Forward osmosis membrane, forward osmosis membrane assembly and method for manufacturing the same

By forming a polymer separation active layer on the surface of the microporous support membrane of the positive permeability membrane, and combining heat treatment and interface polymerization, the problem of difficult to take into account both the water permeability and the reverse diffusion of salt in high concentration concentration in the prior art is solved. , achieving high efficiency, stability and durability of the membrane.

CN113905807BActive Publication Date: 2024-11-26ASAHI KASEI KOGYO KABUSHIKI KAISHA

Patent Information

Application Number
CN202080039655.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-31
Filing Date
2020-05-29
Publication Date
2024-11-26
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

It is difficult to take into account the high water permeability and low salt reverse diffusion during the high concentration concentration process, and the membrane performance is easily reduced during multiple uses, resulting in physical damage and durability problems.

Method used

Develop a positive permeability membrane with a separation active layer of polymer on the surface of the microporous support membrane. The separation active layer is formed by optimizing specific salt reverse diffusion and water permeability, combined with heating treatment and interface polymerization. , ensuring the durability and efficient concentration performance of the membrane.

Benefits of technology

The film performance of salt reverse diffusion and moderate water permeability in high concentration concentration is achieved, ensuring the stability and durability of the film multiple use, avoiding the reverse diffusion and reduction of salt water permeability, and improving the concentration process practicality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113905807B_ABST
    Figure CN113905807B_ABST
Patent Text Reader

Abstract

The present invention provides a forward osmosis membrane and a forward osmosis membrane assembly and a method for manufacturing the same. By developing a forward osmosis membrane that can achieve an extremely excellent reduction in salt back diffusion compared to the past and has a specific water permeability, even if it is used multiple times in the concentration of a raw liquid with a liquid property similar to that used in actual concentration operation, it is possible to perform concentration in which the diffusion of the driving solution is suppressed. The membrane is practical and has durability that can maintain membrane performance within a specific range even if the concentration of a raw liquid with an osmotic pressure is performed multiple times. In one embodiment, a forward osmosis membrane is provided, which is a forward osmosis membrane having a separation active layer of a polymer on the surface of a microporous support membrane, wherein, when pure water as a raw liquid is arranged on the separation active layer side through the forward osmosis membrane and a 3.5 mass % sodium chloride aqueous solution as a driving solution is arranged on the support membrane side, the salt back diffusion amount R1 toward the raw liquid is 0.65 g / (m 2 × hr) or less, and the water permeation F1 toward the draw solution is 3.5 kg / (m 2 ×hr) or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a forward osmosis membrane for separating a solvent from a liquid mixture as an object to concentrate the object, and a forward osmosis membrane module including the forward osmosis membrane and a method for manufacturing the same. More specifically, the present invention relates to a forward osmosis membrane that is particularly suitable for high-concentration concentration of a raw material liquid by achieving an extremely excellent reduction in the amount of salt back diffusion and having a water permeability above a certain level; and a forward osmosis membrane module including the forward osmosis membrane and a method for manufacturing the same. Background Art

[0002] As a method for concentrating a raw material liquid, a forward osmosis method is known.

[0003] Forward osmosis is a method of moving a solvent from a raw material to a driving solution by making the raw material liquid adjacent to a driving solution having an osmotic pressure higher than that of the raw material liquid by means of a forward osmosis membrane. The driving force of the forward osmosis method is the osmotic pressure difference between the raw material liquid and the driving solution. Therefore, unlike the distillation method or reverse osmosis method as existing concentration techniques, it does not require heating or high pressure, and it is expected that the raw material liquid can be concentrated without losing the valuable components in the raw material liquid.

[0004] The forward osmosis method is similar to the reverse osmosis method in that the solvent is preferentially permeated over the solute using a semipermeable membrane. However, in the forward osmosis method, the solvent is permeated from the dilute solution (raw solution) side to the concentrated solution (drawing solution) side by utilizing the osmotic pressure difference. From this aspect, it is different from the reverse osmosis method in which the concentrated solution side is pressurized by resisting the osmotic pressure difference so that water is permeated from the concentrated solution side to the dilute solution side. Therefore, even if the reverse osmosis membrane designed in a manner to exert a high water permeability under pressure as described in non-patent literature 1 is directly applied to the forward osmosis method, it may not be suitable for the forward osmosis method.

[0005] The membrane suitable for forward osmosis is designed so that the permeation rate of the solvent from the raw material solution to the driving solution (water permeability) is large, and the diffusion of the components in the driving solution to the raw material solution (salt back diffusion) is small. However, it is usually not easy to achieve high water permeability and low salt back diffusion, and there is a paradox that if the performance of one is improved, the performance of the other will be sacrificed.

[0006] To address this problem, Patent Document 1 establishes a method for forming a separation active layer on the inner surface of the hollow fiber membrane of an assembled hollow fiber membrane module by interfacial polymerization. By forming a uniform separation active layer, a forward osmosis membrane with high water permeability and low reverse diffusion is obtained.

[0007] In addition, in Patent Documents 2 and 3, a separation active layer is formed on the surface of a support membrane having a high-porosity structure to improve the diffusivity of the solute inside the support membrane, thereby obtaining a forward osmosis membrane having an appropriate water permeability.

[0008] In addition, Non-Patent Document 2 compares and evaluates various forward osmosis membranes, and describes the result that a forward osmosis membrane having a separation active layer on the inner surface of a hollow fiber has a high water permeability.

[0009] As a method for improving the separation performance of a semipermeable membrane, Patent Document 4 proposes a method for improving the organic matter removal rate by subjecting a composite reverse osmosis membrane to hot water treatment.

[0010] Patent Documents 5 and 6 propose methods of simultaneously improving organic matter removal and water permeability by treating a composite reverse osmosis membrane with hot water containing trialkylamine or the like, and Patent Document 7 proposes a method of treating a membrane with hypochlorite after hot water treatment.

[0011] In addition, Patent Document 8 proposes a method of obtaining a reverse osmosis membrane having high performance under low pressure by improving a solution and supplying the produced semipermeable membrane to a dryer at 100° C. or higher.

