A device and method for detecting dynamic properties of carbon graphite material

By designing a detection device for detecting carbon graphite materials under high-speed and light load conditions, the problem that the prior art cannot detect the friction and wear performance of carbon graphite materials at high speed and low pressure is solved, and the simulation practical application environment is realized The dynamic performance detection reduces research costs and provides characteristic data to support the selection of carbon graphite materials.

CN113588474BActive Publication Date: 2024-11-26ZIGONG DONGXIN CARBON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110859705.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-28
Publication Date
2024-11-26
Estimated Expiration
2041-07-28

AI Technical Summary

Technical Problem

Existing test instruments are unable to detect the friction and wear properties of carbon graphite materials at high speed and low pressure, resulting in increased research risks and costs.

Method used

A detection device including a base, rotating shaft, friction ring, pressure device and speed control motor is designed, which can detect the dynamic performance of carbon graphite materials in high-speed and light-load states, and monitor the speed and torque through the speed control motor and torque sensor. , combined with heating resistance and temperature measurement thermocouple, simulate the actual application environment for detection.

Benefits of technology

The dynamic performance parameters of carbon graphite materials were detected under high speed 30~144m/s, light load 10~410KPa, room temperature ~550℃, which reduced the research cost and provided characteristic data for selection, supporting the engine fulcrum carbon graphite Materials research.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113588474B_ABST
    Figure CN113588474B_ABST
Patent Text Reader

Abstract

The present invention discloses a device and method for detecting the dynamic performance of carbon graphite materials. The device comprises a base, a rotating shaft, a friction ring, a pressure device and a speed regulating motor arranged on the base. The rotating shaft is connected to the output shaft of the speed regulating motor. The friction ring is detachably fixedly sleeved on the rotating shaft to rotate synchronously with the rotating shaft. A sample fixture box is arranged on the outer circumference of the friction ring for placing the sample. The sample fixture box is located on the radial diameter of the friction ring and has a through hole for the sample part to pass through. There is a gap between the through hole end of the sample fixture box and the circumferential surface of the friction ring, so that the sample part passes through the through hole of the sample fixture box and contacts the circumferential surface of the friction ring. The pressure device is used to apply pressure to the sample. The device can detect the dynamic performance of carbon graphite materials under high speed and light load (low pressure) conditions, which is conducive to reducing research risks and costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aviation technology, and in particular relates to a device and a method for detecting the dynamic performance of a carbon graphite material. Background Art

[0002] Carbon graphite materials have an irreplaceable position in the fields of aviation, aerospace, ships, nuclear industry, photovoltaics, semiconductors, wind power and new energy vehicles due to their excellent chemical stability, high thermal conductivity, self-lubrication, high temperature resistance, significant red hardness, light weight and high efficiency, low expansion coefficient and machinability. In particular, they are the preferred material for sealing devices such as end face seals, circumferential seals, expansion ring seals and floating ring seals.

[0003] Aircraft engines are engines that provide aircraft with the power they need to fly. As the heart of an aircraft, they directly affect the performance and reliability of the aircraft. Aircraft engines operate under extremely harsh conditions such as high temperature (up to 550-600°C), pressure (up to 410KPa) and high speed (up to 144m / s), and the sealing ring has a vital impact on the engine. If the carbon graphite material is not properly selected and cannot meet the requirements of the application environment, it is very easy to leak. The engine will increase fuel consumption due to leakage, reduce sealing pressure, seriously reduce engine performance, and even cause major safety accidents. The friction pair materials in the engine are usually: 40CrNiMoA chrome plating, 40Cr2MoV chrome plating and 50Mn chrome plating.

[0004] Existing test instruments can only detect the dynamic friction and wear performance of carbon graphite materials at low speed (less than 10m / s), such as the UMT-2 micro-friction and wear tester, UMT-3 controlled environment friction and wear instrument and MR-H5II high-speed ring block wear tester of the National Key Laboratory of Tribology of Tsinghua University, whose temperature, pressure and linear speed are adjustable, and whose spindle speed ranges are 0.001-5000r / min, 0.001-5000r / min and 10-3500r / min respectively. It is impossible to detect the friction and wear performance of carbon graphite materials at high speed and low pressure. After assembling a set of sealing devices for carbon graphite materials tested at low speed, it is undoubtedly to increase the research risk and cost.

[0005] Therefore, providing a device that can detect the dynamic performance of carbon graphite materials under high speed and light load (low pressure) conditions is a technical problem that those skilled in the art urgently need to solve. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a device and method for detecting the dynamic properties of carbon graphite materials. The device can detect the dynamic properties of carbon graphite under high speed and light load (low pressure) conditions, which is conducive to reducing research risks and costs.

