A solar cell and a method for preparing the same

By introducing specific materials and processes into perovskite solar cells, the problems of insufficient stability and efficiency have been solved, achieving high efficiency and stability, and promoting their widespread application.

CN113838979BActive Publication Date: 2024-11-15NINGBO OSDA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110899357.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-06
Publication Date
2024-11-15
Estimated Expiration
2041-08-06

AI Technical Summary

Technical Problem

Perovskite solar cells suffer from problems with instability and insufficient conversion efficiency.

Method used

Solar cells are fabricated using specific materials and processes, including FTO conductive glass, Spiro-OMeTAD hole transport layer, perovskite absorber layer doped with polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide, Ni, Sn, La, Nb nano-precursor electron transport layer, and Ag or Al metal counter electrode. The stability and efficiency are improved by designing interface modification layers.

Benefits of technology

It significantly improves the stability and conversion efficiency of perovskite solar cells, enhances the interfacial conductivity and electron mobility of the cells, reduces defect density, and promotes the effective extraction and transport of charge.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a solar cell and a preparation method thereof, which comprises, from top to bottom, a conductive substrate, a hole transport layer, a perovskite light absorption layer, an interface modification layer, an electron transport layer and a metal counter electrode; the conductive substrate is one of FTO conductive glass, ITO conductive glass or AZO conductive glass; the hole transport layer is a Spiro-OMeTAD hole transport layer; the perovskite absorption layer is a perovskite absorption layer obtained by reacting methylamine iodine, PbI2, methylamine acetate (MAAc), polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide; the interface modification layer is a mixed layer of 2-naphthalenethiol, a silane coupling agent and tungsten phosphate; the electron transport layer is an electron transport layer obtained by reacting Ni, Sn, La, Nb nano-precursors and protonated ethanolamine; the metal counter electrode is Ag or Al. By modifying the electron transport layer, the perovskite absorption layer and the interface, the efficiency and stability thereof are significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery preparation, and in particular to a solar cell and a preparation method thereof. Background Art

[0002] At present, with the continuous growth of the world's population, the continuous innovation of industry and information technology, the demand and consumption of energy in human society are increasing day by day. The development and utilization of diversified and clean renewable energy has attracted widespread attention from countries around the world. Different from traditional energy sources such as coal, oil, and natural gas, solar energy, as the most abundant energy resource in the world, has become the focus of new energy with its advantages of cleanliness, renewableness, and inexhaustible supply. Solar cells are a new green technology that converts solar energy into electrical energy on a large scale. The development of solar cells can alleviate environmental pollution, solve the crisis of traditional energy, and promote the development of sustainable energy. Among them, crystalline silicon solar cells have made significant progress in conversion efficiency and preparation cost, and have occupied most of the application market. However, its high price limits the widespread application of silicon cells. At present, silicon solar cells, which dominate the commercial solar cell market, still cannot meet the requirements of low cost.

[0003] Solar cells with organic metal halides with perovskite crystal structure as light-absorbing layers (abbreviated as perovskite solar cells) that appeared in 2009 have developed rapidly in recent years. In 2013, their laboratory photoelectric conversion efficiency reached 15%, and is expected to exceed 20% in the next few years. Its high efficiency and low cost make it the new solar cell with the greatest market potential. Perovskite solar cells are composed of transparent conductive electrodes, electron transport layers, perovskite structure light-absorbing layers, hole transport layers and positive electrodes. Although there are many related studies and reports on perovskite solar cells, perovskite solar cells are still facing a series of problems that need to be solved urgently, among which stability is the core problem. It is of practical significance to study their stability and efficiency improvement. Summary of the invention

[0004] The purpose of the present invention is to provide a new type of solar cell and a preparation method thereof in view of the shortcomings of stability, conversion efficiency, etc. of perovskite solar cells in the prior art. By modifying the electron transport layer, the perovskite absorption layer and the interface, the efficiency and stability are significantly improved, which is conducive to its further application.

