Maleimide copolymer, method for producing the same, resin composition and injection molded article
By synthesizing the mixing of maleimide-based copolymers with high glass transition temperature and fluidity with other resins, the problem of insufficient fluidity in the prior art is solved, and chemical resistance, heat resistance and impact resistance are achieved. The balance of characteristics improves molding speed and production efficiency.
Patent Information
- Application Number
- CN202080024145.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-10
- Filing Date
- 2020-07-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-07-07
AI Technical Summary
When the existing maleimide-based copolymers improve heat resistance and chemical resistance, the fluidity is insufficient, making it difficult to meet the needs of high fluidity and impact resistance.
By synthesizing maleimide-based copolymers with high glass transition temperature and high flowability, combining resins such as ABS resin, ASA resin or SAN resin, the viscosity and molding performance of the resin composition are optimized and the flowability is improved. and productivity.
While maintaining the balance of chemical resistance, heat resistance and impact resistance, the flowability of the resin composition is significantly improved, and the rapidity of molding and productivity improvement are promoted.
Smart Images

Figure BDA0003277126830000191 
Figure BDA0003277126830000201 
Figure BDA0003277126830000231
Abstract
Description
Background Art
[0001] Acrylonitrile-butadiene-styrene copolymer resin (ABS resin) has excellent mechanical strength, appearance, chemical resistance, moldability, etc., and is widely used in the fields of automobiles, home appliances, OA equipment, residential building materials, daily necessities, etc. For applications such as automotive interior materials that require heat resistance, ABS resins mixed with maleimide-based copolymers are also used as heat resistance imparting agents (for example, Patent Documents 1 and 2).
[0002] However, ABS resins prepared with maleimide copolymers have the disadvantage of low chemical resistance. To overcome this disadvantage, maleimide copolymers obtained by copolymerizing vinyl cyanide monomers have been proposed (e.g., Patent Documents 3 and 4). The copolymers obtained by copolymerizing vinyl cyanide monomers proposed so far have high heat resistance, but there is an urgent need to further improve their fluidity.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 57-98536
[0006] Patent Document 2: Japanese Patent Application Publication No. 57-125242
[0007] Patent Document 3: Japanese Patent Application Publication No. 2004-339280
[0008] Patent Document 4: Japanese Patent Application Publication No. 2007-9228 Summary of the invention
[0009] Problems to be solved by the invention
[0010] The present invention aims to provide a maleimide copolymer and a method for producing the same, which can obtain a resin composition having excellent fluidity while maintaining a balance between chemical resistance, heat resistance and impact resistance. In addition, a resin composition is provided, which is obtained by kneading and mixing a maleimide copolymer with one or more resins selected from ABS resin, acrylonitrile-styrene-acrylic rubber copolymer resin (ASA resin), acrylonitrile-ethylene·propylene rubber-styrene copolymer resin (AES resin) or styrene-acrylonitrile copolymer resin (SAN resin), and has excellent physical property balance of chemical resistance, heat resistance and impact resistance, and high fluidity.
[0011] Technical means to solve the problem
[0012] In the present invention, if a maleimide copolymer having a high glass transition temperature and high fluidity is used, the viscosity of the resin composition can be reduced without increasing the amount added to the resin composition, which contributes to the high-speed molding and improved productivity.
[0013] That is, the present invention has the following points.
[0014] (1) A maleimide copolymer comprising an aromatic vinyl monomer unit, a vinyl cyanide monomer unit, and a maleimide monomer unit, wherein the maleimide copolymer has a glass transition temperature of 165°C to 200°C and a melt mass flow rate of 25 to 80 g / 10 min at 265°C and a load of 98 N as measured by the method described in JIS K 7210.
[0015] (2) The maleimide copolymer according to (1), which contains 40 to 59.5% by mass of an aromatic vinyl monomer unit, 5 to 20% by mass of a vinyl cyanide monomer unit, and 35 to 50% by mass of a maleimide monomer unit.
[0016] (3) The maleimide copolymer according to (1) or (2), further comprising 0.5 to 10% by mass of a dicarboxylic acid anhydride monomer unit in the maleimide copolymer.
[0017] (4) The maleimide copolymer according to any one of (1) to (3), wherein the content of the residual maleimide monomer is less than 300 ppm.
[0018] (5) A method for producing a maleimide copolymer as described in any one of (1) to (4), which comprises the following steps: an initial polymerization step: mixing the entire amount of vinyl cyanide monomer, 10 to 90% by weight of the aromatic vinyl monomer, and 0 to 30% by weight of the unsaturated dicarboxylic anhydride monomer to initiate copolymerization; an intermediate polymerization step: adding 50 to 90% by weight of the remaining aromatic vinyl monomer and the entire amount of the remaining unsaturated dicarboxylic anhydride monomer in batches or continuously, respectively, and continuing copolymerization; a final polymerization step: adding the entire amount of the remaining aromatic vinyl monomer to obtain a copolymer having aromatic vinyl monomer units, vinyl cyanide monomer units, and dicarboxylic anhydride monomer units; and an imidization step: imidizing the dicarboxylic anhydride monomer units of the obtained copolymer into maleimide monomer units using ammonia or a primary amine.