[0007] The technical solution of the present invention is achieved in this way:

[0008] A device for detecting the dynamic performance of carbon graphite material comprises a base, a rotating shaft, a friction ring, a pressure device and a speed regulating motor arranged on the base, wherein the rotating shaft is connected to the output shaft of the speed regulating motor, the friction ring is detachably fixedly sleeved on the rotating shaft to rotate synchronously with the rotating shaft, a sample fixture box is arranged on the outer circumference of the friction ring for placing the sample, the sample fixture box is located on the radial diameter of the friction ring and has a through hole for the sample part to pass through, and a gap is formed between the through hole end of the sample fixture box and the circumferential surface of the friction ring, so that the sample part passes through the through hole of the sample fixture box and contacts the circumferential surface of the friction ring; the pressure device is used to apply pressure to the sample.

[0009] Furthermore, the sample fixture box is arranged on the outer circumference of the friction ring through a support frame, and the support frame is fixed on the base. The support frame includes two vertically arranged end plates and a plurality of support rods arranged between the two end plates. The two end plates are fixed side by side on the base, each support rod is arranged horizontally and the two ends of each support rod are respectively fixed to the edges of the two end plates, all support rods are evenly distributed along the circumference of the end plates, and the centers of the two end plates are provided with through holes for the rotating shaft to pass through; the sample fixture box is fixed on the support rods, and bearing seats are respectively provided on the bases outside the two end plates for supporting the rotating shaft.

[0010] Furthermore, the friction rings include a plurality of spiral friction rings and a plurality of smooth friction rings, and all the friction rings are arranged at intervals.

[0011] Furthermore, the sample fixture box can be movably fixed on the support rod, so as to facilitate the selection of the corresponding friction ring to detect the dynamic performance of the sample.

[0012] Furthermore, a torque sensor is provided between the rotating shaft and the output shaft of the speed regulating motor. The torque sensor is connected to the rotating shaft and the output shaft of the speed regulating motor through two couplings. One end of the two couplings is respectively connected to the two ends of the torque sensor, and the other end is respectively connected to one end of the rotating shaft or the output shaft of the speed regulating motor. The torque sensor is connected to the control unit to monitor the torque and transmit it to the control unit to facilitate the detection of the friction coefficient of the sample.

[0013] Furthermore, a speed sensor is provided on the speed regulating motor, and the speed sensor is connected to the control unit to monitor the speed of the speed regulating motor and transmit the speed to the control unit.

[0014] Furthermore, the sample holder box is provided with a heating resistor around it, so as to heat the sample placed in the sample holder box.

[0015] Furthermore, a friction ring machine handle is provided at the other end of the rotating shaft to facilitate manual detection of the rotating speed.

[0016] A method for detecting the dynamic properties of carbon graphite materials (I), using the above-mentioned device to detect the dynamic properties of the sample, specifically comprising the following steps:

[0017] S1: Processing samples: Process the carbon graphite blank into samples, then use ultrasonic cleaning for 10 to 30 minutes, and then place it in a vacuum drying oven for 8 to 24 hours for standby use; one end of the sample has a convex portion passing through the through hole of the sample fixture box, and a pressure hole and a temperature measuring hole are opened at the other end of the sample, the pressure hole is set in the middle, and the temperature measuring hole is eccentrically set and extends obliquely to the convex portion, which is used to detect the temperature change of the sample;

[0018] S2: After the sample is loaded into the sample fixture box, the convex surface of the sample is in contact with the friction ring, a temperature measuring thermocouple is inserted into the temperature measuring hole, and a pressure device is inserted into the pressure hole;

[0019] S3: After checking that the device and control system are normal, start the device, apply radial pressure to the sample within 30-410KPa, run-in the sample and the friction ring, and when the running-in area reaches more than 95%, close the device, remove the sample, and use the measuring system consisting of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare and measure the original height of the initial running-in sample, and record it;

[0020] S4: Put the sample taken out in step S3 into the sample fixture box again, set the circumferential speed of the device to 10-144 m / s and keep it constant, apply radial pressure to the sample, observe the sample temperature and friction coefficient in real time, record them every 30 minutes, and after running for 2 hours, take out the sample, compare the measurement height and calculate the wear amount using the measuring system consisting of the detection platform, standard gauge block, micrometer bracket and micrometer;

[0021] S5: Place the sample taken out in step S4 into a temperature-controlled sample fixture box, keep the circumferential linear speed constant, increase the pressure step by step by 10-30 KPa, observe the sample temperature and friction coefficient in real time, record once every 30 minutes, and after running for 2 hours, take out the sample, and use the measuring system consisting of the detection platform, standard gauge block, dial gauge bracket, and dial gauge to compare the measurement height and calculate the wear amount;

[0022] S6: Repeat step S5 until the characterization of the limit PV value appears, remove the sample, and thus obtain the dynamic performance parameters of the sample under different working conditions.