[0012] Prior art literature

[0013] Patent Literature

[0014] Patent Document 1: International Publication No. 2016 / 027869

[0015] Patent Document 2: U.S. Patent Application Publication No. 2013 / 0313185

[0016] Patent Document 3: Japanese Patent Application Publication No. 2016-155078

[0017] Patent Document 4: Japanese Patent Publication No. 07-114941

[0018] Patent Document 5: Japanese Patent No. 3665692

[0019] Patent Document 6: Japanese Patent No. 3862184

[0020] Patent Document 7: International Publication No. 99 / 22836

[0021] Patent Document 8: Japanese Patent No. 3181134

[0022] Non-patent literature

[0023] Non-patent document 1: NY Yip, A. Tiraferri, WA Phillip, JD Schiffman and M. Elimelech, "High Performance Thin-Film Composite Forward Osmosis Membrane", Environ. Sci. Technol., 44, 3812-3818 (2010)

[0024] Non-patent literature 2: S.Chou, L.Shi, R.Wang, CYTang, C.Qiu and AGFane, "Characteristics and potential applications oFa novel forward osmosis hollowfiber membrane", Desalination, 261, 365-372 (2010) Summary of the invention

[0025] Problems to be solved by the invention

[0026] However, the methods described in Patent Document 1 and Non-Patent Document 2 cannot be said to sufficiently reduce the amount of salt back diffusion, and there is still room for improvement in the forward osmosis membrane itself.

[0027] In addition, in the method described in patent documentation 2 and 3, although the water permeability increases, there is the shortcoming that the salt reverse diffusion amount also increases. When considering actual concentration treatment, in the stock solution as the concentrated object, there are many kinds of components mixed, and the solute exists in high concentration across the two sides of the forward osmosis membrane in most cases. Especially in the high concentration concentration of the stock solution, while the solvent is moved from the stock solution with very high solute concentration, it is also necessary to reduce the salt reverse diffusion. In this case, as the preferred performance of the forward osmosis membrane, compared with high water permeability, a certain degree of water permeability and lower salt reverse diffusion are considered to be more preferred. However, as seen in the above-mentioned document, in the development of the forward osmosis membrane, high water permeability is emphasized in most cases, and from this aspect, the forward osmosis membrane also has a lot of room for improvement.

[0028] The method described in Patent Document 4 has the problem that the water permeability of the treated membrane is significantly reduced. In addition, the methods described in Patent Documents 5 to 7 have the problem that the treated membrane is not washed and the membrane residue is dissolved during actual use. In addition, regarding the method described in Patent Document 8, the semipermeable membrane is usually hydrophilic, and when it becomes dry, the softness or strength of the semipermeable membrane will be lost, and it will take time or a hydrophilizing agent to recover.

[0029] In addition, the above method is a method developed based on a flat reverse osmosis membrane, and even if the reverse osmosis membrane produced by the above method is used for forward osmosis treatment, it is difficult to show high performance. In addition, any of the above methods is treated in a state where the separation active layer of the membrane is exposed, so the separation active layer is easily physically damaged, which also becomes a problem in the module required in most cases of actual use of the membrane.

[0030] Therefore, an object of one embodiment of the present invention is to provide a forward osmosis membrane and a forward osmosis membrane assembly and a method for manufacturing the same by developing a forward osmosis membrane that can achieve an extremely excellent reduction in salt back diffusion (one of the performance indicators of a conventional forward osmosis membrane) compared with the past when the performance is tested when water is used as the raw liquid and an aqueous sodium chloride solution is used as the driving solution, and has a specific water permeability. The forward osmosis membrane can perform concentration in which the diffusion of the driving solution is suppressed even if it is used multiple times in the concentration of a raw liquid with a liquid property similar to that used in actual concentration operation (i.e., having an osmotic pressure), is practical, and has durability that can maintain the membrane performance within a specific range even if the concentration of the raw liquid with osmotic pressure is performed multiple times.

[0031] Means for solving problems

[0032] The inventors did not aim for high water permeability, which was the development guideline of many forward osmosis membranes in the prior art, but instead pursued low salt back diffusion at the expense of a certain degree of water permeability. They also focused on the possibility that setting the appropriate range of both properties would affect the actual concentration operation behavior and the durability of the forward osmosis membrane, and developed a practical forward osmosis membrane based on a development guideline that did not exist before.

[0033] That is, an example of an embodiment of the present invention is as follows.

[0034] Method 1

[0035] A forward osmosis membrane having a separation active layer of a high molecular polymer provided on the surface of a microporous support membrane, wherein:

[0036] When pure water as a raw material solution is arranged on the separation active layer side through the forward osmosis membrane and a 3.5 mass % sodium chloride aqueous solution as a driving solution is arranged on the microporous support membrane side, the salt back diffusion amount R1 toward the raw material solution is 0.65 g / (m 2 × hr) or less, and the water permeation rate F1 toward the above-mentioned draw solution is 3.5 kg / (m 2 ×hr) or above.

[0037] Method 2

[0038] The forward osmosis membrane according to the first aspect, wherein the amount of salt back diffusion R1 toward the raw material solution is 0.45 g / (m 2 ×hr) or less.

[0039] Method 3

[0040] The forward osmosis membrane according to the above embodiment 1 or 2, wherein the amount of salt back diffusion R1 toward the raw material solution is 0.30 g / (m 2 ×hr) or less.

[0041] Method 4

[0042] The forward osmosis membrane according to any one of the above aspects 1 to 3, wherein the permeation rate F1 to the draw solution is 5.0 kg / (m 2 ×hr) or above.

[0043] Method 5

[0044] The forward osmosis membrane according to any one of the above aspects 1 to 4, wherein the permeation rate F1 to the draw solution is 6.5 kg / (m 2 ×hr) or above.

[0045] Method 6

[0046] The forward osmosis membrane according to any one of the above aspects 1 to 5, wherein the amount of salt back diffusion R1 toward the raw material solution is 0.01 g / (m 2 ×hr) or above.

[0047] Method 7

[0048] The forward osmosis membrane according to any one of the above aspects 1 to 6, wherein the water permeation rate F1 to the draw solution is 50 kg / (m 2 ×hr) or less.