[0019] (6) A resin composition comprising 5 to 40% by mass of the maleimide copolymer according to any one of (1) to (4) and 60 to 95% by mass of a resin, wherein the resin is one or more selected from ABS resin, ASA resin, AES resin or SAN resin.
[0020] (7) An injection molded article using the resin composition described in (6).
[0021] (8) The injection-molded article according to (7), which is used as an interior part or exterior part of an automobile.
[0022] Effects of the Invention
[0023] According to the present invention, a maleimide copolymer can be obtained, which can obtain a resin composition having excellent fluidity while maintaining a balance between chemical resistance, heat resistance and impact resistance, and a method for producing the same. In addition, a resin composition can be obtained by kneading and mixing a maleimide copolymer with one or more resins selected from ABS resin, ASA resin, AES resin or SAN resin, the resin composition having excellent physical property balance of chemical resistance, heat resistance and impact resistance and high fluidity. DETAILED DESCRIPTION
[0024] <Terminology>
[0025] In this specification, for example, the description "A to B" means A or more and B or less.
[0026] The embodiments of the present invention are described in detail below: The maleimide-based copolymer of the present invention has an aromatic vinyl monomer unit, a vinyl cyanide monomer unit, and a maleimide monomer unit.
[0027] Aromatic vinyl monomers that can be used for maleimide copolymers are used to improve the hue of the resin composition, and include, for example, styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, ethylstyrene, p-tert-butylstyrene, α-methylstyrene, and α-methyl-p-methylstyrene. Among them, styrene is preferred because it has a good effect of improving the hue. Aromatic vinyl monomers can be used alone or in combination of two or more.
[0028] The amount of the aromatic vinyl monomer unit contained in the maleimide copolymer is preferably 40 to 59.5% by mass, and more preferably 45 to 55% by mass. Specifically, for example, it is 40, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 59.5% by mass, or it may be within the range between any two values exemplified here. By making the amount of the aromatic vinyl monomer unit 40% by mass or more, the hue of the obtained resin composition will not turn yellow, and by making it 59.5% by mass or less, the heat resistance of the obtained resin composition can be improved.
[0029] The cyanide vinyl monomers that can be used in maleimide copolymers are used to improve the chemical resistance of the resin composition, and include, for example, acrylonitrile, methacrylonitrile, ethacrylonitrile, and fumaronitrile. Among them, acrylonitrile is preferred because it has a good effect of improving chemical resistance. The cyanide vinyl monomers can be used alone or in combination of two or more.
[0030] The amount of the cyanide vinyl monomer unit contained in the maleimide copolymer is preferably 5 to 20% by mass, and more preferably 7 to 15% by mass. Specifically, for example, it is 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 20% by mass, and may also be within the range between any two of the values exemplified here. By making the amount of the cyanide vinyl monomer unit 5% or more by mass, the chemical resistance of the obtained resin composition is improved, and by making it 20% or less by mass, the hue of the obtained resin composition will not be yellowish.
[0031] Maleimide monomers that can be used for maleimide copolymers are used to improve the heat resistance of resin compositions, such as N-alkylmaleimides such as N-methylmaleimide, N-butylmaleimide, and N-cyclohexylmaleimide, as well as N-phenylmaleimide, N-chlorophenylmaleimide, N-methylphenylmaleimide, N-methoxyphenylmaleimide, and N-tribromophenylmaleimide. Among them, N-phenylmaleimide with good effect of improving heat resistance is preferred. Maleimide monomers can be used alone or in combination of two or more. In order to contain maleimide monomer units in maleimide copolymers, it is sufficient to copolymerize aromatic vinyl monomers, vinyl cyanide monomers, and maleimide monomers. Alternatively, a dicarboxylic anhydride monomer unit derived from an unsaturated dicarboxylic anhydride monomer of a copolymer obtained by copolymerizing an aromatic vinyl monomer, a vinyl cyanide monomer, and an unsaturated dicarboxylic anhydride monomer described below may be imidized with ammonia or a primary amine.
[0032] The amount of maleimide monomer units contained in the maleimide copolymer is preferably 35 to 50% by mass, and more preferably 37 to 45% by mass. Specifically, for example, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50% by mass, or within the range between any two values exemplified herein. By making the amount of maleimide monomer units 35% by mass, the heat resistance of the obtained maleimide copolymer is improved, and by making it 50% by mass, the impact strength of the obtained maleimide copolymer will not be reduced.