[0023] A method for detecting the dynamic properties of carbon stone material graphite (II), using the above-mentioned device to detect the dynamic properties of the sample, specifically comprising the following steps:

[0024] S1: Processing samples: Process the carbon graphite blank into samples, then use ultrasonic cleaning for 10 to 30 minutes, and then place it in a vacuum drying oven for 8 to 24 hours for standby use; one end of the sample has a convex portion passing through the through hole of the sample fixture box, and a pressure hole and a temperature measuring hole are opened at the other end of the sample, the pressure hole is set in the middle, and the temperature measuring hole is eccentrically set and extends obliquely to the convex portion, which is used to detect the temperature change of the sample;

[0025] S2: After the sample is loaded into the sample fixture box, the convex surface of the sample is in contact with the friction ring, a temperature measuring thermocouple is inserted into the temperature measuring hole, and a pressure device is inserted into the pressure hole;

[0026] S3: After checking that the device and control system are normal, start the device, apply radial pressure to the sample within 30-410KPa, run-in the sample and the friction ring, and when the running-in area reaches more than 95%, close the device, remove the sample, and use the measuring system consisting of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare and measure the original height of the initial running-in sample, and record it;

[0027] S4: Put the sample taken out in step S3 into the sample fixture box again, set the pressure of the device to 10-410KPa and keep constant pressure, and maintain a certain linear speed, observe the sample temperature and friction coefficient in real time, record once every 30 minutes, and after running for 2 hours, take out the sample, and use the measuring system composed of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare the measurement height and calculate the wear amount;

[0028] S5: Place the sample taken out in step S4 into a temperature-controlled sample fixture box, keep the pressure constant, increase the linear speed step by step by 10 m / s, observe the sample temperature and friction coefficient in real time, record them every 30 minutes, and after running for 2 hours, remove the sample, and use a measuring system consisting of a detection platform, a standard gauge block, a dial gauge bracket, and a dial gauge to compare the measurement height and calculate the wear amount;

[0029] S6: Repeat step S5 until the characterization of the limit PV value appears, remove the sample, and thus obtain the dynamic performance parameters of the sample under different working conditions.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The present invention evaluates the dynamic performance of carbon graphite sealing materials by testing the PV value obtained from high linear speed V: 10-144 m / s, light load (low pressure P: 30-410 KPa) and friction surface temperature T: room temperature-550°C, thereby providing characteristic data for the selection of engine fulcrum carbon graphite materials and promoting the research of engine fulcrum carbon graphite materials.

[0032] 2. The device is easy to operate and can study the dynamic performance parameters of carbon graphite materials under the conditions of high speed 30-144m / s, light load (low pressure) 10-410KPa, and room temperature-550℃, which is conducive to selecting carbon graphite materials with suitable performance according to the actual application environment, thereby helping to reduce research costs.

[0033] 3. The device has multiple support rods, so multiple sample fixture boxes are set on the support rods to achieve simultaneous batch testing of the dynamic performance of carbon graphite materials. At the same time, there are multiple friction rings with different shapes on the rotating shaft, so that the corresponding friction rings can be selected according to the actual application conditions to detect the dynamic performance parameters of the carbon graphite material under actual working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 -Schematic diagram of the structure of the present invention.

[0035] Figure 2 -Test schematic diagram.

[0036] Figure 3 -Schematic diagram of the sample structure.

[0037] Figure 4-X Characteristic curve diagram of PV, temperature T and wear W of X1#-1.

[0038] Figure 5-X Characteristic curve diagram of PV, temperature T and wear W of X1#-2.

[0039] Figure 6-X Characteristic curve diagram of PV, temperature T and wear W of X2#-1.

[0040] Figure 7-X Characteristic curve diagram of PV, temperature T and wear W of X2#-2.

[0041] Figure 8-X Characteristic curves of PV, temperature T and wear W of X3#-1.

[0042] Figure 9-X Characteristic curve diagram of PV, temperature T and wear W of X3#-2.

[0043] Figure 10-X Characteristic curves of PV, temperature T and wear W of X4#-1.

[0044] Among them: 1-friction ring machine handle; 2-friction ring; 3-pressor; 4-sample fixture box; 5-bearing seat; 6-torque sensor, 7-coupling; 8-speed regulating motor; 9-speed sensor; 10-rotating shaft; 11-support frame; 12-base; 13-protective cover. DETAILED DESCRIPTION

[0045] See also Figure 1 , a device for detecting the dynamic properties of carbon graphite material, comprising a base 12, a rotating shaft 10, a friction ring 2, a pressure device 3 and a speed regulating motor 8 arranged on the base 12, the rotating shaft 10 is connected to the output shaft of the speed regulating motor 8, the friction ring 2 is detachably fixedly sleeved on the rotating shaft 10 to rotate synchronously with the rotating shaft 10, a sample fixture box 4 is arranged on the outer circumference of the friction ring 2 for placing the sample, the sample fixture box 4 is located on the radial diameter of the friction ring 2 and the sample fixture box 4 has a through hole for the sample part to pass through, and the through hole end of the sample fixture box 4 has a gap from the circumferential surface of the friction ring 2, so that the sample part passes through the through hole of the sample fixture box 4 and contacts the circumferential surface of the friction ring 2; the pressure device 3 is used to apply pressure to the sample.

[0046] The speed regulating motor here can adjust the motor speed within a certain range, so as to facilitate the detection of the dynamic performance of the carbon graphite sample at different speeds, and the friction ring here has a larger diameter, so that the friction ring has a larger linear speed during the high-speed rotation of the speed regulating motor, and thus the dynamic performance of the carbon graphite under high linear speed conditions can be detected. The setting of the pressure device can apply different pressure loads to the carbon graphite sample, so as to measure the dynamic performance of the carbon graphite under different pressure conditions.

