A method for processing lithium battery electrodes

By cutting and applying conductive adhesive, a single-sided coated pole piece is formed, which solves the problems of easily damaged pole pieces and inaccurate testing in the existing technology, and improves the accuracy and stability of lithium battery pole piece processing. .

CN113358428BActive Publication Date: 2024-10-01WANXIANG 123 CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110453421.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-26
Publication Date
2024-10-01
Estimated Expiration
2041-04-26

AI Technical Summary

Technical Problem

When the existing lithium battery pole piece processing methods are made into button batteries, the cycle stability is poor and the pole pieces are easily damaged. The double-sided coated pole pieces increase the impedance due to the non-electrochemically active surface, and the capacity test is inaccurate.

Method used

Use the cut pole piece to wash away the surface lithium salt in a solvent, apply conductive adhesive and roll it for solidification to form a single-sided coated pole piece to avoid scratch damage, and thinly apply conductive adhesive on the foil. The agent is used to adhere the pole piece to the current collector to reduce errors and improve test accuracy.

Benefits of technology

It effectively avoids scratching of pole pieces, reduces the risk of electrolyte penetration to increase additional capacity, improves test accuracy, and enhances cycle stability and capacity test accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113358428B_ABST
    Figure CN113358428B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium-ion battery failure analysis, and discloses a method for processing a lithium battery pole piece, comprising the following steps: (1) cutting the disassembled pole piece, then soaking the cut pole piece in a solvent to wash away the lithium salt on the surface, and laying the pole piece flat after drying; (2) coating a conductive adhesive on a current collector, and laying it flat after drying; (3) placing the current collector with the conductive adhesive in a closed space, attaching the pole piece obtained in step (1) to the surface of the conductive adhesive, and rolling and curing; (4) punching the cured pole piece into a disc, thereby obtaining a pole piece with a single-sided coating. The present invention uses a conductive adhesive with high conductivity and bonding strength to process the pole piece, which can reduce the time for pole piece processing and effectively avoid the pole piece from being scratched; prevent the electrolyte from penetrating to the other side of the pole piece to increase the extra capacity, and increase the test accuracy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery failure analysis, and in particular to a lithium battery pole piece processing method. Background Art

[0002] When a lithium battery fails, the process data of the battery itself is generally analyzed first, and the positive and negative electrodes are basically analyzed. These include charge and discharge curves, capacity performance, and AC impedance testing, which are all key tests after the battery is disassembled. When testing the capacity of the positive and negative electrodes, it is necessary to make a button battery. The positive and negative electrode plates are coated with materials on both sides. In the prior art, a scraper or cotton swab is used to scrape off one side when making a button battery to make a button battery.

[0003] The existing technical solutions have the following disadvantages:

[0004] (1) The button-type battery made by scraping off one side of the electrode has poor cycle stability and the electrode is easily damaged;

[0005] (2) Since the other side of the electrode with double-sided coating is basically non-electrochemically active, the impedance is increased and the capacity test is inaccurate. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a lithium battery pole piece processing method, which can effectively prevent the pole piece from being scratched; in addition, it can prevent the electrolyte from penetrating to the other side of the pole piece to increase additional capacity and increase test accuracy.

[0007] The specific technical solution of the present invention is: a lithium battery pole piece processing method, comprising the following steps:

[0008] (1) Cut the disassembled electrode pieces, soak the cut electrode pieces in a solvent to wash away the lithium salt on the surface, and lay the dried electrode pieces flat;

[0009] (2) Applying a conductive adhesive on the current collector and laying it flat after drying;

[0010] (3) placing the current collector with the conductive adhesive in a closed space, attaching the electrode obtained in step (1) to the surface of the conductive adhesive, and rolling and curing;

[0011] (4) Punching the solidified electrode into a disc to obtain a single-sided coated electrode.

[0012] The present invention proposes a method of coating a thin layer of conductive adhesive on a foil, and then bonding the electrode to the foil current collector, thereby turning a double-layer coated electrode into a single layer for making button batteries. The electrode processing method of the present invention can reduce the time of scraping a double-sided electrode into a single-sided coated electrode, effectively avoiding the electrode from being scratched. It can also reduce the error of assembling batteries using double-sided electrode pieces, prevent the electrolyte from penetrating to the other side of the electrode piece to increase the extra capacity, and increase the test accuracy.