[0005] In order to achieve the above purpose, this application adopts the following technical solutions:

[0006] A solar cell comprises, from top to bottom, a conductive substrate, a hole transport layer, a perovskite light absorption layer, an interface modification layer, an electron transport layer and a metal counter electrode; the conductive substrate is one of FTO conductive glass, ITO conductive glass or AZO conductive glass; the hole transport layer is a Spiro-OMeTAD hole transport layer; the perovskite absorption layer is a perovskite absorption layer doped with polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide, wherein the perovskite absorption layer is prepared by reacting methylamine iodine and Pb I2 is dissolved in methylamine acetate (MAAc), polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide are added to prepare a precursor mixture, the precursor mixture is coated on the hole transport layer, and annealed on a heating plate to obtain a perovskite absorption layer; the electron transport layer is prepared by preparing Ni, Sn, La, and Nb nano precursors, and protonated ethanolamine is added to form a dispersed solution, the dispersed solution is coated on the surface of the interface modification layer, and annealed to obtain an electron transport layer; the metal counter electrode is Ag or Al.

[0007] Preferably, the thickness of the hole transport layer is 30-40 nm, the thickness of the perovskite light absorption layer is 650-900 nm; the thickness of the interface modification layer is 10-30 nm; the thickness of the electron transport layer is 40-60 nm; and the thickness of the metal counter electrode is 60-70 nm.

[0008] The above-mentioned method for preparing a solar cell comprises the following steps:

[0009] S1: Cleaning the conductive substrate;

[0010] S2: preparing a hole transport layer: ultrasonically spin coating the Spiro-OMeTAD solution on the surface of the conductive substrate obtained in step S1, annealing, and naturally cooling to room temperature to form a Spiro-OMeTAD hole transport layer;

[0011] S3: preparing a perovskite absorption layer: dissolving methylamine iodine and PbI2 in methylamine acetate, adding polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide to prepare a precursor mixture; coating the precursor mixture on the hole transport layer in step S2, and annealing on a heating plate to obtain a perovskite absorption layer;

[0012] S4: Preparation of interface modification layer: 2-naphthalenethiol, silane coupling agent and tungsten phosphate are prepared into a mixed solution, and ultrasonically spin-coated on the surface of the perovskite absorption layer obtained in step S3, and annealed to obtain the interface modification layer;

[0013] S5: Preparation of electron transport layer: preparing Ni, Sn, La and Nb nano-precursors, and adding protonated ethanolamine to form a dispersed solution; coating the dispersed solution on the surface of the interface modification layer obtained in step S4, and annealing to obtain an electron transport layer;

[0014] S6: Evaporating Ag or Al counter electrode on the surface of the electron transport layer obtained in step S5 to obtain a perovskite solar cell.

[0015] Preferably, the specific steps of cleaning the conductive substrate in step S1 are: ultrasonically cleaning the conductive substrate with detergent, deionized water, acetone, anhydrous ethanol, and isopropanol for 20-30 minutes each, and then drying it in a vacuum drying oven at 75-85°C; then drying it with N2 and treating it with a UV ozone cleaner for 10-15 minutes.

[0016] Preferably, the specific steps for preparing the hole transport layer in step S2 are: mixing 4-tert-butylpyridine, Li-TFSI and chlorobenzene in a volume ratio of 1-3:2-5:100 to obtain a mixed solution A, and then adding Spiro-OMeTAD, with a solid-liquid ratio of 1:50-70; stirring until completely dissolved to obtain a Spiro-OMeTAD solution, ultrasonically spin coating the surface of the conductive substrate obtained in step S1, annealing at a temperature of 80-100°C for 5-10 minutes, and naturally cooling to room temperature to form a Spiro-OMeTAD hole transport layer.