[0047] The friction ring is detachably fixed on the rotating shaft, so that the friction ring can be replaced according to actual conditions.

[0048] When testing the dynamic performance of different samples, in order to simulate actual working conditions, the shape and structure of the friction surface of the test sample in contact with the circumferential surface of the friction ring are designed according to actual applications.

[0049] During specific implementation, the sample fixture box 4 is arranged on the outer circumference of the friction ring 2 through a support frame 11, and the support frame 11 is fixed on a base 12. The support frame 11 includes two vertically arranged end plates and a plurality of support rods arranged between the two end plates. The two end plates are fixed side by side on the base 12, each support rod is arranged horizontally and the two ends of each support rod are respectively fixed to the edges of the two end plates, all support rods are evenly distributed along the circumference of the end plates, and a through hole for the rotating shaft to pass through is provided in the center of the two end plates; the sample fixture box 4 is fixed on the support rod, and bearing seats 5 are respectively provided on the bases outside the two end plates for supporting the rotating shaft 10.

[0050] There are multiple support rods here, so that multiple sample fixture boxes can be arranged on the radial circumference and / or axial direction of the friction ring to achieve simultaneous testing of multiple samples.

[0051] In a specific implementation, the friction ring 2 includes a plurality of spiral friction rings and a plurality of smooth friction rings, and all the friction rings 2 are arranged at intervals.

[0052] The smooth friction ring here is a friction ring with a smooth outer circumferential surface, specifically a 40CrNiMoA chrome-plated smooth friction ring, which can simulate the flexible circumferential carbon-graphite sealing mode of an aircraft engine, and can produce air film friction reduction and less wear when the pressure P is small and the linear velocity V is large; the spiral friction ring is a friction ring with a spiral thread on the outer circumferential surface, specifically a 40Cr2MoV chrome-plated spiral friction ring and a 50Mn chrome-plated spiral friction ring. The spiral friction ring can detect the dynamic performance of carbon-graphite samples when they are not affected by airflow or are less affected by airflow.

[0053] In this embodiment, two smooth friction rings and two spiral friction rings are provided. 40CrNiMoA chrome-plated, 40Cr2MoV chrome-plated and 50Mn chrome-plated are all typical friction pair materials.

[0054] During specific implementation, the sample fixture box can be movably fixed on the support rod, so as to facilitate the selection of the corresponding friction ring to detect the dynamic performance of the sample.

[0055] In this way, the dynamic performance of the corresponding friction pair test specimen can be selected according to needs to achieve the purpose of simulating the working conditions of actual applications.

[0056] During specific implementation, a torque sensor 6 is provided between the rotating shaft 10 and the output shaft of the speed regulating motor 8. The torque sensor 6 is connected to the rotating shaft 10 and the output shaft of the speed regulating motor 8 through two couplings 7. One end of the two couplings 7 is respectively connected to the two ends of the torque sensor 6, and the other end is respectively connected to one end of the rotating shaft 10 or the output shaft of the speed regulating motor 8. The torque sensor 6 is connected to the control unit for monitoring the torque and transmitting it to the control unit for detecting the friction coefficient of the sample.

[0057] In this embodiment, a protective cover 13 is also provided on the coupling to protect the coupling.

[0058] During specific implementation, a speed sensor 9 is provided on the speed regulating motor 8 , and the speed sensor 9 is connected to the control unit to monitor the speed of the speed regulating motor 8 and transmit the speed to the control unit.

[0059] In a specific implementation, the sample holder box 4 is surrounded by a heating resistor to heat the sample placed in the sample holder box.

[0060] It is convenient to detect the dynamic properties of carbon graphite material samples at different temperatures and high temperatures.

[0061] In specific implementation, a friction ring handle 1 is provided at the other end of the rotating shaft 10 to facilitate manual detection of the rotation speed.

[0062] In this way, the staff can manually detect the rotation speed of the shaft through the probe, which is also the rotation speed of the friction ring.

[0063] See also Figure 2 , is the test principle diagram of using the device to detect carbon graphite samples, and its test principle is:

[0064] The implementation principle of the test sliding linear speed (V) is: the speed regulating motor runs at the required speed through voltage regulation, and the speed regulating motor drives the friction ring to run at the required linear speed through the coupling.

[0065] The principle of implementing the test pressure (P): The sample is assembled in the sample fixture box and can move freely up and down. The pressure required for the test is applied to the upper end of the sample by the sample pressure device.

[0066] The realization principle of the sample temperature (T): through the resistance heating around the fixture box, the temperature is monitored by the thermocouple embedded in the temperature measuring hole, and the required temperature is set and automatically controlled by the control system

[0067] Friction ring: It consists of 2 threaded friction rings and 2 smooth friction rings for test options.