[0013] Preferably, the shape of the pole piece after cutting in step (1) is one of a circle and a quadrilateral.

[0014] Preferably, the area of ​​the pole piece after cutting in step (1) is larger than the area of ​​the disc in step (4), so as to facilitate the subsequent stamping operation.

[0015] Preferably, the conductive adhesive in step (2) is a pressure-sensitive acrylic conductive adhesive, and the conductive adhesive emulsion is prepared by mixing 70 to 90 parts by weight of acrylic resin, 6 to 10 parts of graphene conductive agent, 3 to 15 parts of rosin resin and 1 to 5 parts of curing agent.

[0016] Preferably, the acrylic resin is epoxy acrylic resin, the graphene conductive agent is an ionic liquid-graphene composite material, and the curing agent is triethylenetetramine.

[0017] Preferably, the preparation method of the ionic liquid-graphene composite material is as follows: 70-90 parts of ionic liquid and 10-30 parts of graphene by weight; dissolving the ionic liquid in a solution, adding graphene and mixing, stirring for 5-12 hours, filtering and drying.

[0018] The present invention firstly uses a conductive adhesive prepared from conventional graphene sheet conductive powder to conduct experiments, and finds that when the coating thickness decreases, the conductivity of the conductive adhesive decreases and the test accuracy decreases. Therefore, the conductive adhesive is improved, and an ionic liquid is loaded on the graphene to prepare a composite material for use as a conductive agent. Since the added ionic liquid is a room temperature molten salt completely composed of anions and cations, it has excellent conductive properties. When loaded inside or on a graphene sheet, the gap between the graphene sheets can be expanded and the conductivity of the graphene can be improved. At the same time, during the charging and discharging process of the battery, the anions and cations of the ionic liquid move in a direction under the action of the current, which greatly improves the conductivity of the conductive adhesive. The ionic liquid has high viscosity, thereby effectively improving the conductive properties and viscosity of the conductive adhesive.

[0019] Preferably, the coating thickness in step (2) is 10 to 50 μm.

[0020] In the present invention, the influence of coating thickness on test accuracy is studied by setting different coating thicknesses. The experimental results show that the smaller the thickness of the coating material, the higher the test accuracy.

[0021] Preferably, the current collector is made of Cu foil or Al foil according to the positive and negative polarities of the electrode sheet, and the thickness of the current collector is 30 to 50 μm.

[0022] Preferably, the diameter of the disc in step (4) is 12-14 mm, and the obtained pole piece is a single-sided coated pole piece, which can almost completely seal the back material and will not curl like a single-sided coated pole piece.

[0023] Preferably, the lithium battery pole piece processing method of the present invention is applied to pole piece failure processing, fresh pole piece processing and SLP battery assembly.

[0024] Further preferably, the lithium battery pole piece processing method of the present invention is applied to pole piece failure processing.

[0025] Compared with the prior art, the beneficial effects of the present invention are:

[0026] (1) The present invention discloses a method of coating a thin layer of acrylic conductive adhesive on a foil material and then bonding a pole piece to a foil material current collector; the time for scraping a double-sided pole piece into a single-sided coated pole piece can be reduced, and the pole piece can be effectively prevented from being scratched;

[0027] (2) It can prevent the electrolyte from penetrating to the other side of the electrode to increase the additional capacity, reduce the error of assembling batteries using double-sided electrodes, and increase the test accuracy. The smaller the coating thickness, the higher the test accuracy.

[0028] (3) The present invention synthesizes a highly conductive and highly viscous conductive adhesive by improving the preparation process of the conductive adhesive. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a graph showing the percentage of additional charge and discharge capacity of the pole piece in the present invention;

[0030] Figure 2 It is a charge and discharge curve diagram of the button battery in the present invention. DETAILED DESCRIPTION

[0031] The present invention is further described below in conjunction with the examples. The raw materials and equipment involved in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art; and the reagents used in the present invention are all lithium battery grade.