[0049] Method 8

[0050] A forward osmosis membrane as described in any one of the above-mentioned methods 1 to 7, wherein the above-mentioned microporous support membrane includes a membrane having at least one selected from the group consisting of polyethersulfone, polysulfone, polyketone, polyetheretherketone, polyphenylene ether, polyvinylidene fluoride, polyacrylonitrile, polyimine, polyimide, polybenzoxazole, polybenzimidazole and polyamide as a main component.

[0051] Method 9

[0052] In the forward osmosis membrane according to the eighth aspect, the microporous support membrane is a membrane containing at least one selected from the group consisting of polyethersulfone, polysulfone, polyketone, and polybenzimidazole as a main component.

[0053] Method 10

[0054] In the forward osmosis membrane according to the above aspect 9, the microporous support membrane is a membrane containing at least one selected from the group consisting of polyethersulfone and polysulfone as a main component.

[0055] Method 11

[0056] The forward osmosis membrane according to any one of aspects 8 to 10, wherein the permeation rate F1 to the draw solution is 5.0 kg / (m 2 ×hr) or above.

[0057] Method 12

[0058] The forward osmosis membrane according to any one of the above aspects 8 to 11, wherein the amount of salt back diffusion R1 toward the raw material solution is 0.45 g / (m 2 ×hr) or less.

[0059] Method 13

[0060] The forward osmosis membrane according to any one of aspects 1 to 12, wherein the high molecular weight polymer is a polycondensation product of one or more first monomers selected from the group consisting of polyfunctional amines and one or more second monomers selected from the group consisting of polyfunctional acid halides.

[0061] Method 14

[0062] The forward osmosis membrane according to the above aspect 13, wherein the high molecular weight polymer is polyamide.

[0063] Method 15

[0064] The forward osmosis membrane according to any one of aspects 1 to 14, wherein the forward osmosis membrane is a hollow fiber.

[0065] Method 16

[0066] In the forward osmosis membrane according to the fifteenth aspect, the separation active layer is present on the inner surface of the microporous support membrane.

[0067] Method 17

[0068] A forward osmosis membrane module is provided, wherein the forward osmosis membrane according to any one of aspects 1 to 16 is assembled.

[0069] Method 18

[0070] In the forward osmosis membrane module according to the seventeenth aspect, the forward osmosis membrane is a hollow fiber, and the forward osmosis membrane module includes a hollow fiber bundle composed of a plurality of the hollow fibers.

[0071] Method 19

[0072] A forward osmosis membrane module as described in the above-mentioned embodiment 18, wherein, in a scanning electron microscope image obtained by photographing a cross-section of the separation active layer in the thickness direction, the coefficient of variation of the average thickness of the separation active layer in the radial direction and the longitudinal direction of the above-mentioned hollow fiber bundle is 0 to 60%.

[0073] Method 20

[0074] A method for manufacturing a forward osmosis membrane assembly, which is the method for manufacturing a forward osmosis membrane assembly described in the above-mentioned embodiment 18 or 19, comprising the following steps:

[0075] a separation active layer forming step of providing a separation active layer on the inner surface of the microporous support membrane; and

[0076] The heat treatment step is a step of supplying a fluid at 55° C. or higher in a flowing and wet state to at least the inner surface side of the hollow fiber after the separation active layer forming step.

[0077] Method 21

[0078] In the method for producing a forward osmosis membrane module according to aspect 20, the heat treatment step is performed by continuously supplying hot water at a temperature of 70° C. to 95° C. to at least the inner surface side of the hollow fiber.

[0079] Method 22

[0080] In the method for producing a forward osmosis membrane module according to the above aspect 20, the heat treatment step is performed using steam at a temperature of 100° C. to 150° C.

[0081] Effects of the Invention

[0082] The forward osmosis membrane of one embodiment of the present invention has extremely low salt back diffusion and a water permeability above a specific level, so it can have both practicality such as concentration of a driving solution with suppressed diffusion even after multiple uses, and durability such as maintaining membrane performance within a specific range even after multiple concentrations of a raw material solution with osmotic pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] Figure 1 This is a schematic cross-sectional view of one embodiment of a forward osmosis membrane module. DETAILED DESCRIPTION

[0084] An embodiment of the present invention (hereinafter also referred to as “the present embodiment”) will be described in detail below as a non-limiting example.

[0085] The present embodiment can be suitably used for the concentration of, for example, liquid food or pharmaceutical solution. When using the forward osmosis membrane of the present embodiment, it is possible to concentrate at a high rate without heating the concentrated object, and then it is possible to achieve non-heating high-concentration concentration that prevents the deterioration of the components or the mixing of impurities while highly suppressing the outflow or inflow of the solute. In addition, the present embodiment can also be suitably used for seawater desalination, salt water desalination, the treatment of associated water discharged from gas fields such as shale gas or oil fields, the concentration of fertilizer solutions, or the use of the desired concentrate as the dilution purpose of the driving solution, etc., in addition to being used for purposes such as dehydration.

[0086] The forward osmosis membrane of this embodiment is composed of a separation active layer and a microporous support membrane. The separation active layer is composed of a semipermeable membrane that only transmits specific substances, and the microporous support membrane physically supports the separation active layer on the surface of the microporous support membrane, more specifically, on its inner surface or outer surface.

[0087] The water permeation F1 and salt back diffusion R1 of the forward osmosis membrane in this embodiment were evaluated by performing forward osmosis treatment at 25° C. using pure water as a raw material solution and a 3.5 mass % sodium chloride aqueous solution as a drive solution.

[0088] In addition, the salt back diffusion amount R2, the water permeability F2, and the salt permeability R2 / F2 calculated by dividing R2 by F2 of the forward osmosis membrane in this embodiment are evaluated by using a raw solution (for example, a raw solution containing a solute (for example, a 20 mass % sodium chloride aqueous solution)) and a driving solution having an osmotic pressure higher than that of the raw solution (for example, a 35 mass % magnesium chloride aqueous solution) to perform forward osmosis treatment under the condition that each solution is 25°C.

[0089] These evaluations were performed five times, and the average value was used for evaluation.