[0068] In the following embodiments, four types of green bodies of carbon graphite materials XX1#, XX2#, XX3#, and XX4# produced by a representative domestic enterprise are selected as raw materials. XX1#, XX2#, XX3#, and XX4# are benchmarked against the standards of the Ministry of Aviation Industry of the People's Republic of China, enterprise standards, model standards, etc., and the materials are judged to meet the standards. The performance parameters of XX1#, XX2#, XX3#, and XX4# are shown in Table 1.

[0069] Table 1. Performance parameters of XX1#, XX2#, XX3#, and XX4#

[0070]

[0071]

[0072] Take two blanks of XX1#, XX2#, XX3# and XX4# for backup, and the size of each blank shall be ≥40×25×12.5mm. Figure 3 The samples were processed and then ultrasonically cleaned for 30 min and finally dried in a vacuum drying oven for 12 h. They were then named XX1#-1, XX1#-2, XX2#-1, XX2#-2, XX3#-1, XX3#-2, XX4#-1 and XX4#-2.

[0073] The friction rings used in the following Examples 1-6 are 40CrNiMoA chrome-plated smooth friction rings, and the friction rings used in Example 7 are 40Cr2MoV chrome-plated spiral friction rings. The relevant performance parameters thereof are shown in Table 2.

[0074] Table 2. Friction ring performance parameters

[0075] Material Name Surface roughness Radial runout (mm) Dimensions in mm Pitch Slot width Helix Angle 40CrNiMoA chrome plating 0.2-0.4 0.04 Φ500 - - - 40Cr2MoV chrome plating 0.4-0.8 0.03 Φ500 10 3 6°

[0076] Generally, the allowable PV value = limit PV ÷ α, where α is 1.2 to 1.5. In the following embodiments, α = 1.5.

[0077] Example 1

[0078] The sample in this embodiment is XX1#-1.

[0079] (1) After the processed sample XX1#-1 is loaded into the temperature-controlled sample fixture box, a temperature measuring thermocouple is inserted into the small hole (Φ1.5) on the side of the sample. The constant speed (80m / s)-variable load test method is adopted, and the radial pressure is applied in the range of 30-410KPa;

[0080] (2) After ensuring that the dynamic performance detection device and control system are normal, start the device, run-in the sample and friction ring, stop the machine when the running-in area reaches more than 95%, remove the sample, and use the measuring system consisting of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare and measure the original height of the initial running-in sample (accuracy 0.0001), and record it;

[0081] The measurement process first uses a standard gauge block close to the specimen height to calibrate the height of the micrometer and zero it, then uses the ground specimen for measurement. The reading of the micrometer is the difference between the gauge block height and the original height of the specimen being tested. In subsequent measurements, as wear increases, the difference between the micrometer calibrated with the gauge block height and the specimen being tested will also gradually increase, and the increased portion is the wear value of the specimen.

[0082] (3) The sample removed in step (2) is loaded into the temperature-controlled sample fixture box again, and the peripheral linear speed of the device is set to 80 m / s. The sample temperature and friction coefficient are observed in real time and recorded every 30 minutes. After running for 2 hours, the sample is removed and the measurement height is compared and the wear amount is calculated using a measuring system consisting of a detection platform, a standard gauge block, a micrometer bracket, and a micrometer;

[0083] (4) Place the sample removed in step (3) into a temperature-controlled sample fixture box, keep the circumferential linear velocity constant, increase the pressure step by step by 20 KPa, observe the sample temperature and friction coefficient in real time, and record them every 30 minutes. After running for 2 hours, remove the sample and use a measuring system consisting of a testing platform, a standard gauge block, a micrometer bracket, and a micrometer to compare the measurement height and calculate the wear amount;

[0084] (5) Repeat step (4) until the limit PV value appears, and remove the sample;

[0085] (6) The corresponding material is processed into an engine graphite sealing ring, installed and verified, and it is known that the PV value of the engine fulcrum is less than the allowable PV value to determine whether the application is normal.

[0086] In this implementation, the characteristic curves of PV, temperature T, and wear W of XX1#-1 are as follows: Figure 4 As shown by Figure 4 It can be seen that when the temperature of the sample and the friction pair is not increased, the speed is constant at 80m / s, and the load is variable from 30-410KPa, the wear value of the XX1#-1 sample has an inflection point when the temperature is 52°C, the limit PV is 10.4MPa*m / s, the limit point wear value is 0.006mm / h, the allowable PV value is 6.9MPa*m / s, and it has been demonstrated that the graphite rings processed with this material are in normal use in the engine installation test.

[0087] Example 2

[0088] The sample in this embodiment is XX1#-2.

[0089] (1) After the processed sample XX1#-2 is loaded into the temperature-controlled sample fixture box, a temperature measuring thermocouple is inserted into the small hole (Φ1.5) on the side of the sample. The constant load (300KPa)-variable speed test method is adopted, and the circumferential linear speed of the slip ring is set in the range of 10-80m / s;

[0090] (2) After ensuring that the dynamic performance detection device and control system are normal, run-in the sample and friction ring. When the running-in area reaches more than 95%, stop the machine, remove the sample, and use the measuring system consisting of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare and measure the original height of the initial running-in sample (accuracy 0.0001), and record it;

[0091] The measurement process first uses a standard gauge block close to the specimen height to calibrate the height of the micrometer and zero it, then uses the ground specimen for measurement. The reading of the micrometer is the difference between the gauge block height and the original height of the specimen being tested. In subsequent measurements, as wear increases, the difference between the micrometer calibrated with the gauge block height and the specimen being tested will also gradually increase, and the increased portion is the wear value of the specimen.