[0032] Embodiment 1:

[0033] A lithium battery electrode processing method comprises the following steps:

[0034] (1) Cut the disassembled electrode into a rectangle, then soak the cut electrode in DMC solvent to wash away the lithium salt on the surface, dry it and lay it flat on a glass plate;

[0035] (2) The automatic scraper was adjusted to a coating thickness of 10 μm and a coating speed of 10 mm / s. An acrylic conductive adhesive (mixed by weight of 85 parts of epoxy acrylic resin, 7 parts of [TETA][Cl]-graphene, 7 parts of rosin resin and 1 part of triethylenetetramine curing agent; the preparation method of [TETA][Cl]-graphene is as follows: by weight of 85 parts of [TETA][Cl] ionic liquid and 15 parts of graphene sheet conductive powder; the ionic liquid was dissolved in an ethanol solution, and the graphene was added and mixed, stirred for 8 h, and the [TETA][Cl]-graphene composite material was obtained by rotary evaporation and vacuum drying for 12 h.) was coated on an Al foil with a thickness of 30 μm. The baking temperature was controlled at 50°C and gradually increased to 100°C. After baking for 10 min, it was spread on a glass plate.

[0036] (3) placing the Al foil with the conductive adhesive in a glove box, attaching the electrode sheet after drying in step (1) to the adhesive, and rolling it with a roller for several times, waiting for solidification, to ensure that the electrode sheet and the current collector are firmly adhered;

[0037] (4) Punching the solidified electrode into a disc with a diameter of 12 mm using a punching die, thereby obtaining a single-sided coated electrode (represented by CS1);

[0038] The above-mentioned electrode pieces were used to assemble 2025 button batteries, and the charge and discharge tests were performed at a voltage of 4.3V using a current of 0.1C and 0.29mA.

[0039] Embodiment 2:

[0040] A lithium battery electrode processing method comprises the following steps:

[0041] (1) Cut the disassembled electrode into a rectangle, then soak the cut electrode in DMC solvent to wash away the lithium salt on the surface, dry it and lay it flat on a glass plate;

[0042] (2) The automatic scraper was adjusted to a coating thickness of 15 μm and a coating speed of 10 mm / s. An acrylic conductive adhesive (mixed by weight of 85 parts of epoxy acrylic resin, 7 parts of [TETA][Cl]-graphene, 7 parts of rosin resin and 1 part of triethylenetetramine curing agent; the preparation method of [TETA][Cl]-graphene is as follows: by weight of 85 parts of [TETA][Cl] ionic liquid and 15 parts of graphene sheet conductive powder; the ionic liquid was dissolved in an ethanol solution, and the graphene was added and mixed, stirred for 8 h, and the [TETA][Cl]-graphene composite material was obtained by rotary evaporation and vacuum drying for 12 h.) was coated on an Al foil with a thickness of 30 μm. The baking temperature was controlled at 50°C and gradually increased to 100°C. After baking for 10 min, it was spread on a glass plate.

[0043] (3) placing the Al foil with the conductive adhesive in a glove box, attaching the electrode sheet after drying in step (1) to the adhesive, and rolling it with a roller for several times, waiting for solidification, to ensure that the electrode sheet and the current collector are firmly adhered;

[0044] (4) Punching the solidified electrode into a disc with a diameter of 12 mm using a punching die, thereby obtaining a single-sided coated electrode (represented by CS2);

[0045] The above-mentioned electrode pieces were used to assemble 2025 button batteries, and the charge and discharge tests were performed at a voltage of 4.3V using a current of 0.1C and 0.29mA.