[0090] In addition, when using a forward osmosis membrane having a support membrane and a separation active layer disposed on one side of the support membrane, the water permeation F may be significantly different depending on whether the raw liquid is located on the separation active layer side or the support membrane side. In this embodiment, under an actual concentration environment, the raw liquid can be evaluated by arranging it on the separation active layer side where the risk of membrane contamination is less. In this case, the water permeation is usually reduced compared to when the raw liquid is arranged on the support membrane side.

[0091] The salt back diffusion amount R of the forward osmosis membrane (which can be R1 or R2, so R1 and R2 are collectively referred to as R) refers to the amount of solute that moves from the draw solution to the raw material solution when the raw material solution to be concentrated is circulated on the separation active layer side through the forward osmosis membrane and the draw solution having a higher osmotic pressure than the draw solution is arranged on the support membrane side. The salt back diffusion amount R is defined by the following formula (1).

[0092] R=G / (M×H) ···Formula (1)

[0093] Here, G is the amount of solute that permeates (g), and M is the effective surface area of ​​the forward osmosis membrane (m 2 ), and H is time (hr).

[0094] The separation active layer is substantially arranged on the surface of the support membrane. In the case of the concept of the surface and the back side, it is preferably arranged on either side, but it can also be present on both sides. The separation active layer can be a symmetrical structure or an asymmetrical structure relative to the microporous support membrane. In addition, when the separation active layer is present on both sides of the support membrane, the separation active layers on both sides can be kept continuous or discontinuous by means of the microporous support membrane. In the case of configuring the separation active layer on both sides of the support membrane, the separation active layer side in the present disclosure refers to the layer side that is considered to be better in the whole forward osmosis membrane to prevent the solute of the driving solution. As an evaluation method for better preventing the solute of the driving solution on one side, for example, the reverse diffusion amount R1 of the above-mentioned salt toward the raw material solution can be evaluated by configuring pure water as a raw material solution on one side and 3.5% by mass of a sodium chloride aqueous solution as a driving solution on the other side across the forward osmosis membrane, and making the configuration of these solutions opposite, when comparing these two evaluation systems, the raw material liquid side in the evaluation system with a smaller R1 is used as a side (separation active layer side) that better prevents the solute of the driving solution.

[0095] The salt back diffusion amount R1 (salt back diffusion) of the forward osmosis membrane of this embodiment is extremely low, and the lower it is as much as possible, the better. If the salt back diffusion amount is too large, the solute in the draw solution will be mixed into the raw material solution, or the solute in the raw material solution will be mixed into the draw solution, the purity of the raw material solution concentrate will be reduced and the component balance will be destroyed, the draw solution will be contaminated, and the components in the draw solution will be reduced over time.

[0096] The reason for this is not clear, but it is found that even if the salt back diffusion amount R1 is 1.2 g / (m 2 × hr), when this value is exceeded, the salt back diffusion amount R2 increases significantly, and as a result, the salt permeability R2 / F2 tends to increase. In order to avoid these problems, the salt back diffusion amount R1 of the forward osmosis membrane of this embodiment is 0.65 g / (m 2× hr) or less, preferably 0.45 g / (m 2 × hr) or less, more preferably 0.30 g / (m 2 ×hr) or less.

[0097] It should be noted that the salt reverse diffusion amount R1 of the forward osmosis membrane of this embodiment can be 0.01 g / (m 2 ×hr) or above.

[0098] The water permeability F of the forward osmosis membrane (which can be F1 or F2, so F1 and F2 are collectively referred to as F) refers to the amount of water that moves from the raw material solution to the drive solution when the raw material solution to be concentrated is circulated on the separation active layer side across the forward osmosis membrane and a drive solution having a higher osmotic pressure than the raw material solution is configured on the support membrane side. The water permeability F of the forward osmosis membrane is defined by the following formula (2).

[0099] F=L / (M×H) ···Formula (2)

[0100] Here, L is the amount of water permeated (kg), M is the effective surface area of ​​the forward osmosis membrane (m 2 ), and H is time (hr).

[0101] The higher the water permeability F1 (water permeability or water permeability performance) of the forward osmosis membrane of this embodiment, the better. However, from the perspective of practicality of raw material liquid concentration and efficient solvent movement, in one embodiment, it is 3.5 kg / (m 2 From the same perspective, the water permeability F1 is preferably 5.0 kg / (m 2 × hr) or more, more preferably 6.0 kg / (m 2 × hr) or more, particularly preferably 6.5 kg / (m 2 The reason is not clear, for example, as a result of using a reverse osmosis membrane as a forward osmosis membrane, when the water permeation F1 is less than 3.5 kg / (m 2 × hr), the water permeability F2 is significantly reduced, the influence of the salt reverse diffusion R2 is relatively significant, and the salt permeability R2 / F2 increases, which cannot constitute a practical forward osmosis membrane. On the other hand, when the water permeability is particularly large, the salt reverse diffusion is also increased in many cases. Therefore, the water permeability F1 is preferably 50kg / (m 2 ×hr) or less.

[0102] The salt permeability R1 / F1 obtained by dividing the salt reverse diffusion amount R1 of the present embodiment by the water permeability F1 is an index representing the selectivity of the penetration of the solvent and the penetration of the salt. The lower the value, the less likely the salt is to penetrate and the easier the solvent is to penetrate, so it is preferred. However, in the existing common forward osmosis membrane, if the salt reverse diffusion amount is reduced, the water permeability will be significantly reduced in most cases, and as a result, the value of R1 / F1 will mostly increase. From the perspective of the practicality of the concentration of the raw liquid and the movement of the solvent to achieve high efficiency, in the forward osmosis membrane of the present embodiment, the value of R1 / F1 is preferably less than 0.08, more preferably less than 0.06, further preferably less than 0.04, and particularly preferably less than 0.03. The value of R1 / F1 is ideally 0, but from the perspective of the ease of manufacturing of the forward osmosis membrane, it can be, for example, more than 0.0001.