[0033] The maleimide copolymer may also contain a dicarboxylic anhydride monomer unit having an effect of improving the compatibility of the maleimide copolymer with other resins. In order to introduce the dicarboxylic anhydride monomer unit into the maleimide copolymer, an unsaturated dicarboxylic anhydride monomer may be copolymerized with the above-mentioned monomer, or the imidization rate may be adjusted to residual dicarboxylic anhydride monomer units when the copolymer obtained by copolymerizing the above-mentioned aromatic vinyl monomer with a cyanide vinyl monomer and an unsaturated dicarboxylic anhydride monomer is imidized. As unsaturated dicarboxylic anhydride monomers, for example, there are maleic anhydride, itaconic anhydride, citraconic anhydride, and aconitic anhydride. Among them, maleic anhydride with a good effect of improving compatibility is preferably used. Unsaturated dicarboxylic anhydride monomers may be used alone or in combination of two or more.
[0034] The amount of the dicarboxylic anhydride monomer unit contained in the maleimide copolymer is preferably 0.5 to 10% by mass, and more preferably 0.1 to 2% by mass. Specifically, for example, it is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 2, 3, 4, 5, 6, 7, 8, 9, 10% by mass, and it can also be in the range between any two values exemplified here. By making the amount of the dicarboxylic anhydride monomer unit 0.5% by mass or more, the compatibility of the obtained maleimide copolymer with resins such as ABS is improved, and by making it less than 10% by mass, the thermal stability of the obtained resin composition is improved.
[0035] The maleimide copolymer may be copolymerized with copolymerizable monomers other than aromatic vinyl monomers, vinyl cyanide monomers, maleimide monomers and unsaturated dicarboxylic anhydride monomers within a range that does not hinder the effect of the present invention. Examples of monomers copolymerizable with the maleimide copolymer include acrylate monomers such as methyl acrylate, ethyl acrylate, and butyl acrylate; methacrylate monomers such as methyl methacrylate and ethyl methacrylate; vinyl carboxylic acid monomers such as acrylic acid and methacrylic acid; acrylic acid amide and methacrylic acid amide. Monomers copolymerizable with the maleimide copolymer may be used alone or in combination of two or more.
[0036] The amount of residual maleimide monomers contained in the maleimide copolymer is preferably less than 300 ppm, more preferably less than 230 ppm, and further preferably less than 200 ppm. When the amount of residual maleimide monomers is less than 300 ppm, the hue of the obtained resin composition is further improved.
[0037] The residual maleimide monomer amount is a value measured under the conditions described below.
[0038] Device name: Gas chromatograph GC-2010 (manufactured by Shimadzu Corporation)
[0039] Column: Capillary column DB-5ms (manufactured by Agilent Technologies, Inc.)
[0040] Temperature: Inlet 280℃, Detector 280℃
[0041] Temperature increase analysis was performed at a column temperature of 80°C (initial stage).
[0042] (Temperature analysis conditions) 80°C: hold for 12 minutes
[0043] 80~280℃: Raise the temperature at 20℃ / min for 10 minutes
[0044] 280℃: hold for 10 minutes
[0045] Detector: FID
[0046] Procedure: 0.5 g of the sample is dissolved in 5 ml of 1,2-dichloroethane solution (0.014 g / L) containing undecane (internal standard substance). Then, 5 ml of n-hexane is added and shaken with an oscillator for 10 to 15 minutes to precipitate it. In the state where the polymer is precipitated and precipitated, only the supernatant is injected into the gas chromatograph. Based on the peak area of the obtained maleimide monomer, the quantitative value is calculated using the coefficient obtained from the internal standard substance.
[0047] From the perspective of efficiently improving the heat resistance of ABS resin, ASA resin and other mixed resins, the glass transition temperature of the maleimide copolymer is 165°C to 200°C, preferably 170°C to 200°C, and more preferably 175°C to 185°C. Specifically, for example, it is 165, 170, 175, 176, 177, 178, 179, 180, 185, 190, 195, 200°C, and can also be within the range between any two values exemplified here. The glass transition temperature is a measured value measured using DSC under the measurement conditions described below.
[0048] Device name: Differential Scanning Calorimeter Robot DSC6200 (manufactured by Seiko Instruments)
[0049] Heating rate: 10℃ / min
[0050] In order to increase the glass transition temperature of the maleimide-based copolymer, the content of the maleimide monomer unit contained in the maleimide-based copolymer may be increased, or other monomers having a higher glass transition temperature may be copolymerized.
[0051] The melt mass flow rate of the maleimide copolymer is a value measured at 265°C and 98N load according to the method described in JIS K 7210, and is 25 to 80 g / 10 minutes. Specifically, it is 25, 26, 27, 28, 29, 30, 35, 40, 45, 50, 60, 65, 70, 75, 80 g / 10 minutes, and may be within the range between any two values exemplified here. If it is less than 25 g / 10 minutes, the fluidity of the mixed resin decreases, and if it is greater than 80 g / 10 minutes, the impact resistance decreases.