[0092] (3) The sample removed in step (2) is placed back into the temperature-controlled sample fixture box, the pressure of the device is set to 300 kPa, the sample temperature and friction coefficient are observed in real time, and recorded every 30 minutes. After running for 2 hours, the sample is removed, and the measurement height is compared and the wear amount is calculated using a measuring system consisting of a testing platform, a standard gauge block, a micrometer bracket, and a micrometer;

[0093] (4) Place the sample removed in step (3) into a temperature-controlled sample fixture box, keep the pressure constant, increase the linear speed step by step by 10 m / s, observe the sample temperature and friction coefficient in real time, record them every 30 minutes, and after running for 2 hours, remove the sample and use a measuring system consisting of a testing platform, a standard gauge block, a dial gauge bracket, and a dial gauge to compare the measurement height and calculate the wear amount;

[0094] (5) Repeat step (4) until the limit PV value appears, and remove the sample;

[0095] (6) The corresponding material is processed into an engine graphite sealing ring, installed and verified, and it is known that the PV value of the engine fulcrum is less than the allowable PV value to determine whether the application is normal.

[0096] In this implementation, the characteristic curves of PV, temperature T, and wear W of XX1#-2 are as follows: Figure 5 As shown by Figure 5 It can be seen that when the temperature of the sample and the friction pair is not increased, the fixed load is 300KPa, and the speed is changed from 10-80m / s, the wear value of the XX1#-2 sample has an inflection point when the temperature is 87℃, the limit PV is 12MPa*m / s, the limit point wear value is 0.157μm / Km, the allowable PV value is 8.0MPa*m / s, and it has been demonstrated that the graphite ring engine installed test using this material is normal.

[0097] Example 3

[0098] The sample in this embodiment is XX2#-1, and its test steps are the same as those in Example 1.

[0099] In this implementation, the characteristic curves of PV, temperature T, and wear W of XX2#-1 are as follows: Figure 6 As shown by Figure 6 It can be seen that when the temperature of the sample and the friction pair is not increased, the speed is constant at 80m / s, and the load is variable from 30-410KPa, the wear value of the XX2#-1 sample has an inflection point when the temperature is 75℃, the limit PV is 13.6MPa*m / s, the limit point wear value is 0.006mm / h, the allowable PV value is 9.1MPa*m / s, and it has been demonstrated that the graphite rings processed with this material are in normal use in the engine installation test.

[0100] Example 4

[0101] The sample in this embodiment is XX2#-2, and its test steps are the same as those in Example 2.

[0102] In this implementation, the characteristic curves of PV, temperature T, and wear W of XX2#-2 are as follows: Figure 7 As shown by Figure 7It can be seen that when the temperature of the sample and the friction pair is not increased, the fixed load is 300KPa, and the speed is changed from 10-80m / s, the wear value of the XX2#-2 sample has an inflection point when the temperature is 86℃, the limit PV is 15MPa*m / s, the limit point wear value is 0.009μm / km, and the allowable PV value is 10MPa*m / s. ​​It has been demonstrated that the engine installation test is in normal use.

[0103] Example 5

[0104] The sample in this embodiment is XX3#-1, and its test steps are the same as those in Example 1.

[0105] In this implementation, the characteristic curves of PV, temperature T, and wear W of XX3#-1 are as follows: Figure 8 As shown by Figure 8 It can be seen that when the temperature of the sample and the friction pair is not increased, the speed is constant at 80m / s, and the load is variable from 30-410KPa, the wear value of the XX3#-1 sample has an inflection point when the temperature is 61°C, the limit PV is 18.4MPa*m / s, the limit point wear value is 0.003mm / h, the allowable PV value is 12.3MPa*m / s, and it has been demonstrated that the graphite rings processed with this material are in normal use in the engine installation test.

[0106] Example 6

[0107] The sample in this embodiment is XX3#-2, and its test steps are the same as those in Example 2.

[0108] In this implementation, the characteristic curves of PV, temperature T, and wear W of XX3#-2 are as follows: Fig. 9 As shown by Fig. 9 It can be seen that when the temperature of the sample and the friction pair is not increased, the fixed load is 300KPa, and the speed is changed from 10-80m / s, the wear value of the XX3#-2 sample has an inflection point when the temperature is 77℃, the limit PV is 18MPa*m / s, the limit point wear value is 0.006μm / km, the allowable PV value is 12MPa*m / s, and it has been demonstrated that the graphite ring gas turbine installed test using this material is in normal use.