[0103] By setting the forward osmosis membrane of this embodiment to have an initial water permeation rate F1 of 3.5 kg / (m 2 ×hr) or more, and R1 is 0.65g / (m 2 × hr) or less, for example, in the concentration of a raw material solution having an osmotic pressure, even if the forward osmosis membrane is used multiple times, concentration can be performed with the diffusion of the draw solution suppressed, and thus it has high practicality.

[0104] Furthermore, from the comparison of the membrane performance R1 / F1 between the initial stage and the stage after the concentration operation, the forward osmosis membrane of the present embodiment can maintain the membrane performance within a desired range even when used multiple times, and can have high durability.

[0105] The reason is still uncertain, but it is believed that it is because, in the forward osmosis membrane of the present embodiment, due to the proper balance between the initial permeable water amount F1 and the salt reverse diffusion amount R1, it is not easy to load materials such as driving solutes in the separation active layer, and the osmotic pressure in the separation active layer is not easy to rise, so it can be suppressed that the water etc. that exceed the water content originally possessed by the separation active layer quickly invades the inside of the separation active layer, and as a result, the high-dimensional structure of the separation active layer will not be destroyed. The high-dimensional structure represented by the molecular structure of the separation active layer and the interaction between hydrogen bonds and aromatic rings will strongly affect the permeability of water and salt. Once the high-dimensional structure is destroyed, materials such as driving solutes are more likely to invade and be loaded inside the separation active layer. Such an invasion causes the osmotic pressure in the separation active layer to rise, and a series of destructions of the separation active layer may be caused thereby. As a result, the performance of the forward osmosis membrane will be reduced to a certain value.

[0106] In this embodiment, since the water permeability F1 is above a specific value and the salt reverse diffusion amount R1, which is an index of salt permeability, is low, the salt load in the separation active layer can be suppressed for a long time by, for example, flushing. Based on the above, the forward osmosis membrane of this embodiment is not only practical, but also durable. It should be noted that this embodiment is not limited to the above considerations.

[0107] The salt permeability R2 / F2 obtained by dividing the salt back diffusion amount R2 of the present embodiment by the water permeability F2 is an indicator of selectivity closer to the actual concentration environment from the perspective of the osmotic pressure of the raw liquid. The lower the salt permeability R2 / F2, the less likely the salt is to permeate and the easier the solvent is to permeate. Therefore, it is preferred. The reason is still unclear, but it is probably due to the influence of ion exchange, etc., when there are solutes on both sides of the forward osmosis membrane, the salt permeability is often reduced. In particular, as mentioned above, even if the salt back diffusion amount R1 is 1.2 g / (m 2 × hr), when this value is exceeded, the salt back diffusion amount R2 increases significantly, while on the other hand, the water permeation amount F2 hardly increases, and as a result, R2 / F2 tends to increase. When the forward osmosis membrane of this embodiment is used, the values ​​of R2, F2 and R2 / F2 can be the values ​​in the ranges exemplified as the values ​​of R1, F1 and R1 / F1, respectively.

[0108] The draw solution is a solution that has a higher osmotic pressure than the raw material solution containing the substance to be separated or concentrated and has a function of transferring the solvent from the raw material solution via the forward osmosis membrane.

[0109] The draw solution exhibits a high osmotic pressure by containing a draw solute at a high concentration.

[0110] As the draw solute, for example, alkali metal salts, alkaline earth metal salts, ammonium salts, sugars, monoalcohols, diols, water-soluble polymers, etc. can be cited. As specific examples of these,

[0111] Examples of the alkali metal salt include sodium chloride, potassium chloride, sodium sulfate, sodium thiosulfate, sodium sulfite, and the like;

[0112] Examples of the alkaline earth metal salt include magnesium chloride, calcium chloride, and magnesium sulfate;

[0113] Examples of the ammonium salt include ammonium chloride, ammonium sulfate, and ammonium carbonate.

[0114] Examples of sugars include common sugars such as sucrose, fructose, and glucose, and special sugars such as oligosaccharides and rare sugars.

[0115] Examples of the monoalcohol include methanol, ethanol, 1-propanol, and 2-propanol;

[0116] As diol, for example, ethylene glycol, propylene glycol, etc. can be mentioned;

[0117] Examples of the water-soluble polymer include polyethylene oxide, polypropylene oxide, and copolymers of ethylene oxide and propylene oxide.

[0118] The microporous support membrane in the present embodiment (sometimes also referred to as the support membrane in the present disclosure) refers to a membrane for supporting the separation active layer of a polymer (representatively a polymer film), and preferably does not substantially show separation performance to the object to be separated. As the microporous support membrane, any microporous support membrane including the known microporous support membrane can be used. The microporous support membrane in the present embodiment preferably has micropores on its surface with a pore size preferably between 0.001 μm and 0.1 μm, more preferably between 0.005 μm and 0.05 μm. On the other hand, with respect to the structure other than the surface of the microporous support membrane, in order to reduce the permeation resistance of the fluid to be passed through, as long as the strength can be maintained, it is preferably a structure that is as sparse as possible. The sparse structure of this part is preferably, for example, any structure in a mesh, finger-like cavity, or a mixed structure thereof.

[0119] The microporous support membrane is particularly preferably a hollow fiber because a larger surface area per unit module of the forward osmosis membrane module can be obtained.

[0120] When a specific pressure is applied to the microporous support membrane in this embodiment, the water permeability of the support membrane, which is expressed as the amount of pure water that permeates a specific membrane area within a specific time, is preferably 100 kg / (m 2 × hr) / 100 kPa or more, more preferably 200 kg / (m 2 ×hr) / 100kPa or more. If the water permeability of the support membrane is too low, the water permeability F of the forward osmosis membrane module obtained as a result is also likely to decrease. Within the range that does not damage the mechanical strength of the support membrane, the larger the water permeability of the support membrane, the better. Generally, if the water permeability increases, the mechanical strength decreases. Therefore, the target water permeability of the microporous support membrane in this embodiment is preferably 50,000kg / (m 2 × hr) / 100 kPa or less, more preferably 10,000 kg / (m 2 ×hr) / 100kPa or less.