[0046] Embodiment 3:

[0047] A lithium battery electrode processing method comprises the following steps:

[0048] (1) Cut the disassembled electrode into a rectangle, then soak the cut electrode in DMC solvent to wash away the lithium salt on the surface, dry it and lay it flat on a glass plate;

[0049] (2) The automatic scraper was adjusted to a coating thickness of 50 μm and a coating speed of 10 mm / s. An acrylic conductive adhesive (mixed by weight of 85 parts of epoxy acrylic resin, 7 parts of [TETA][Cl]-graphene, 7 parts of rosin resin and 1 part of triethylenetetramine curing agent; the preparation method of [TETA][Cl]-graphene is as follows: by weight of 85 parts of [TETA][Cl] ionic liquid and 15 parts of graphene sheet conductive powder; the ionic liquid was dissolved in an ethanol solution, and the graphene was added and mixed, stirred for 8 h, and the [TETA][Cl]-graphene composite material was obtained by rotary evaporation and vacuum drying for 12 h.) was coated on an Al foil with a thickness of 30 μm. The baking temperature was controlled at 50 °C and gradually increased to 100 °C. After baking for 10 min, it was spread on a glass plate.

[0050] (3) placing the Al foil with the conductive adhesive in a glove box, attaching the electrode sheet after drying in step (1) to the adhesive, and rolling it with a roller for several times, waiting for solidification, to ensure that the electrode sheet and the current collector are firmly adhered;

[0051] (4) Punching the solidified electrode into a disc with a diameter of 12 mm using a punching die, thereby obtaining a single-sided coated electrode (represented by CS3);

[0052] The above-mentioned electrode pieces were used to assemble 2025 button batteries, and the charge and discharge tests were performed at a voltage of 4.3V using a current of 0.1C and 0.29mA.

[0053] Embodiment 4:

[0054] A lithium battery electrode processing method comprises the following steps:

[0055] (1) Cut the disassembled electrode into a rectangle, then soak the cut electrode in DMC solvent to wash away the lithium salt on the surface, dry it and lay it flat on a glass plate;

[0056] (2) Adjust the automatic scraper to a coating thickness of 10 μm and a coating speed of 10 mm / s, and apply an acrylic conductive adhesive (mixed by weight of 70 parts of epoxy acrylic resin, 10 parts of [TETA][Cl]-graphene, 15 parts of rosin resin and 5 parts of triethylenetetramine curing agent; the preparation method of [TETA][Cl]-graphene is as follows: by weight of 70 parts of [TETA][Cl] ionic liquid and 30 parts of graphene sheet conductive powder; the ionic liquid is dissolved in an ethanol solution, the graphene is added and mixed, stirred for 12 h, and the [TETA][Cl]-graphene composite material is obtained by rotary evaporation and vacuum drying for 12 h.) on an Al foil with a thickness of 50 μm, and the baking temperature is controlled at 50 °C and gradually increased to 100 °C, and then baked for 10 min and spread on a glass plate;

[0057] (3) placing the Al foil with the conductive adhesive in a glove box, attaching the electrode sheet after drying in step (1) to the adhesive, and rolling it with a roller for several times, waiting for solidification, to ensure that the electrode sheet and the current collector are firmly adhered;

[0058] (4) Punching the solidified electrode into a disc with a diameter of 13 mm using a punching die, thereby obtaining a single-sided coated electrode (represented by CS4);

[0059] The above-mentioned electrode pieces were used to assemble 2025 button batteries, and the charge and discharge tests were performed at a voltage of 4.3V using a current of 0.1C and 0.29mA.

[0060] Embodiment 5:

[0061] A lithium battery electrode processing method comprises the following steps:

[0062] (1) Cut the disassembled electrode into a rectangle, then soak the cut electrode in DMC solvent to wash away the lithium salt on the surface, dry it and lay it flat on a glass plate;

[0063] (2) Adjust the automatic scraper to a coating thickness of 10 μm and a coating speed of 10 mm / s, and apply an acrylic conductive adhesive (mixed by weight of 90 parts of epoxy acrylic resin, 6 parts of [TETA][Cl]-graphene, 3 parts of rosin resin and 1 part of triethylenetetramine curing agent; the preparation method of [TETA][Cl]-graphene is as follows: by weight of 90 parts of [TETA][Cl] ionic liquid and 10 parts of graphene sheet conductive powder; the ionic liquid is dissolved in an ethanol solution, and the graphene is added and mixed, stirred for 5 h, and the [TETA][Cl]-graphene composite material is obtained by rotary evaporation and vacuum drying for 12 h.) on an Al foil with a thickness of 40 μm, and the baking temperature is controlled at 50°C and gradually increased to 100°C, and then baked for 10 min and spread on a glass plate;