[0052] In order to reduce the melt mass flow rate of the maleimide-based copolymer, the content of the dicarboxylic anhydride monomer unit contained in the maleimide-based copolymer may be increased, or other monomers having a lower melt mass flow rate may be copolymerized.
[0053] The polymerization methods of maleimide copolymers include solution polymerization and bulk polymerization. Maleimide copolymers with more uniform copolymer composition can be obtained by adding and polymerizing in batches. From this point of view, solution polymerization is preferred. From the perspective of not producing by-products and having little adverse effects, the solvent for solution polymerization is preferably a non-polymerizing solvent, such as ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and acetophenone; ethers such as tetrahydrofuran and 1,4-dioxane; aromatic hydrocarbons such as benzene, toluene, xylene, and chlorobenzene; N,N-dimethylformamide, dimethyl sulfoxide, and N-methyl-2-pyrrolidone. Considering the ease of solvent removal when recovering maleimide copolymers by devolatilization, methyl ethyl ketone and methyl isobutyl ketone are preferred. Regarding the polymerization process, continuous polymerization, intermittent (batch) and semi-intermittent are all applicable.
[0054] The polymerization method of the maleimide copolymer is not particularly limited, but it can be preferably obtained by free radical polymerization, and the polymerization temperature is preferably in the range of 80 to 150°C. As the polymerization initiator, it is not particularly limited, for example, known azo compounds such as azobisisobutyronitrile, azobiscyclohexanecarbonitrile, azodimethylpropionitrile, and azodimethylbutyronitrile can be used; known organic peroxides such as benzoyl peroxide, tert-butyl peroxybenzoate, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy 2-ethylhexanoate, di-tert-butyl peroxide, dicumyl peroxide, and ethyl 3,3-di(tert-butylperoxy)butyrate can be used, and one of these can be used or two or more can be used in combination. From the viewpoint of polymerization reaction speed and polymerization rate control, it is preferred to use an azo compound or organic peroxide with a 10-hour half-life of 70 to 120°C. The amount of the polymerization initiator used is not particularly limited, and is preferably 0.1 to 1.5% by mass, more preferably 0.1 to 1.0% by mass, relative to 100% by mass of all monomer units. If the amount of the polymerization initiator used is 0.1% by mass or more, sufficient polymerization rate can be obtained, and if it is 1.5% by mass or less, the polymerization reaction is easily controlled, and it is easy to obtain a maleimide copolymer with a target weight average molecular weight.
[0055] The weight average molecular weight of the maleimide copolymer is 50,000 to 300,000, preferably 50,000 to 200,000. Specifically, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 25, 300,000, or within the range of any two values exemplified herein. If the weight average molecular weight is 50,000 or less, the impact resistance is reduced, and if it exceeds 300,000, the fluidity is reduced.
[0056] Chain transfer agents can be used in the manufacture of maleimide copolymers. The chain transfer agents used are not particularly limited, and examples thereof include n-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, α-methylstyrene dimer, ethyl mercaptoglycolate, limonene, and terpinene. The amount of the chain transfer agent used is not particularly limited as long as it is within the range of the maleimide copolymer with the target weight average molecular weight, but is preferably 0.01 to 0.8 mass %, more preferably 0.1 to 0.5 mass %, relative to 100 mass % of all monomers to be copolymerized. If the amount of the chain transfer agent used is 0.01 mass % to 0.8 mass %, the maleimide copolymer with the target weight average molecular weight can be easily obtained.
[0057] As a method for introducing maleimide monomer units into maleimide-based copolymers, there are methods of copolymerizing maleimide monomers with other monomers (direct method); or pre-copolymerizing unsaturated dicarboxylic anhydride monomers, aromatic vinyl monomers, and vinyl cyanide monomers, and then imidizing the dicarboxylic anhydride monomer units in the copolymer with ammonia or primary amine to convert them into maleimide monomer units (post-imidization method). The post-imidization method is preferred because the amount of residual maleimide monomers in the copolymer is small.
[0058] The so-called primary amines include alkylamines such as methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, n-pentylamine, n-hexylamine, n-octylamine, cyclohexylamine, and decylamine, as well as chlorine or bromine substituted alkylamines; aromatic amines such as aniline, toluidine, and naphthylamine, among which aniline and cyclohexylamine are preferred. These primary amines can be used alone or in combination of two or more. The amount of primary amine added is not particularly limited, and is preferably 0.7 to 1.1 molar equivalents relative to the dicarboxylic anhydride monomer unit, and more preferably 0.85 to 1.05 molar equivalents. If it is 0.7 molar equivalents or more relative to the dicarboxylic anhydride monomer unit in the maleimide copolymer, the thermal stability is good, so it is preferred. In addition, if it is 1.1 molar equivalents or less, the amount of primary amines remaining in the maleimide copolymer is reduced, so it is preferred.