[0017] Preferably, the specific steps of preparing the perovskite absorption layer in step S3 are: dissolving 6-10 parts of methylamine iodine and 5-15 parts of PbI2 in 40-60 parts of methylamine acetate (MAAc) and stirring thoroughly; raising the temperature to 40-60°C, adding 2-5 parts of polyethylene oxide silicone oil, and stirring at a rate of 500-800r / min for 5-10min; then adding 3-7 parts of 1-aminoethyl-3-methylimidazolium bromide, stirring at a rate of 500-800r / min for 10-20min to obtain a precursor mixture; spin coating the precursor mixture at a speed of 1000-2000rpm for 10-20s on the hole transport layer in step S2, and then spin coating the hole transport layer in step S2 at a speed of 4000-6000rpm for 20-30s, and annealing on a hot plate at a temperature of 100-120°C for 40-60min to obtain a perovskite absorption layer.

[0018] Preferably, the specific steps for preparing the interface modification layer in step S4 are: mixing 3-6 parts of 2-naphthalenethiol, 2-7 parts of silane coupling agent and 5-10 parts of tungsten phosphate, stirring and mixing at a rate of 1000-2000 rpm, and ultrasonically spin coating on the surface of the perovskite absorption layer obtained in step S3, and annealing at a temperature of 60-80°C for 10-20 minutes to obtain the interface modification layer.

[0019] Preferably, the specific steps of preparing the electron transport layer in step S5 are: mixing Ni powder, Sn powder, La2O3 and Nb2O5 powder to obtain a mixed solid A; then adding it to anhydrous ethanol solution, the solid-to-liquid ratio of the two is 1:30-40; wherein the molar ratio of Ni, Sn, La and Nb is 1:(1.05-1.2):(0.2-0.4):(0.8-1.3); heating to 60-80°C, adding H2O2 solution, the mixed solid A and H2O2 The solid-liquid ratio of the solution is 1:8-12. After stirring for 10-15 minutes, an ammonia solution is added dropwise, wherein the liquid-solid ratio of the ammonia solution to the mixed solid A is 0.3-0.6:1, and the solution is aged for 3-6 hours to obtain a precipitate. 30-50 parts of the precipitate and 6-10 parts of protonated ethanolamine are added to 50-70 parts of ethanol solution to form a dispersion, and the dispersion is applied to the surface of the interface modification layer obtained in step S4, and annealed at a temperature of 100-120° C. for 15-25 minutes to obtain an electron transport layer.

[0020] Preferably, the specific steps of step S6 are: vacuum evaporating Ag or Al counter electrode on the surface of the electron transport layer obtained in step S5.

[0021] Beneficial effects:

[0022] 1. In the preparation of the perovskite absorption layer, the present invention introduces long-chain polymer polyethylene oxide silicone oil, which can effectively block the penetration of water and oxygen in the air and improve the stability of the battery; the lone pair of electrons of -NH2 in 1-aminoethyl-3-methylimidazolium bromide is used to react with the unsaturated Pb 2+ The defects are combined with covalent Pb-N bonds, which reduces the defect density and inhibits charge recombination. At the same time, due to the presence of Pb-N coordination bonds and long-chain polymers, the alkyl chains in the ionic liquid are almost vertically distributed along the surface of the perovskite, and the stability is well improved. At the same time, under the synergistic effect of the ionic liquid and methylamine acetate, the solubility of the solution is improved, the crystallization degree of the perovskite light-absorbing layer is increased, and the battery efficiency is improved.

[0023] 2. The present invention introduces a mixed component of Ni, Sn, La2O3, and Nb in the preparation of the electron transport layer, which has high electron mobility and electron transport energy, can reduce the recombination of interfacial charges at the interface, and thus improve battery performance and stability; the protonated EA+ in the molecule contacts the perovskite more effectively, the electron extraction speed is accelerated, the accumulated charge on the interface is released, and the battery efficiency is improved.

[0024] 3. The present invention introduces an interface modification layer between the perovskite absorption layer and the electron transport layer, and utilizes the synergistic effect of double-end groups such as 2-naphthalenethiol, silane coupling agent, and tungsten phosphate to allow sulfur-containing, oxygen-containing, and other groups to interact with the transport layer to passivate the surface of the transport layer; the electron-donating group end interacts with the perovskite active layer to improve the interface conductivity, passivate the surface defects of the perovskite active layer, and to a certain extent inhibit the ion migration in the perovskite active layer, thereby improving the battery stability.