[0121] As the material of the microporous support membrane, any material can be used as long as it is a material that can be formed on the microporous support membrane. However, when manufacturing the forward osmosis membrane in the present embodiment, it is necessary to prevent it from being chemically damaged by the monomer solution used, etc. In addition, in the present embodiment, it is preferably possible to form a microporous hollow fiber. Therefore, from the aspects of chemical resistance, film forming, durability, etc., as the material of the microporous support membrane, for example, preferably selected from polyethersulfone, polysulfone, polyketone, polyetheretherketone, polyphenylene ether, polyvinylidene fluoride, polyacrylonitrile, polyimine, polyimide, polybenzoxazole, polybenzimidazole and polyamide at least one as the main component, more preferably selected from polyethersulfone, polysulfone, polyketone and polybenzimidazole at least one as the main component, further preferably selected from polysulfone and polyethersulfone at least one as the main component, and then preferably polyethersulfone. In addition, the above-mentioned "main component" refers to the component with the most mass proportion in the whole, and in one mode, it is the component with the proportion exceeding 50 mass % in the whole.

[0122] When the microporous support membrane is a hollow fiber, the hollow fiber diameter is not particularly limited. Considering the membrane stability, ease of handling, membrane area when made into a module, etc., the outer diameter is preferably in the range of 100μm to 3,000μm and the inner diameter is 30μm to 2,500μm, and the outer diameter is more preferably in the range of 200μm to 1,500μm and the inner diameter is 50μm to 1,000μm.

[0123] Such a microporous support membrane, for example, a microporous hollow fiber support membrane can be produced by a known dry-wet membrane production method, melt membrane production method, wet membrane production method, or the like using a material selected from the above-mentioned materials.

[0124] The forward osmosis membrane of the present embodiment can be used in the form of a membrane assembly (forward osmosis membrane assembly) having a plurality of membranes. The shape of the membrane assembly is not particularly limited. Usually, there is a section where the liquid contacts only one surface side of the membrane and a section where the liquid contacts only the other surface side of the membrane, and the two are separated by an adhesive resin that fixes the membrane to the assembly housing. If a hollow fiber membrane is taken as an example, there is a section where the liquid contacts only the inner surface side of the membrane and a section where the liquid contacts only the outer surface side of the membrane. The size of the assembly housing is not particularly limited. For example, a cylindrical housing with a diameter of 0.5 inches to 20 inches and a length of 4 cm to 10 m can be used. In addition, as an adhesive resin, for example, a urethane-based, epoxy-based adhesive or the like can be used to make an assembly.

[0125] Figure 1The hollow fiber membrane module 1 (forward osmosis membrane module) shown has the following structure: a fiber bundle consisting of a plurality of hollow fibers 4 is filled in a cylindrical body, and both ends of the hollow fiber bundle are fixed to the cylinder by adhesive fixing parts 5, 6. The cylindrical body has outer conduits 2, 3 on its side, which are sealed by end caps 7, 8. The adhesive fixing parts 5, 6 here are respectively cured in a manner that does not block the holes of the hollow fibers. The end caps 7, 8 are respectively connected to the inner side (hollow part) of the hollow fiber 4, and have unconnected inner conduits 9, 10 on the outside. These conduits can be used to introduce liquid into the inner side of the hollow fiber 4, or to take out liquid. The outer conduits 2, 3 are respectively connected to the outer side of the hollow fiber 4, but not to the inside.

[0126] The hollow fiber membrane module 1 has a structure in which a liquid flowing inside and a liquid flowing outside are in contact with each other only via the hollow fibers 4 (forward osmosis membranes).

[0127] In this embodiment, the effective surface area of ​​the membrane refers to the region where the feed solution and the draw solution exist across the forward osmosis membrane during forward osmosis treatment (ie, the area of ​​the portion of the forward osmosis membrane where the feed solution or the draw solution is in contact).

[0128] For example, in the case of hollow fibers, the effective surface area of ​​the membrane (internal surface area of ​​the hollow fiber membrane) is defined by the following mathematical formula (3) based on the length, inner diameter and number of hollow fibers excluding the junctions in the module.

[0129] a=c×π×b×n···(3)

[0130] Here, a is the inner surface area of ​​the hollow fiber membrane (m 2 ), b is the length of the hollow fiber excluding the joint (m), c is the inner diameter of the hollow fiber (m), and n is the number of hollow fibers.

[0131] Regarding the thickness of the polymer film, the thinner the better as long as there are no pinholes. However, in order to maintain mechanical strength and chemical resistance, it is preferred to have an appropriate thickness. Therefore, considering film formation stability, water permeability, etc., the thickness of the polymer film is preferably 0.1 μm to 3 μm, and more preferably 0.2 μm to 2 μm.

[0132] In this embodiment, the coefficient of variation showing the fluctuation of the average thickness of the separation active layer is preferably within a specific range. The following describes the case where the fluctuation of the average thickness of the separation active layer at each position in the hollow fiber module in the hollow fiber module as a preferred example of the forward osmosis membrane module is expressed as a coefficient of variation. In the present disclosure, the coefficient of variation is the value obtained by dividing the standard deviation of the average thickness value at each measurement position by the average value between the measurement positions of the average thickness, and is expressed as a percentage (%).

[0133] In one embodiment, from the perspective of being able to further eliminate partial functional defects during manufacturing, the coefficient of variation of the average thickness of the separation active layer obtained by taking a scanning electron microscope image of a cross-section of the separation active layer in the thickness direction (more specifically, obtained by measuring the mass of the microscope image output using the method described in [Examples] of the present disclosure) is preferably 0 to 60% in the radial direction and the longitudinal direction of the hollow fiber bundle, more preferably 0 to 50%, further preferably 0 to 40%, and most preferably 0 to 30%.

[0134] More specifically, the coefficient of variation is determined by the following procedure: one hollow fiber is sampled from each of three locations, namely, the center in the radial direction of the module, the position of 50% of the radius, and the outermost circumference, and each of these hollow fibers is divided into three equal parts along the length direction. The thickness of the separation active layer is measured at each of the measurement locations of the obtained nine samples with n being equal to or greater than 1 (the number n is the same for each location), and the number average of the nine locations is calculated.