[0059] When the maleimide monomer unit is introduced by the post-imidization method, in the reaction of ammonia or primary amine with the dicarboxylic anhydride monomer unit in the copolymer, especially in the reaction of converting the dicarboxylic anhydride monomer unit into the maleimide monomer unit, a catalyst may be used as needed for the purpose of improving the dehydration ring-closing reaction. The type of catalyst is not particularly limited, and for example, a tertiary amine can be used. As the tertiary amine, there is no particular limitation, and for example, trimethylamine, triethylamine, tripropylamine, tributylamine, N, N-dimethylaniline, N, N-diethylaniline can be cited. The amount of tertiary amine added is not particularly limited, and is preferably 0.01 molar equivalent or more relative to the dicarboxylic anhydride monomer unit. The temperature of the imidization reaction in the present invention is preferably 100 to 250°C, and more preferably 120 to 200°C. If the temperature of the imidization reaction is 100°C or more, the reaction rate is sufficiently fast, which is preferred from the perspective of productivity. If the temperature of the imidization reaction is 250°C or less, it is preferred to suppress the reduction in physical properties caused by thermal degradation of the maleimide copolymer.
[0060] When the post-imidization method is used for polymerization, the aromatic vinyl monomer, the cyanide vinyl monomer, and the unsaturated dicarboxylic anhydride monomer can also be all put into the polymerization at the initial stage of polymerization, but the alternating copolymerization of the aromatic vinyl monomer and the unsaturated dicarboxylic anhydride monomer is strong, so the aromatic vinyl monomer and the unsaturated dicarboxylic anhydride monomer will be consumed in the early stage of polymerization, and a copolymer with many cyanide vinyl monomer units is easily generated in the later stage of polymerization. As a result, the hue of the obtained maleimide copolymer sometimes deteriorates, or the composition distribution becomes larger, and the miscibility is insufficient when mixed with ABS resin, resulting in poor physical properties. Therefore, in order to obtain a maleimide copolymer with good hue and small composition distribution, it is preferably subjected to the following steps.
[0061] Initial polymerization step: The entire amount of the vinyl cyanide monomer, 10 to 90% by weight of the aromatic vinyl monomer, and 0 to 30% by weight of the unsaturated dicarboxylic acid anhydride monomer are mixed, added at the initial stage of polymerization, and copolymerization is initiated.
[0062] Mid-term polymerization process: the remaining amount of the aromatic vinyl monomer feed amount and the remaining amount of the unsaturated dicarboxylic anhydride monomer feed amount are added in batches or continuously, and the copolymerization is continued at the same time.
[0063] Final polymerization step: After all the unsaturated dicarboxylic acid anhydride monomers are added, 1 / 10 or more of the batch or continuous addition amount of the aromatic vinyl monomer is added to carry out polymerization.
[0064] Imidization step: The obtained copolymer having aromatic vinyl monomer units, vinyl cyanide monomer units and dicarboxylic anhydride monomer units is imidized with ammonia or a primary amine to obtain a maleimide copolymer.
[0065] The method for removing volatile components such as the solvent or unreacted monomers used in solution polymerization from the solution after the solution polymerization of the maleimide copolymer or the solution after the post-imidization (devolatilization method) can be a known method. For example, a vacuum devolatilization tank with a heater or a devolatilization extruder with an air outlet can be used. The maleimide copolymer in a molten state after devolatilization can be transferred to a granulation step, extruded in a linear form from a porous die head, and processed into granules by cold cutting, aerial hot cutting, or underwater hot cutting.
[0066] The maleimide copolymer thus obtained can be used as a heat resistance imparting agent for a resin composition obtained by kneading and mixing with various resins. The various resins are not particularly limited, and include ABS resin, ASA resin, AES resin, and SAN resin. Since the maleimide copolymer has excellent compatibility with these resins, a high heat resistance imparting effect can be obtained. The mixing ratio of the maleimide copolymer to these resins is preferably 5 to 40% by mass of the maleimide copolymer; 60 to 95% by mass of one or more resins selected from ABS resin, ASA resin, AES resin, and SAN resin, and more preferably 10 to 30% by mass of the maleimide copolymer; 70 to 90% by mass of one or more resins selected from ABS resin, ASA resin, AES resin, and SAN resin.
[0067] When the blending ratio of the maleimide-based copolymer is within this range, the effect of improving the heat resistance of the resin composition can be obtained without reducing the chemical resistance and hue of the resin composition.
[0068] The method for mixing the maleimide copolymer with various resins is not particularly limited, and known melt mixing techniques can be used. As suitable melt mixing devices, there are screw extruders such as single screw extruders, fully meshing co-rotating twin screw extruders, fully meshing counter-rotating twin screw extruders, non- or incompletely meshing twin screw extruders, Banbury mixers, kneaders, and mixing rolls.
[0069] When the maleimide copolymer is kneaded and mixed with these resins, a stabilizer, an ultraviolet absorber, a flame retardant, a plasticizer, a lubricant, glass fiber, an inorganic filler, a colorant, an antistatic agent, etc. may be further added.