[0025] 4. The present invention improves the perovskite absorption layer, interface modification layer and electron transport layer. Under the joint action of polyethylene oxide silicone oil, 1-aminoethyl-3-methylimidazolium bromide, 2-naphthalenethiol, silane coupling agent, etc., the surface of the perovskite active layer is passivated, the defect density is greatly reduced, the charge recombination is suppressed, and the battery stability is improved; under the action of Ni, Sn, La2O3, Nb, protonated ethanolamine, methylamine acetate, 2-naphthalenethiol, phosphotungstic acid, silane coupling agent, etc., the electron mobility and electron transport capacity are improved, the crystallinity of the perovskite light absorption layer is improved, and then the battery efficiency is improved, which is conducive to its wider application. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with the following embodiments, which are only used to illustrate the present invention but not to limit the present invention. Example 1

[0027] S1: Clean the conductive substrate; ultrasonically clean the conductive substrate with detergent, deionized water, acetone, anhydrous ethanol, and isopropanol for 20 minutes each, and then dry it in a vacuum drying oven at 75°C; then blow dry it with N2 and treat it in a UV ozone cleaning machine for 10 minutes;

[0028] S2: Preparation of hole transport layer: 1 ml of 4-tert-butylpyridine, 2 ml of Li-TFSI and 100 ml of chlorobenzene were mixed to obtain a mixed solution A, and then 2 g of Spiro-OMeTAD was added; the mixture was stirred until completely dissolved to obtain a Spiro-OMeTAD solution, and the solution was ultrasonically spin-coated on the surface of the conductive substrate obtained in step S1, annealed at 80°C for 5 min, and naturally cooled to room temperature to form a Spiro-OMeTAD hole transport layer;

[0029] S3: Preparation of perovskite absorption layer: 6g of methylamine iodine and 5g of PbI2 are dissolved in 40ml of methylamine acetate (MAAc) and stirred thoroughly; the temperature is raised to 40°C, 2g of polyethylene oxide silicone oil is added, and stirred at a rate of 500r / min for 5min; then 3g of 1-aminoethyl-3-methylimidazolium bromide is added, and stirred at a rate of 500r / min for 10min to obtain a precursor mixture; the precursor mixture is spin-coated on the hole transport layer described in step S2 at a rotation speed of 1000rpm for 10s, and then spin-coated on the hole transport layer described in step S2 at a rotation speed of 4000rpm for 20s, and annealed on a hot plate at a temperature of 100°C for 40min to obtain a perovskite absorption layer;

[0030] S4: Preparation of interface modification layer: 3 g of 2-naphthalenethiol, 2 g of silane coupling agent and 5 g of tungsten phosphate were mixed, stirred and mixed at a rate of 1000 rpm, and ultrasonically spin-coated on the surface of the perovskite absorption layer obtained in step S3, and annealed at a temperature of 60° C. for 10 min to obtain an interface modification layer;

[0031] S5: Preparation of electron transport layer: Ni powder, Sn powder, La2O3 and Nb2O5 powder are mixed to obtain a mixed solid A, wherein the molar ratio of Ni, Sn, La and Nb is 1:1.05:0.2:0.8; 3g of the mixed solid A is added to 90ml of anhydrous ethanol solution, the temperature is raised to 60°C, 24ml of H2O2 solution is added, and after stirring for 10min, 0.9ml of ammonia solution is added dropwise, and the mixture is aged for 3h to obtain a precipitate; 30g of the precipitate and 6g of protonated ethanolamine are added to 50ml of ethanol solution to form a dispersion, and the dispersion is applied to the surface of the interface modification layer obtained in step S4, and annealed at 100°C for 15min to obtain an electron transport layer;

[0032] S6: vapor-depositing a Ag counter electrode on the surface of the electron transport layer obtained in step S5 to obtain a perovskite solar cell. Example 2