[0135] Here, the thickness at each measurement position is obtained as the average thickness in a measurement range of about 5 to 100 μm in length. The length of the measurement range is preferably 5 to 50 μm, more preferably 5 to 20 μm, and most preferably 13 μm. Regarding the separation active layer in the hollow fiber membrane module of the present embodiment, as described below, it is preferred that the surface thereof has a fine concave-convex shape. Therefore, when evaluating the thickness of the separation active layer, it is appropriate to evaluate it using the average thickness of the above-mentioned measurement range at each measurement position.

[0136] In addition, the coefficient of variation of the average thickness at each measuring position from the radial outermost periphery to the center of the hollow fiber membrane module, and the coefficient of variation from one end to the other end in the length direction of the module are preferably 0 to 60%, more preferably 0 to 50%, further preferably 0 to 40%, and most preferably 0 to 30%, respectively.

[0137] As described above, regarding the preferred separation active layer in the hollow fiber membrane assembly of the present embodiment, when the average thickness measured at a plurality of measurement positions is compared, the fluctuation is small. In the evaluation of the average thickness, the length direction of the above-mentioned measurement range can be the length direction of the hollow fiber, can be the circumferential direction of the hollow fiber, or can be a direction inclined relative to the length direction of the hollow fiber. In addition, the length directions of the measurement ranges in the plurality of scanning electron microscope images used in the calculation of the average value between the measurement positions can be the same direction or different directions.

[0138] The present inventors speculate as follows about the mechanism by which the surface of the separation active layer in the hollow fiber membrane module of the present embodiment has a fine concavoconvex shape. However, the present embodiment is not limited to the following theory.

[0139] The separation active layer of the present embodiment is preferably formed by interfacial polymerization. It is known that in interfacial polymerization, when the liquid film of the first monomer solution formed on the surface of the hollow fiber contacts the second monomer solution, the two are incompatible and polymerize at the interface, thereby forming a polymerized layer. As a result, the separation active layer formed becomes a shape having many fine concave-convex shapes on the surface. When the separation active layer is formed by a method other than interfacial polymerization, a separation active layer having a shape with many fine concave-convex shapes on the surface cannot be formed.

[0140] In addition, a preferred method for producing the forward osmosis membrane in this embodiment is to promote the crosslinking reaction by heat treatment as described below. In order to make the effect of the heat treatment uniform as a whole, it is preferred that the average thickness variation coefficient of the separation active layer is small as described above.

[0141] The separation active layer of the high molecular polymer in this embodiment is a membrane that can preferentially permeate the solvent, block the solute, and substantially has separation performance. As such a separation active layer, for example, polyamide, polyvinyl alcohol / polypiperazineamide, sulfonated polyethersulfone, polypiperazineamide, and polyimide are suitable.

[0142] In the present embodiment, particularly from the aspect of the ease of forming a flawless film on a microporous support membrane, polyamide is suitable for use. In addition, the more preferred forward osmosis membrane of the present embodiment is a hollow fiber, and in order to prevent physical damage to the separation active layer, the preferred forward osmosis membrane is on the inner surface of the hollow fiber.

[0143] In addition, the high molecular polymer is preferably a polycondensation product of one or more first monomers selected from the group consisting of polyfunctional amines and one or more second monomers selected from the group consisting of polyfunctional acyl halides. More specifically, for example, the above-mentioned polyamide obtained by the interfacial polycondensation reaction of polyfunctional amines and polyfunctional acyl halides can be cited. The separation performance when using these high molecular polymers as separation active layers refers to the performance of separating the solvent in the liquid mixture from the solutes such as ions dissolved therein.

[0144] Examples of the polyfunctional amine include polyfunctional aromatic amines, polyfunctional aliphatic amines, monomers having two or more reactive amino groups, and prepolymers thereof.

[0145] The polyfunctional aromatic amine refers to an aromatic amino compound having two or more amino groups in one molecule, and more specifically, for example, m-phenylenediamine, p-phenylenediamine, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylamine, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenylamine, 3,5-diaminobenzoic acid, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 3,4-diaminodiphenyl sulfone, 1,3,5-triaminobenzene, 1,5-diaminonaphthalene, etc., and a single substance or a mixture thereof can be used. In the present embodiment, it is particularly suitable to use one or more selected from m-phenylenediamine and p-phenylenediamine.

[0146] The polyfunctional aliphatic amine refers to an aliphatic amino compound having two or more amino groups in one molecule, and more specifically, for example, the following can be mentioned:

[0147] Primary amines having a cyclohexane ring, such as 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-bis(p-aminocyclohexyl)methane, 1,3-bis-(aminomethyl)cyclohexane, 2,4-bis-(aminomethyl)cyclohexane, and 1,3,5-triaminocyclohexane;

[0148] Secondary amines having a piperazine ring such as piperazine, 2-methylpiperazine, ethylpiperazine, and 2,5-dimethylpiperazine;

[0149] Secondary amines having a piperidine ring, such as 1,3-bis(4-piperidinyl)methane, 1,3-bis(4-piperidinyl)propane, and 4,4'-bispiperidine;

[0150] Amines having both a primary and secondary amine group, such as 4-(aminomethyl)piperidine; and

[0151] Ethylenediamine, propylenediamine, 1,2-propylenediamine, 1,2-diamino-2-methylpropane, 2,2'-dimethyl-1,3-propylenediamine, tris(2-aminoethyl)amine, N,N'-dimethylethylenediamine, N,N'-dimethylpropylenediamine, etc.

[0152] These may be used singly or in mixture. A mixture of these polyfunctional aliphatic amines and the above-mentioned polyfunctional aromatic amines may also be used.

[0153] Examples of monomers having two or more reactive amino groups include polyethyleneimine, amine-modified polyepichlorohydrin, and amino polystyrene. Examples of prepolymers that can be used include prepolymers composed of one or more selected from piperazine, 4-(aminomethyl)piperidine, ethylenediamine, and 1,2-diamino-2-methylpropane.

[0154] Examples of the polyfunctional halide include polyfunctional aromatic acid halides, polyfunctional aliphatic acid halides, etc. These components may be difunctional or more in order to react with the polyfunctional amine to form a polymer.