[0070] The resin composition is suitable for use in injection-molded articles because of its excellent fluidity.
[0071] Examples of the injection molded body include housings / exterior materials for televisions, copiers, telephones, clocks, refrigerators, cleaners, air conditioners, washing machines, PCs, DVD / Blu-ray players, stereos, dryers, keyboards, tablet computers, digital cameras, briefcases, pachinko machines, home game consoles, and other electrical products, instrument boxes, instrument panels, registers, control switches, console boxes, bumper moldings, roof rails, emblems, instrument panel trims, electronic housings, wheel covers, wheel covers, fenders, door handles, door panels, Rearview mirrors, rear lamp covers, headlight covers, lamp covers, roof spoilers, rear spoilers, antenna covers, front grilles, radiator grilles, center consoles, car audio, car navigation, other automotive interior and exterior materials, carport parts, window frames, door covers, door handles, fence parts, system racks, drain plates, toilet seats, window frames, vanity panels, dressing tables, lattice fences, terrace platforms, benches and other residential parts, food trays, toys, sports equipment, furniture, musical instruments, semiconductor transport containers, plasma dust collection units and other daily necessities parts. Among them, it is suitable for automotive interior and exterior materials that require high heat resistance, and due to its excellent fluidity, it is suitable for large injection molded bodies such as lamp covers and spoilers.
[0072] Example
[0073] Hereinafter, the details will be described using examples, but the present invention is not limited to the following examples.
[0074] <Production Example of Maleimide Copolymer (A-1)>
[0075] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 20.3 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-1. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0076] <Production Example of Maleimide Copolymer (A-2)>
[0077] 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added to an autoclave with a capacity of about 120 liters equipped with a stirrer, and the gas phase was replaced with nitrogen, and then the temperature was raised to 92°C over 40 minutes under stirring. After the temperature was raised, a solution of 25 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added over 7 hours while maintaining 92°C. After the addition of maleic anhydride was completed, 2 parts by mass of styrene were continuously added over 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 17.7 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-2. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0078] <Production Example of Maleimide Copolymer (A-3)>
[0079] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 35 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 2 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 21.3 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-3. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0080] <Production Example of Maleimide Copolymer (A-4)>
[0081] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 24 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 13 parts by mass of styrene was continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 17.4 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-4. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0082] <Production Example of Maleimide Copolymer (A-5)>
[0083] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.8 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 19.8 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-5. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0084] <Production Example of Maleimide Copolymer (A-6)>
[0085] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.11 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 20.7 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-6. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0086] <Production Example of Maleimide Copolymer (A-7)>
[0087] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 17.2 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-7. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0088] <Production Example of Maleimide Copolymer (A-8)>
[0089] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 15 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 1 part by mass of styrene was continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 19.8 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-8. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0090] <Production Example of Maleimide Copolymer (B-1)>
[0091] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.01 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 20.3 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components to obtain pelletized maleimide copolymer B-1. Table 1 shows the analysis results of the obtained maleimide copolymer B-1.
[0092] <Production Example of Maleimide Copolymer (B-2)>
[0093] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.01 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised, a solution of 27 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours while maintaining 92°C. After the addition of maleic anhydride was completed, 10 parts by mass of styrene was continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 18.9 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components to obtain pelletized maleimide copolymer B-2. The analysis results of the obtained maleimide copolymer B-2 are shown in Table 1.
[0094] <Production Example of Maleimide Copolymer (B-3)>
[0095] 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added to an autoclave with a capacity of about 120 liters equipped with a stirrer, and the gas phase was replaced with nitrogen, and then the temperature was raised to 92°C over 40 minutes under stirring. After the temperature was raised, a solution of 20 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added over 7 hours while maintaining 92°C. After the addition of maleic anhydride was completed, 17 parts by mass of styrene was continuously added over 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 13.3 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components to obtain pelletized maleimide copolymer B-3. Table 1 shows the analysis results of the obtained maleimide copolymer B-3.
[0096] <Production Example of Maleimide Copolymer (B-4)>
[0097] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 16.6 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components to obtain pelletized maleimide copolymer B-4. The analysis results of the obtained maleimide copolymer B-4 are shown in Table 1.
[0098] <Production Example of Maleimide Copolymer (B-5)>
[0099] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.9 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 19.8 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components to obtain pelletized maleimide copolymer B-5. Table 2 shows the analysis results of the obtained maleimide copolymer B-5.
[0100] <Production Example of Maleimide Copolymer (B-6)>
[0101] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.9 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C over 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 27 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added over 7 hours. After the addition of maleic anhydride was completed, 10 parts by mass of styrene was continuously added over 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 18.4 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components to obtain pelletized maleimide copolymer B-6. Table 2 shows the analysis results of the obtained maleimide copolymer B-6.