[0064] (3) placing the Al foil with the conductive adhesive in a glove box, attaching the electrode sheet after drying in step (1) to the adhesive, and rolling it with a roller for several times, waiting for solidification, to ensure that the electrode sheet and the current collector are firmly adhered;

[0065] (4) Punching the cured electrode into a disc with a diameter of 14 mm using a punching die to obtain a single-sided coated electrode; assembling a 2025 button battery with the above electrode, and performing a charge and discharge test at a voltage of 4.3 V and a current of 0.1 C and 0.29 mA.

[0066] Embodiment 6:

[0067] A lithium battery electrode processing method comprises the following steps:

[0068] (1) Cut the disassembled electrode into a rectangle, then soak the cut electrode in DMC solvent to wash away the lithium salt on the surface, dry it and lay it flat on a glass plate;

[0069] (2) Adjust the automatic scraper to a coating thickness of 10 μm and a coating speed of 10 mm / s, and apply an acrylic conductive adhesive (mixed by weight of 85 parts of epoxy acrylic resin, 7 parts of graphene sheet conductive powder, 7 parts of rosin resin, and 1 part of triethylenetetramine curing agent) on an Al foil with a thickness of 30 μm. The baking temperature is controlled at 50° C. and gradually increased to 100° C. After baking for 10 minutes, spread it on a glass plate;

[0070] (3) placing the Al foil with the conductive adhesive in a glove box, attaching the electrode sheet after drying in step (1) to the adhesive, and rolling it with a roller for several times, waiting for solidification, to ensure that the electrode sheet and the current collector are firmly adhered;

[0071] (4) Punching the solidified electrode into a disc with a diameter of 12 mm using a punching die, thereby obtaining a single-sided coated electrode (represented by CS1);

[0072] The above-mentioned electrode pieces were used to assemble 2025 button batteries, and the charge and discharge tests were performed at a voltage of 4.3V using a current of 0.1C and 0.29mA.

[0073] Comparative Example 1:

[0074] The 2025 button cell was assembled with a single-sided electrode (indicated by SS) without any damage after scraping, and the charge and discharge test was performed at 4.3V using 0.1C and 0.29mA current.

[0075] Comparative Example 2:

[0076] The 2025 button cell was assembled with unscratched, double-sided coated pole pieces (indicated by DS), and the charge and discharge test was performed at 4.3V using 0.1C and 0.29mA current.

[0077] Data analysis:

[0078] The surface resistance and viscosity of the conductive adhesives prepared in Example 1 and Example 6 were measured using a surface resistance tester and a bonding strength tester, respectively. The results are as follows:

[0079] Surface resistance / Ω Bond strength / MPa Example 1 0.16 0.69 Example 6 0.32 0.51

[0080] As can be seen from the table, the surface resistance and bonding strength of the conductive adhesive with added [TETA][Cl]-graphene conductive agent are higher than those of the conductive adhesive with added graphene sheet conductive powder. This is because the ionic liquid is loaded onto graphene to make a composite material used as a conductive agent. Since the added ionic liquid is a room temperature molten salt composed entirely of anions and cations, it has excellent conductive properties. When loaded into or on the graphene sheet, it can expand the gap between the graphene sheets and improve the conductivity of the graphene. At the same time, during the charging and discharging process of the battery, the anions and cations of the ionic liquid move in a directional manner under the action of the current, which greatly improves the conductivity of the conductive adhesive. The ionic liquid has high viscosity, thereby effectively improving the conductive properties and viscosity of the conductive adhesive.