[0033] S1: Clean the conductive substrate; ultrasonically clean the conductive substrate with detergent, deionized water, acetone, anhydrous ethanol, and isopropanol for 30 minutes each, and then dry it in a vacuum drying oven at 85°C; then blow dry it with N2 and treat it in a UV ozone cleaning machine for 15 minutes;

[0034] S2: Preparation of hole transport layer: 3 ml of 4-tert-butylpyridine, 5 ml of Li-TFSI and 100 ml of chlorobenzene were mixed to obtain a mixed solution A, and then 1.5 g of Spiro-OMeTAD was added; the mixture was stirred until completely dissolved to obtain a Spiro-OMeTAD solution, and ultrasonically spin-coated on the surface of the conductive substrate obtained in step S1, annealed at 100°C for 10 min, and naturally cooled to room temperature to form a Spiro-OMeTAD hole transport layer;

[0035] S3: Prepare the perovskite absorption layer: dissolve 10g of methylamine iodine and 15g of PbI2 in 60ml of methylamine acetate (MAAc) and stir thoroughly; raise the temperature to 60°C, add 5g of polyethylene oxide silicone oil, and stir at a rate of 800r / min for 10min; then add 7g of 1-aminoethyl-3-methylimidazolium bromide, and stir at a rate of 800r / min for 20min to obtain a precursor mixture; spin-coat the precursor mixture on the hole transport layer described in step S2 at a speed of 2000rpm for 20s, and then spin-coat the hole transport layer described in step S2 at a speed of 6000rpm for 30s, and anneal on a hot plate at a temperature of 120°C for 60min to obtain a perovskite absorption layer;

[0036] S4: Preparation of interface modification layer: 6 g of 2-naphthalenethiol, 7 g of silane coupling agent and 10 g of tungsten phosphate were mixed, stirred and mixed at a rate of 2000 rpm, and ultrasonically spin-coated on the surface of the perovskite absorption layer obtained in step S3, and annealed at a temperature of 80° C. for 20 min to obtain an interface modification layer;

[0037] S5: Preparation of electron transport layer: Ni powder, Sn powder, La2O3 and Nb2O5 powder are mixed to obtain a mixed solid A, wherein the molar ratio of Ni, Sn, La and Nb is 1:1.2:0.4:1.3; 3 g of the mixed solid A is added to 120 ml of anhydrous ethanol solution, the temperature is raised to 80°C, 36 ml of H2O2 solution is added, 1.8 ml of ammonia solution is added dropwise after stirring for 15 min, and the mixture is aged for 6 h to obtain a precipitate; 50 g of the precipitate and 10 g of protonated ethanolamine are added to 70 ml of ethanol solution to form a dispersion, the dispersion is coated on the surface of the interface modification layer obtained in step S4, and annealed at 120°C for 25 min to obtain an electron transport layer;

[0038] S6: Vapor-depositing an Al counter electrode on the surface of the electron transport layer obtained in step S5 to obtain a perovskite solar cell. Example 3

[0039] S1: Clean the conductive substrate; ultrasonically clean the conductive substrate with detergent, deionized water, acetone, anhydrous ethanol, and isopropanol for 25 minutes each, and then dry it in a vacuum drying oven at 80°C; then blow dry it with N2 and treat it in a UV ozone cleaning machine for 12 minutes;

[0040] S2: Preparation of hole transport layer: 2 ml of 4-tert-butylpyridine, 3 ml of Li-TFSI and 100 ml of chlorobenzene were mixed to obtain a mixed solution A, and then 1.6 g of Spiro-OMeTAD was added and stirred until completely dissolved to obtain a Spiro-OMeTAD solution, which was ultrasonically spin-coated on the surface of the conductive substrate obtained in step S1, annealed at 90°C for 7 min, and naturally cooled to room temperature to form a Spiro-OMeTAD hole transport layer;

