surface of the through-hole layer to generate compressive stress in the silicon nitride layer SiN, so as to increase the squeezing force between the silicon nitride layer SiN and the side wall of the through-hole tungsten plug; Step S5: depositing a TiN adhesion layer and a metal tungsten layer in sequence to form a through-hole tungsten plug covering layer on the through-hole layer; Step S6: performing a tungsten chemical mechanical planarization process on the through-hole tungsten plug cover layer and the silicon nitride layer SiN to form a planarized through-hole layer; wherein the planarized through-hole layer stops at the upper surface of the silicon oxide layer SiO2 in the dielectric layer.
2. The method for manufacturing a metal wiring of a semiconductor device according to claim 1, characterized in that: The gas source used in the plasma treatment process in step S4 includes argon Ar, hydrogen H2 or nitrogen N2.
3. The method for manufacturing a metal wiring of a semiconductor device according to claim 1, characterized in that: The plasma treatment process is a plasma bias bombardment process.
4. The method for manufacturing a metal wiring of a semiconductor device according to claim 3, characterized in that: The plasma bias bombardment process is a heavy ion plasma bias bombardment process.
5. The method for manufacturing a metal wiring of a semiconductor device according to claim 1, characterized in that: The dielectric layer includes a flow-type chemical vapor deposition silicon oxide layer, and the step S4 further includes performing a water vapor annealing process on the flow-type chemical vapor deposition silicon oxide layer to further increase the compressive stress between the dielectric in the dielectric layer and the sidewall of the through-hole tungsten plug.
6. The method for manufacturing a metal wiring of a semiconductor device according to claim 1, characterized in that: The material of the contact hole etching stop layer is silicon nitride or nitrogen-doped silicon carbide.
7. The method for manufacturing a metal wiring of a semiconductor device according to claim 1, characterized in that: The polishing in step S6 stops on the surface of the silicon dioxide SiO2 of the interconnect layer structure according to the polishing ratio of the silicon nitride layer SiN to the silicon dioxide SiO2.
8. The method for manufacturing a metal wiring of a semiconductor device according to claim 1, characterized in that: At least one of the through-hole tungsten plugs contacts the metal cobalt interconnection line in the interconnection line layer structure.
Citation Information
Patent Citations
Etch stop layer and its forming method
CN101192533A
Preparation method of a conductive embolism and a semiconductor device with the conductive embolism
CN109256358A
Semiconductor device and manufacturing method thereof
KR1020100012207A