[0081] like Figure 1As shown, ΔC=(Cd or Ccs-Cs) / Cs represents the additional charge and discharge capacity deviation of the double-sided electrode, where Cd is the double-sided half-cell capacity, Cs is the single-sided half-cell capacity, and Ccs represents the half-cell capacity of the single-sided conductive adhesive foil. Among them, ΔCsc1 is the smallest, approaching 0, ΔCsc2 is slightly smaller, ΔCd>ΔCsc3>ΔCsc4>ΔCsc>ΔCsc1, indicating that the double-sided electrode is the least representative of the single-sided electrode for capacity testing, and the negative active material will affect the capacity; when using a single-sided foil, the capacity test deviation is the smallest when the conductive adhesive coating is 10um thick and the foil thickness is 30um. From the data in the figure, it can be concluded that when the conductive adhesive coating is 10-15um, it has little effect on the overall capacity, the test deviation is less than 1%, and the test accuracy is high. When the conductive adhesive coating exceeds 15um and increases to 50um, the overall capacity will be affected more, and the test deviation is close to 10%. When the conductive adhesive coating thickness is 10um and the conductive foil thickness is 50um, it will also have a certain impact, but compared with the conductive adhesive coating thickness, it is relatively small. This shows that when controlling the thickness of the conductive adhesive coating, it is also necessary to control the thickness of the conductive foil. When selecting a suitable foil, the thinner the conductive adhesive coating thickness, the smaller the corresponding test deviation, and the more accurate this method is.

[0082] pass Figure 1 By comparison, it was found that the single-sided coating error was smaller than the double-sided coating. At the same time, when the conductive adhesive coating was 10um thick and the foil thickness was 30um, the capacity test deviation was the smallest. Therefore, the pole pieces prepared in Example 1 and Comparative Example 1 were subjected to charge and discharge tests.

[0083] like Figure 2 As shown in the figure, from the charge and discharge curves, the half-cell charge and discharge curve of the single-sided electrode is almost consistent with the curve of the single-sided foil (coating 10um), with only a slight deviation, which is almost less than 1% and falls within the allowable deviation range.

[0084] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A lithium battery pole piece processing method, characterized in that: Includes steps: (1) Cut the disassembled electrode, soak it in a solvent to wash away the surface lithium salt, and lay it flat after drying; (2) The conductive adhesive is coated on the current collector with a coating thickness of 10-50 μm, and then spread flat after drying; the conductive adhesive is mixed by weight of 70-90 parts of acrylic resin, 6-10 parts of graphene conductive agent ionic liquid-graphene composite material, 3-15 parts of rosin resin and 1-5 parts of curing agent; the preparation method of ionic liquid-graphene composite material is as follows: by weight, 70-90 parts of ionic liquid are dissolved in ethanol solution, 10-30 parts of graphene are added and mixed, stirred for 5-12 hours, filtered and dried; ionic liquid is a room temperature molten salt composed entirely of anions and cations; (3) placing the current collector with the conductive adhesive in a closed space, attaching the electrode from step (1) to the surface of the conductive adhesive, and rolling and curing; (4) The cured electrode is punched into a disc to obtain a single-sided coated electrode.

2. A lithium battery electrode processing method according to claim 1, characterized in that: The shape of the pole piece after cutting in the step (1) is one of a circle and a quadrilateral.

3. A lithium battery electrode processing method according to claim 1, characterized in that: The area of ​​the pole piece after cutting in step (1) is larger than the area of ​​the disc in step (4).

4. A lithium battery electrode processing method according to claim 1, characterized in that: The conductive adhesive is a pressure-sensitive acrylic conductive adhesive.

5. A lithium battery electrode processing method as claimed in claim 4, characterized in that: The acrylic resin is epoxy acrylic resin.

6. A lithium battery electrode processing method as claimed in claim 5, characterized in that: The curing agent uses triethylenetetramine.

7. A lithium battery electrode processing method according to claim 1, characterized in that: The current collector is selected from Al foil and Cu foil according to the positive and negative polarities of the electrode.

8. A lithium battery electrode processing method as claimed in claim 7, characterized in that: The thickness of the current collector is 30-50 μm.

9. A lithium battery electrode processing method as claimed in claim 1, characterized in that: The diameter of the disc in step (4) is 12-14 mm.

10. A lithium battery pole piece processing method according to any one of claims 1 to 9, characterized in that: The lithium battery pole piece processing method of the present invention is applied to pole piece failure processing, fresh pole piece processing and SLP battery assembly.