[0041] S3: Preparation of perovskite absorption layer: 8g of methylamine iodine and 12g of PbI2 are dissolved in 55ml of methylamine acetate (MAAc) and stirred thoroughly; the temperature is raised to 50°C, 4g of polyethylene oxide silicone oil is added, and stirred at a rate of 700r / min for 8min; then 5g of 1-aminoethyl-3-methylimidazolium bromide is added, and stirred at a rate of 650r / min for 15min to obtain a precursor mixture; the precursor mixture is spin-coated on the hole transport layer described in step S2 at a rotation speed of 1500rpm for 15s, and then spin-coated on the hole transport layer described in step S2 at a rotation speed of 5000rpm for 25s, and annealed on a hot plate at a temperature of 110°C for 50min to obtain a perovskite absorption layer;

[0042] S4: Preparation of interface modification layer: 5 g of 2-naphthalenethiol, 5 g of silane coupling agent and 7 g of tungsten phosphate were mixed, stirred and mixed at a rate of 1800 rpm, and ultrasonically spin-coated on the surface of the perovskite absorption layer obtained in step S3, and annealed at a temperature of 70° C. for 15 min to obtain an interface modification layer;

[0043] S5: Preparation of electron transport layer: Ni powder, Sn powder, La2O3 and Nb2O5 powder are mixed to obtain a mixed solid A, wherein the molar ratio of Ni, Sn, La and Nb is 1:1.1:0.3:1.0; 3 g of the mixed solid A is added to 105 ml of anhydrous ethanol solution, heated to 70°C, 30 ml of H2O2 solution is added, stirred for 12 min, 1.5 ml of ammonia solution is added dropwise, and aged for 5 h to obtain a precipitate; 40 g of the precipitate and 8 g of protonated ethanolamine are added to 65 g of ethanol solution to form a dispersion, the dispersion is coated on the surface of the interface modification layer obtained in step S4, and annealed at 110°C for 20 min to obtain an electron transport layer;

[0044] S6: vapor-depositing a Ag counter electrode on the surface of the electron transport layer obtained in step S5 to obtain a perovskite solar cell.

[0045] Comparative Example 1

[0046] The difference from Example 1 is that long-chain high molecular weight polyethylene oxide silicone oil is not added in step S3, and other steps and conditions remain unchanged.

[0047] Comparing Comparative Example 1 with Example 1, it can be seen that due to the lack of high molecular weight polyethylene oxide silicone oil, the penetration of water and oxygen in the air cannot be blocked, and the battery stability is reduced.

[0048] Comparative Example 2

[0049] The difference from Example 1 is that 1-aminoethyl-3-methylimidazolium bromide is not added in step S3, and other steps and conditions remain unchanged.

[0050] Comparison of Comparative Example 2 and Example 1 shows that due to the lack of 1-aminoethyl-3-methylimidazolium bromide, the lone pair of electrons of -NH2 cannot react with the unsaturated Pb 2+ The defects are combined by covalent bonds Pb-N, the defect density is large, the charges are prone to recombination, and the battery stability is significantly reduced.

[0051] Comparative Example 3

[0052] The difference from Example 1 is that no silane coupling agent is added in step S4, and other steps and conditions remain unchanged.

[0053] Comparative Example 4

[0054] The difference from Example 1 is that 2-naphthalenethiol is not added in step S4, and other steps and conditions remain unchanged.

[0055] By comparing Comparative Example 3, Comparative Example 4 and Example 1, it can be seen that due to the lack of one of the three, the double-end groups fail to fully exert the synergistic effect, the surface passivation effect of the electron transport layer and the perovskite active layer is limited, and the battery stability is reduced.

[0056] Comparative Example 5

[0057] The difference from Example 1 is that intramolecular protonated EA+ is not added in step S5, and other steps and conditions remain unchanged.

[0058] By comparing Comparative Example 5 with Example 1, it can be seen that due to the lack of intramolecular protonated EA+, the electron extraction rate is slow when in contact with perovskite, and the battery efficiency is reduced.

[0059] Comparative Example 6

[0060] The difference from Example 1 is that Ni and La2O3 are not added in step S5, and other steps and conditions remain unchanged.

[0061] Comparing Comparative Example 6 with Example 1, it can be seen that the lack of Ni and La2O3 reduces the electron mobility and electron transport energy, and the performance of the device decreases when it is exposed to air.