[0109] Example 7

[0110] The sample in this embodiment is XX4#-1, and its test steps are the same as those in Example 1. This embodiment is used as a comparative example. During the test verification, the XX4#-1 material is processed into an engine graphite sealing ring and installed for verification. It is known that the PV value of this fulcrum of the engine is higher than the allowable PV value to determine whether the application is normal.

[0111] In this implementation, the characteristic curves of PV, temperature T, and wear W of XX4#-1 are as follows: Fig.10 As shown by Fig.10It can be seen that when the temperature of the sample and the friction pair is not increased, the speed is constant at 80m / s, and the load is variable from 30-410KPa, the wear value of the XX4#-1 sample has an inflection point when the temperature is 89°C, the limit PV is 7.2MPa*m / s, the limit point wear value is 0.1375mm / h, and the allowable PV value is 4.8MPa*m / s. ​​It has been demonstrated that the graphite rings processed with this material have abnormal wear during the engine installation test. Therefore, the dynamic performance of XX4#-2 has not been verified under constant pressure and variable speed conditions.

[0112] The statistical analysis of the test data of Examples 1 to 7 is shown in Table 3.

[0113] Table 3. Statistical analysis of experimental data

[0114]

[0115] Through the above tests and analysis, it can be known that the PV values ​​of different fulcrums of the engine are different. As long as the PV value of the engine working condition is within the allowable PV of the material test, the graphite ring works normally. When the PV value of the engine working condition exceeds the allowable PV of the material test, the graphite ring wears abnormally. Therefore, it has been proved through practice that the test data shows that the VW wear value can obviously represent the material limit PV value, and the PV-T temperature has no obvious acceleration trend. This is related to the fact that the test friction ring is open and placed in the natural atmospheric environment, and the friction ring has a high speed and the heat dissipation conditions are relatively sufficient.

[0116] The results of the typical engine pivot seal materials tested according to the device and method for the dynamic performance of carbon graphite materials show that the test bench and test method are feasible, the test data can characterize the characteristics of the material, and can provide test data support for the analysis of the friction and wear mechanism, selection, and improvement of graphite sealing materials. The state limit PV values ​​of different materials are quite different, and the test data can be used as one of the bases for the selection of engine pivot graphite sealing materials, and can provide identification methods and improvement paths for the research of engine pivot graphite sealing materials.

[0117] Finally, it should be noted that the above embodiments of the present invention are only examples for illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

Claims

1. A method for detecting the dynamic properties of carbon graphite materials, characterized in that: A device for detecting the dynamic properties of carbon graphite is used to detect the dynamic properties of a sample. The device includes a base, a rotating shaft, a friction ring, a pressure device and a speed regulating motor arranged on the base. The rotating shaft is connected to the output shaft of the speed regulating motor. The friction ring is detachably fixedly sleeved on the rotating shaft to rotate synchronously with the rotating shaft. A sample fixture box is arranged on the outer circumference of the friction ring for placing the sample. The sample fixture box is located on the radial diameter of the friction ring and has a through hole for the sample part to pass through. There is a gap between the through hole end of the sample fixture box and the circumferential surface of the friction ring, so that the sample part passes through the through hole of the sample fixture box and contacts the circumferential surface of the friction ring. The pressure device is used to apply pressure to the sample. The specific steps include: S1: Processing samples: Process the carbon graphite blank into samples, then use ultrasonic cleaning for 10-30 minutes, and then place it in a vacuum drying oven for 8-24 hours for standby use; one end of the sample has a convex portion passing through the through hole of the sample fixture box, and a pressure hole and a temperature measuring hole are opened at the other end of the sample, the pressure hole is set in the middle, and the temperature measuring hole is eccentrically set and extends obliquely to the convex portion, which is used to detect the temperature change of the sample; S2: After the sample is loaded into the sample fixture box, the convex surface of the sample is in contact with the friction ring, a temperature measuring thermocouple is inserted into the temperature measuring hole, and a pressure device is inserted into the pressure hole; S3: After checking that the device and control system are normal, start the device, apply radial pressure to the sample within 30~410KPa, run-in the sample and the friction ring, and when the running-in area reaches more than 95%, close the device, remove the sample, and use the measuring system composed of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare and measure the original height of the initial running-in sample, and record it; S4: Put the sample taken out in step S3 into the sample fixture box again, set the circumferential speed of the device to 10-144 m / s and keep it constant, apply radial pressure to the sample, observe the sample temperature and friction coefficient in real time, record them every 30 minutes, and after running for 2 hours, take out the sample, compare the measurement height and calculate the wear amount using the measuring system consisting of the detection platform, standard gauge block, micrometer bracket and micrometer; S5: Place the sample removed in step S4 into a temperature-controlled sample fixture box, keep the circumferential linear speed constant, increase the pressure step by step by 10-30 KPa, observe the sample temperature and friction coefficient in real time, and record them every 30 minutes. After running for 2 hours, remove the sample, and use a measuring system consisting of a detection platform, a standard gauge block, a dial gauge bracket, and a dial gauge to compare the measurement height and calculate the wear amount; S6: Repeat step S5 until the characterization of the limit PV value appears, remove the sample, and thus obtain the dynamic performance parameters of the sample under different working conditions.