[0102] <Production Example of Maleimide Copolymer (B-7)>
[0103] Into an autoclave with a capacity of about 120 liters equipped with a stirrer, 20 parts by mass of styrene, 10 parts by mass of acrylonitrile, 5 parts by mass of maleic anhydride, 0.1 parts by mass of tert-butyl peroxy-2-ethylhexanoate, 0.6 parts by mass of α-methylstyrene dimer, and 12 parts by mass of methyl ethyl ketone were added, and after replacing the gas phase with nitrogen, the temperature was raised to 92°C for 40 minutes under stirring. After the temperature was raised to 92°C, a solution of 31 parts by mass of maleic anhydride and 0.22 parts by mass of tert-butyl peroxy-2-ethylhexanoate dissolved in 75 parts by mass of methyl ethyl ketone and 28 parts by mass of styrene were continuously added for 7 hours. After the addition of maleic anhydride was completed, 6 parts by mass of styrene were continuously added for 2 hours. After the addition of styrene, the temperature was raised to 120°C, and the reaction was performed for 1 hour to complete the polymerization. Thereafter, 12.6 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization solution, and the reaction was performed at 140°C for 7 hours. The imidization reaction liquid after the reaction was completed was put into a vented screw extruder to remove volatile components, thereby obtaining pelletized maleimide copolymer A-1. Table 1 shows the analysis results of the obtained maleimide copolymer.
[0104] Table 1
[0105]
[0106] Table 2
[0107]
[0108] (Weight average molecular weight)
[0109] The weight average molecular weight is a polystyrene-equivalent value measured by gel permeation chromatography (GPC) under the following conditions.
[0110] Device name: SYSTEM-21Shodex (Showa Denko K.K.)
[0111] Column: 3 PL gel MIXED-B connected in series
[0112] Temperature: 40℃
[0113] Detection: Differential refractive index
[0114] Solvent:Tetrahydrofuran
[0115] Concentration: 2% by mass
[0116] Standard curve: drawn using standard polystyrene (PS) (manufactured by PL).
[0117] (Melt flow rate: MFR)
[0118] The melt mass flow rate was measured in accordance with JIS K 7210 under the conditions of 265° C. and 98N load.
[0119] (Glass transition temperature)
[0120] Glass Transition Temperature The glass transition midpoint temperature (Tmg) of the maleimide copolymer was measured using the following apparatus and measurement conditions in accordance with JIS K-7121.
[0121] Device name: Robot DSC6200 (manufactured by Seiko Instruments)
[0122] Heating rate: 10℃ / min
[0123] (Residual maleimide monomer amount)
[0124] Dissolve 0.5 g of the sample in 5 ml of a 1,2-dichloroethane solution (0.014 g / L) containing undecane (internal standard substance). Then, add 5 ml of n-hexane and oscillate it with an oscillator for 10 to 15 minutes to precipitate it. Inject only the supernatant into a gas chromatograph while the polymer is precipitated. Calculate the quantitative value based on the peak area of the obtained maleimide monomer using the coefficient obtained from the internal standard substance.
[0125] Device name: Gas chromatograph GC-2010 (manufactured by Shimadzu Corporation)
[0126] Column: Capillary column DB-5ms (manufactured by Agilent Technologies, Inc.)
[0127] Temperature: Inlet 280℃, Detector 280℃
[0128] Temperature increase analysis was performed at a column temperature of 80°C (initial stage).
[0129] (Temperature analysis conditions) 80°C: hold for 12 minutes
[0130] 80~280℃: Raise the temperature at 20℃ / min for 10 minutes
[0131] 280℃: hold for 10 minutes
[0132] Detector: FID
[0133] <Examples and Comparative Examples>
[0134] Examples 1 to 8, Comparative Examples 1 to 6 (Mixed and kneaded maleimide copolymer and ABS resin)
[0135] Maleimide copolymers A-1 to A-8 and B-1 to B-6, a generally commercially available maleimide copolymer "MS-NIP" (manufactured by Denka Co., Ltd.) without a cyanide vinyl monomer unit, and ABS resin "GR-3000" (manufactured by Denka Co., Ltd.) or ASA resin "Luran S 757G" (manufactured by INEOS Styrolution Co., Ltd.) were mixed in the proportions shown in Tables 3 and 4, and then extruded and pelletized using a twin-screw extruder (TEM-35B manufactured by Toshiba Machine Co., Ltd.). The pellets were used to make test pieces using an injection molding machine, and the values of various physical properties were measured. The results are shown in Tables 3 and 4.
[0136] Table 3
[0137]
[0138] Table 4
[0139]
[0140] (Charpy impact strength)
[0141] According to JIS K-7111, a notched test piece was used, and the impact direction was edge impact, and the measurement was performed at a relative humidity of 50% and an ambient temperature of 23° C. The measurement instrument used was a digital impact tester manufactured by Toyo Seiki Seisaku-sho., Ltd.