[0062] Performance testing method:

[0063] The electrical properties of each embodiment and comparative example were tested, and the solar simulator was turned on and the light intensity was set to 100 mw / cm 2 , place the solar cell in the center of the light spot, connect the solar cell to the IC tester for testing; the electrical data obtained are as follows:

[0064] experiment <![CDATA[Short-circuit current ISC (mA / cm 2 )]]> Open circuit voltage VOC (V) Filling factor FF (%) Conversion efficiency (%) Stability: Unpackaged, time required for photoelectric efficiency to decay by 20% (h) Example 1 26.6 0.93 84.3 20.5 305 Example 2 27.3 0.94 86.7 20.8 330 Example 3 28.1 0.95 88.3 21.3 350 Comparative Example 1 25.3 0.89 80.3 19.2 290 Comparative Example 2 23.2 0.86 78.1 17.3 180 Comparative Example 3 24.2 0.88 81.2 18.3 285 Comparative Example 4 23.9 0.87 79.4 17.5 270 Comparative Example 5 24.1 0.89 80.3 17.8 280 Comparative Example 6 24.2 0.88 80.5 18.2 283

[0065] The above description is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiment. Any equivalent modifications or changes made by ordinary technicians in this field based on the contents disclosed by the present invention should be included in the protection scope recorded in the claims.

Claims

1. A solar cell, characterized in that: The invention comprises, from top to bottom, a conductive substrate, a hole transport layer, a perovskite absorption layer, an interface modification layer, an electron transport layer and a metal counter electrode; the conductive substrate is one of FTO conductive glass, ITO conductive glass or AZO conductive glass; the hole transport layer is a Spiro-OMeTAD hole transport layer; the perovskite absorption layer is a perovskite absorption layer doped with polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide, wherein the perovskite absorption layer is prepared by dissolving methylamine iodine and PbI2 in methylamine acetate (MAAc), adding Polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide are configured to obtain a precursor mixture, which is coated on a hole transport layer and annealed on a heating plate to obtain a perovskite absorption layer; the interface modification layer is a mixed layer of 2-naphthalenethiol, a silane coupling agent, and tungsten phosphate; the electron transport layer is prepared by preparing Ni, Sn, La, and Nb nano precursors, and adding protonated ethanolamine to form a dispersed solution, which is coated on the surface of the interface modification layer and annealed to obtain an electron transport layer; the metal counter electrode is Ag or Al.

2. A solar cell according to claim 1, characterized in that: The thickness of the hole transport layer is 30-40 nm, the thickness of the perovskite absorption layer is 650-900 nm; the thickness of the interface modification layer is 10-30 nm; the thickness of the electron transport layer is 40-60 nm; and the thickness of the metal counter electrode is 60-70 nm.

3. The method for preparing a solar cell according to claim 1, characterized in that: The following steps are included: S1: Cleaning the conductive substrate; S2: preparing a hole transport layer: ultrasonically spin coating the Spiro-OMeTAD solution on the surface of the conductive substrate obtained in step S1, annealing, and naturally cooling to room temperature to form a Spiro-OMeTAD hole transport layer; S3: preparing a perovskite absorption layer: dissolving methylamine iodine and PbI2 in methylamine acetate (MAAc), adding polyethylene oxide silicone oil and 1-aminoethyl-3-methylimidazolium bromide to prepare a precursor mixture; coating the precursor mixture on the hole transport layer in step S2, and annealing on a heating plate to obtain a perovskite absorption layer; S4: Preparation of interface modification layer: 2-naphthalenethiol, silane coupling agent and tungsten phosphate are prepared into a mixed solution, and ultrasonically spin-coated on the surface of the perovskite absorption layer obtained in step S3, and annealed to obtain the interface modification layer; S5: Preparation of electron transport layer: preparing Ni, Sn, La, Nb nano precursors, and adding protonated ethanolamine to form a dispersed solution; coating the dispersed solution on the surface of the interface modification layer obtained in step S4, and annealing to obtain an electron transport layer; S6: Evaporating Ag or Al counter electrode on the surface of the electron transport layer obtained in step S5 to obtain a perovskite solar cell.

