Preparation method for synthesizing 13X molecular sieve with special morphology under assistance of silicon quantum dots
A technology of silicon quantum dots and molecular sieves is applied in the field of preparation of 13X molecular sieves with special morphology assisted by silicon quantum dots, which can solve the problems of insufficient growth, insufficient adsorption performance, and insufficient specific surface area.
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2021-10-08
Smart Images

Figure 1 
Figure 2 
Figure 3
Abstract
Description
technical field
[0001] The invention belongs to the field of adsorption and separation materials, and in particular relates to a method for preparing 13X molecular sieves with special morphology assisted by silicon quantum dots. Background technique
[0002] Over the years, industrial development has continued to rely on fossil fuels, whose consumption leads to CO 2 Emissions are increasing year by year, and its greenhouse effect triggers global warming and destroys the ecological balance. People gradually realize that effective control of CO 2 Pollution is crucial to the development of human society. At present, the industry mainly uses the aqueous solution of amine compounds for CO 2 For neutralization treatment, the process usually requires high temperature operations above 100°C to develop low-energy and high-efficiency CO 2 Adsorbent materials and technologies have become a target of research and industry. Currently, available for CO 2 The adsorbents for gas captur...
Examples
Embodiment 1
[0034] Embodiment 1: The preparation method of silicon quantum dot-assisted synthesis of special morphology 13X molecular sieve in this embodiment is carried out according to the following steps:
[0035] Step 1, using sodium ascorbate (SA) as a reducing agent, and a silane coupling agent as a silicon source, adopting a one-step hydrothermal method to synthesize silicon quantum dots to obtain a silicon quantum dot solution;
[0036] Step 2. Mix 10.0g of 40% (mass) silica sol, 2.5g of sodium hydroxide powder, 2.0g of silicon quantum dot solution, and 33g of deionized water in a beaker, and heat and stir at 500r / min in a water bath at 80°C After 10 minutes, a clear and transparent sodium silicate gel solution was obtained, and stirred at room temperature at a speed of 500 r / min for 30 minutes to obtain a silicon source solution.
[0037] Step 3: Mix 1.5 g of sodium hydroxide powder with a mass concentration of 15%, 2.9 g of sodium aluminate solution, and 16.5 g of deionized wate...
Embodiment 2
[0044] Embodiment 2: The preparation method of silicon quantum dot-assisted synthesis of special morphology 13X molecular sieve in this embodiment is carried out according to the following steps:
[0045] Step 1. Using sodium ascorbate (SA) as a reducing agent and a silane coupling agent as a silicon source, a one-step hydrothermal method is used to synthesize silicon quantum dots to obtain a silicon quantum dot solution. Step 1 prepares silicon quantum dot solution steps and parameters and examples 1 same;
[0046] Step 2. Mix 10.0g of silica sol (40%), 2.5g of sodium hydroxide powder, and 33g of deionized water in a beaker, heat and stir in a water bath at 80°C at a speed of 500r / min for 10min to obtain clear and transparent sodium silicate The gel solution was stirred at room temperature for 30 min at a speed of 500 r / min; a silicon source solution was obtained.
[0047] Step 3, mix 1.5g of sodium hydroxide powder, 2.9g of sodium aluminate solution, 16.5g of deionized wate...
Embodiment 3
[0050] Embodiment 3: The preparation method of silicon quantum dot-assisted synthesis of special morphology 13X molecular sieve in this embodiment is carried out according to the following steps:
[0051] Step 1. Using sodium ascorbate (SA) as a reducing agent and a silane coupling agent as a silicon source, a one-step hydrothermal method is used to synthesize silicon quantum dots to obtain a silicon quantum dot solution. Step 1 prepares silicon quantum dot solution steps and parameters and examples 1 is the same.
[0052] Step 2, silicon source: mix 10.0g of silica sol (40%), 2.5g of sodium hydroxide powder, and 33g of deionized water in a beaker, heat and stir in a water bath at 80°C for 10 minutes (speed 500r / min) to dissolve, and obtain clarification Transparent sodium silicate gel solution, stirred at room temperature (rotating speed 500r / min) for 30min.
[0053] Step 3, aluminum source: mix 1.5g of sodium hydroxide powder, 2.9g of sodium aluminate solution, and 16.5g of...