2. A method for detecting the dynamic properties of carbon stone material graphite, characterized in that: A device for detecting the dynamic properties of carbon graphite is used to detect the dynamic properties of a sample. The device includes a base, a rotating shaft, a friction ring, a pressure device and a speed regulating motor arranged on the base. The rotating shaft is connected to the output shaft of the speed regulating motor. The friction ring is detachably fixedly sleeved on the rotating shaft to rotate synchronously with the rotating shaft. A sample fixture box is arranged on the outer circumference of the friction ring for placing the sample. The sample fixture box is located on the radial diameter of the friction ring and has a through hole for the sample part to pass through. There is a gap between the through hole end of the sample fixture box and the circumferential surface of the friction ring, so that the sample part passes through the through hole of the sample fixture box and contacts the circumferential surface of the friction ring. The pressure device is used to apply pressure to the sample. The specific steps include: S1: Processing samples: Process the carbon graphite blank into samples, then use ultrasonic cleaning for 10-30 minutes, and then place it in a vacuum drying oven for 8-24 hours for standby use; one end of the sample has a convex portion passing through the through hole of the sample fixture box, and a pressure hole and a temperature measuring hole are opened at the other end of the sample, the pressure hole is set in the middle, and the temperature measuring hole is eccentrically set and extends obliquely to the convex portion, which is used to detect the temperature change of the sample; S2: After the sample is loaded into the sample fixture box, the convex surface of the sample is in contact with the friction ring, a temperature measuring thermocouple is inserted into the temperature measuring hole, and a pressure device is inserted into the pressure hole; S3: After checking that the device and control system are normal, start the device, apply radial pressure to the sample within 30~410KPa, run-in the sample and the friction ring, and when the running-in area reaches more than 95%, close the device, remove the sample, and use the measuring system composed of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare and measure the original height of the initial running-in sample, and record it; S4: Put the sample taken out in step S3 into the sample fixture box again, set the pressure of the device to 10~410KPa and keep constant pressure, and maintain a certain linear speed, observe the sample temperature and friction coefficient in real time, record once every 30 minutes, and after running for 2 hours, take out the sample, and use the measuring system composed of the detection platform, standard gauge block, micrometer bracket, and micrometer to compare the measurement height and calculate the wear amount; S5: Place the sample removed in step S4 into a temperature-controlled sample fixture box, keep the pressure constant, increase the linear speed step by step by 10 m / s, observe the sample temperature and friction coefficient in real time, record once every 30 minutes, and after running for 2 hours, remove the sample, and use a measuring system consisting of a detection platform, a standard gauge block, a dial gauge bracket, and a dial gauge to compare the measurement height and calculate the wear amount; S6: Repeat step S5 until the characterization of the limit PV value appears, remove the sample, and thus obtain the dynamic performance parameters of the sample under different working conditions.

3. A method for detecting the dynamic properties of carbon stone material graphite according to claim 1 or 2, characterized in that: The sample fixture box is arranged on the outer circumference of the friction ring through a support frame, and the support frame is fixed on the base. The support frame includes two vertically arranged end plates and a plurality of support rods arranged between the two end plates. The two end plates are fixed on the base side by side, each support rod is arranged horizontally and the two ends of each support rod are respectively fixed to the edges of the two end plates, all support rods are evenly distributed along the circumference of the end plates, and the centers of the two end plates are provided with through holes for the rotation shaft to pass through; the sample fixture box is fixed on the support rods, and the bases outside the two end plates are respectively provided with bearing seats for supporting the rotation shaft.

4. A method for detecting the dynamic properties of carbon stone material graphite according to claim 3, characterized in that: The friction rings include a plurality of spiral friction rings and a plurality of smooth friction rings, and all the friction rings are arranged at intervals.

5. A method for detecting the dynamic properties of carbon stone material graphite according to claim 3, characterized in that: The sample fixture box can be movably fixed on the support rod, so as to facilitate the selection of the corresponding friction ring to detect the dynamic performance of the sample.

6. A method for detecting the dynamic properties of carbon stone material graphite according to claim 3, characterized in that: A torque sensor is provided between the rotating shaft and the output shaft of the speed regulating motor. The torque sensor is connected to the rotating shaft and the output shaft of the speed regulating motor through two couplings. One end of the two couplings is respectively connected to the two ends of the torque sensor, and the other end is respectively connected to one end of the rotating shaft or the output shaft of the speed regulating motor. The torque sensor is connected to the control unit to monitor the torque and transmit it to the control unit to facilitate the detection of the friction coefficient of the sample.

7. A method for detecting the dynamic properties of carbon stone material graphite according to claim 6, characterized in that: The speed regulating motor is provided with a speed sensor, which is connected to the control unit and is used to monitor the speed of the speed regulating motor and transmit the speed to the control unit.

8. A method for detecting the dynamic performance of carbon stone material graphite according to claim 3, characterized in that: The sample holder box is provided with a heating resistor around it, so as to heat the sample placed in the sample holder box.