[0142] (Vicat softening point)
[0143] The test was conducted using a 10 mm x 10 mm, 4 mm thick test piece using the 50 method (load 50 N, heating rate 50°C / hour) according to JIS K7206. The HDT & VSPT tester manufactured by Toyo Seiki Seisaku-sho Co., Ltd. was used as the measuring instrument.
[0144] (Melt flow rate: MFR)
[0145] The measurement was performed at 220°C and a load of 98N in accordance with JIS K 7210.
[0146] (Chemical resistance)
[0147] The 1 / 4 ellipse method was used to observe cracks after 23°C and 48 hours with a specimen shape of 316×20×2mm, a long radius of 250mm, and a short radius of 150mm. In order to eliminate the influence of molding strain, the pellets were press-formed and cut at 260°C to produce the specimens. Toluene was used as the chemical reagent.
[0148] In addition, the critical strain was obtained using the following formula.
[0149] ε=b / 2a 2 {1-(a 2 -b 2 )X 2 / a 4} 1.5 ×t×100
[0150] Critical strain: ε, long radius: a, short radius: b, specimen thickness: t, crack occurrence point: X
[0151] The chemical resistance was evaluated based on the critical strain according to the following criteria.
[0152] ◎: 0.8 or more, ○: 0.6 to 0.7, △: 0.3 to 0.5, ×: 0.2 or less
[0153] As shown in Examples 1 to 8, the maleimide copolymers of A-1 to A-8 of the present invention achieve high glass transition temperature and high melt mass flow rate by reducing the weight average molecular weight without reducing the content of maleimide monomer units in the composition. However, as shown in Comparative Examples 5 and 6, if the weight average molecular weight is reduced by more than a certain amount, reduced heat resistance and reduced chemical resistance are observed. The maleimide copolymers of B-1 to B-6 that do not meet the scope of the present invention are not within the scope of the present invention, and the resin compositions of Comparative Examples 1 to 6 obtained by mixing these maleimide copolymers with ABS resin have poor impact resistance, fluidity, heat resistance, and chemical resistance.
[0154] Industrial Applicability
[0155] The maleimide copolymer of the present invention can obtain a resin composition having an excellent balance of physical properties such as chemical resistance, heat resistance, impact resistance and fluidity by kneading and mixing compatible ABS resin, ASA resin, AES resin and SAN resin, and can improve the fluidity of the mixed resin, thereby achieving high-speed molding and improved production speed.
Claims
1. A maleimide copolymer, which is composed of an aromatic vinyl monomer unit, a cyanide vinyl monomer unit, and a maleimide monomer unit, has a glass transition temperature of 165° C. to 200° C., and a melt mass flow rate of 25 to 80 g / 10 min. at 265° C. and a load of 98 N as measured by the method described in JIS K 7210, wherein the amount of the cyanide vinyl monomer unit contained in the maleimide copolymer is 7 to 20% by mass, and the weight average molecular weight of the maleimide copolymer is 50,000 to 100,000. 2 . The maleimide copolymer according to claim 1 , comprising 40 to 59.5% by mass of an aromatic vinyl monomer unit, 7 to 20% by mass of a vinyl cyanide monomer unit, and 35 to 50% by mass of a maleimide monomer unit. 3 . The maleimide-based copolymer according to claim 1 , further comprising 0.5 to 10% by mass of a dicarboxylic anhydride monomer unit. 4 .
4. The maleimide-based copolymer according to any one of claims 1 to 3, wherein The content of residual maleimide monomer is less than 300 ppm.
5. The method for producing the maleimide copolymer according to any one of claims 1 to 4, comprising the following steps: Initial polymerization step: mixing the entire amount of vinyl cyanide monomer, 10 to 90% by weight of aromatic vinyl monomer, and 0 to 30% by weight of unsaturated dicarboxylic anhydride monomer to initiate copolymerization; Mid-term polymerization step: adding 50-90% by weight of the remaining aromatic vinyl monomer and all of the remaining unsaturated dicarboxylic anhydride monomer in batches or continuously, and continuing copolymerization; Final polymerization step: adding all the remaining amount of the aromatic vinyl monomer to obtain a copolymer having aromatic vinyl monomer units, vinyl cyanide monomer units and dicarboxylic anhydride monomer units; and In the imidization step, the dicarboxylic anhydride monomer units of the obtained copolymer are imidized into maleimide monomer units using ammonia or a primary amine.
6. A resin composition comprising 5 to 40% by weight of the maleimide copolymer according to any one of claims 1 to 4 and 60 to 95% by weight of a resin, wherein the resin is one or more selected from acrylonitrile-butadiene-styrene copolymer resin, acrylonitrile-styrene-acrylic rubber copolymer resin, acrylonitrile-ethylene / propylene rubber-styrene copolymer resin or styrene-acrylonitrile copolymer resin.
7. An injection molded product using the resin composition according to claim 6.
8. The injection molded article according to claim 7, which is used as an interior part or exterior part of an automobile.