4. The method for preparing a solar cell according to claim 3, characterized in that: The specific steps of cleaning the conductive substrate in step S1 are: ultrasonically clean the conductive substrate with detergent, deionized water, acetone, anhydrous ethanol, and isopropanol for 20-30 minutes each, and then dry it in a vacuum drying oven at 75-85°C; then blow dry it with N2 and treat it with a UV ozone cleaner for 10-15 minutes.

5. The method for preparing a solar cell according to claim 3, characterized in that: The specific steps for preparing the hole transport layer in step S2 are: 4-tert-butylpyridine, Li-TFSI and chlorobenzene are mixed in a volume ratio of 1-3:2-5:100 to obtain a mixed solution A, and then Spiro-OMeTAD is added, and the solid-liquid ratio of the two is 1:50-70; stirring until completely dissolved to obtain a Spiro-OMeTAD solution, ultrasonically spin-coating the surface of the conductive substrate obtained in step S1, annealing at a temperature of 80-100°C for 5-10 minutes, and naturally cooling to room temperature to form a Spiro-OMeTAD hole transport layer.

6. The method for preparing a solar cell according to claim 3, characterized in that: The specific steps of preparing the perovskite absorption layer in step S3 are as follows: dissolving 6-10 parts of methylamine iodine and 5-15 parts of PbI2 in 40-60 parts of methylamine acetate (MAAc) and stirring thoroughly; raising the temperature to 40-60°C, adding 2-5 parts of polyethylene oxide silicone oil, and stirring at a rate of 500-800r / min for 5-10min; then adding 3-7 parts of 1-aminoethyl-3-methylimidazolium bromide, stirring at a rate of 500-800r / min for 10-20min to obtain a precursor mixture; spin coating the precursor mixture at a speed of 1000-2000rpm for 10s on the hole transport layer in step S2, and then spin coating the hole transport layer in step S2 at a speed of 4000-6000rpm for 20 seconds, and annealing on a hot plate at a temperature of 100-120°C for 40-60min to obtain a perovskite absorption layer.

7. The method for preparing a solar cell according to claim 3, characterized in that: The specific steps of preparing the interface modification layer in step S4 are: mixing 3-6 parts of 2-naphthalenethiol, 2-7 parts of silane coupling agent and 5-10 parts of tungsten phosphate, stirring and mixing at a rate of 1000-2000 rpm, and ultrasonically spin coating on the surface of the perovskite absorption layer obtained in step S3, and annealing at a temperature of 60-80°C for 10-20 minutes to obtain the interface modification layer.

8. The method for preparing a solar cell according to claim 3, characterized in that: The specific steps of preparing the electron transport layer in step S5 are: mixing Ni powder, Sn powder, La2O3 and Nb2O5 powder to obtain a mixed solid A; then adding it to anhydrous ethanol solution, the solid-liquid ratio of the two is 1:30-40; wherein the molar ratio of Ni, Sn, La and Nb is 1:(1.05-1.2):(0.2-0.4):(0.8-1.3); heating to 60-80°C, adding H2O2 solution, the mixed solid A and H2O2 solution The solid-liquid ratio is 1:8-12, and after stirring for 10-15 minutes, an ammonia solution is added dropwise, wherein the liquid-solid ratio of the ammonia solution to the mixed solid A is 0.3-0.6:1, and the mixture is aged for 3-6 hours to obtain a precipitate; 30-50 parts of the precipitate and 6-10 parts of protonated ethanolamine are added to 50-70 parts of ethanol solution to form a dispersion, and the dispersion is applied to the surface of the interface modification layer obtained in step S4, and annealed at a temperature of 100-120°C for 15-25 minutes to obtain an electron transport layer.

9. The method for preparing a solar cell according to claim 3, characterized in that: The specific steps of step S6 are: vacuum evaporating Ag or Al counter electrode on the surface of the electron transport layer obtained in step S5.