[0155] Polyfunctional aromatic acyl halide refers to an aromatic acyl halide compound having more than two acyl halide groups in one molecule. Specifically, for example, trimesoyl halide, trimesoyl halide, isophthaloyl halide, terephthaloyl halide, benzene tetracarboxylic acid halide, benzophenone tetracarboxylic acid halide, biphenyl dicarboxylic acid halide, naphthalene dicarboxylic acid halide, pyridine dicarboxylic acid halide, benzene disulfonyl halide, etc., and their single substance or mixture can be used. In the present embodiment, it is particularly preferred to use a single trimesoyl chloride, or a mixture of trimesoyl chloride and isophthaloyl chloride, or a mixture of trimesoyl chloride and terephthaloyl chloride.

[0156] The polyfunctional aliphatic acyl halide refers to an aliphatic acyl halide compound having two or more acyl halide groups in one molecule. Specifically, examples thereof include alicyclic polyfunctional acyl halide compounds such as cyclobutanedicarboxyl halide, cyclopentanedicarboxyl halide, cyclopentanetricarboxyl halide, cyclopentanetetracarboxyl halide, cyclohexanedicarboxyl halide, and cyclohexanetricarboxyl halide; and

[0157] Propane tricarbonyl halide, butane tricarbonyl halide, pentane tricarbonyl halide, succinyl halide, glutaryl halide, etc. These components may be used alone or in a mixture, or a mixture of these polyfunctional aliphatic acid halides and the above-mentioned polyfunctional aromatic acid halides may be used.

[0158] The first monomer and the second monomer described above are respectively provided to the polymerization in the form of a solution in which each of them is dissolved in an appropriate solvent.

[0159] As a preferred method for purifying a high molecular polymer film in this embodiment, for example, a method of passing a first solution and a second solution in two stages can be cited, wherein the first solution is a solution containing a monomer with which the microporous support membrane first contacts, and the second solution is a solution containing a monomer that reacts with the monomer in the first solution to form a high molecular polymer, which contacts the support membrane after contacting the first solution. One of the first monomer and the second monomer is contained in the first solution, and the other is contained in the second solution. Either monomer can be contained in any solution, but a method in which two monomers are contained in one solution is not preferred.

[0160] As the solvent of these first solution and the solvent of the second solution, there is no particular limitation as long as the monomer contained in each can be dissolved, a liquid-liquid interface can be formed when the two solutions are in contact, and the microporous support film can not be damaged. As such a solvent, for example, a single substance or a mixture of water, alcohol, etc. can be cited as the solvent of the first solution, and a single substance or a mixture of hydrocarbon solvents such as n-hexane, cyclohexane, n-heptane, n-octane, n-nonane, and n-decane can be cited as the solvent of the second solution. By selecting such a solvent as described above, the first solution and the second solution are in a non-mixed state, and a polymerization condensation reaction (interfacial polymerization reaction) is carried out to obtain a film of a high molecular polymer. It is preferred to select the first monomer as the monomer contained in the first solution, and select the second monomer as the monomer contained in the second solution. The concentrations of these reactive compounds contained in the first solution and the second solution are different according to the type of monomer, the distribution coefficient in the solvent, etc., and are not particularly limited and can be appropriately set by those skilled in the art.

[0161] For example, taking the interfacial polymerization reaction when an aqueous solution of m-phenylenediamine is used as the first solution and a n-hexane solution of trimesoyl chloride is used as the second solution as an example, the following is described:

[0162] The concentration of m-phenylenediamine is preferably 0.1 to 10% by mass, more preferably 0.5 to 5% by mass. The concentration of trimesoyl chloride is preferably 0.01 to 10% by mass, more preferably 0.1 to 5% by mass. If the concentration of these solutions is too low, it is easy to produce the disadvantage of incomplete film formation based on interfacial polymerization, resulting in a decrease in separation performance. On the contrary, if it is too high, the formed film becomes too thick, which not only causes a decrease in water permeability, but also has the possibility of increasing the amount of residual unreacted substances in the membrane and adversely affecting the membrane performance.

[0163] When an acid is generated during the interfacial polymerization reaction, a base as an acid scavenger may be added to the first solution or the second solution. In addition, a surfactant for improving wettability with a microporous support membrane, a catalyst for accelerating the reaction, a salt as a film-forming agent, etc. may be added as needed.

[0164] Examples of acid scavengers include caustic soda such as sodium hydroxide; sodium phosphate such as trisodium phosphate; sodium carbonate such as sodium carbonate; tertiary amines such as trimethylamine, triethylamine, and triethylenediamine; and the like. Examples of surfactants include sodium lauryl sulfate and sodium laurylbenzenesulfonate. Examples of catalysts include dimethylformamide. Examples of film-forming enhancers include a mixture of a trialkylamine such as triethylamine and an organic acid such as camphorsulfonic acid. These may be contained in the first solution or the second solution in advance.

[0165] In addition, in the present embodiment, it is estimated that by adjusting the high-dimensional structure of the polymer film and increasing the crosslinking density, physical durability and solvent resistance can be obtained, and the amount of salt back diffusion can be reduced, so it is particularly preferred to promote (curing) the crosslinking reaction based on heat treatment after the film is formed. In more detail, by subjecting the forward osmosis membrane to heat treatment in an appropriate manner, the separation active layer can be heated uniformly as a whole and in a relatively short time, and a forward osmosis membrane with reduced partial functional defects can be formed.

[0166] In the method for producing a forward osmosis membrane module of the present embodiment, the microporous support membrane is a hollow fiber, and it is preferred that the support membrane be subjected to a heat treatment step in a wet state after a separation active layer is provided on the inner surface of the support membrane.

[0167] More specifically, in one embodiment of the method for manufacturing a forward osmosis membrane module, the microporous support membrane is a hollow fiber, and a separation active layer is provided on the inner surface of the support membrane, and the coefficient of variation of the average thickness of the separation active layer in the radial direction and the longitudinal direction of the hollow fiber bundle calculated by a method of measuring the amount of the separation active layer portion in a scanning electron microscope image obtained by photographing a cross section in the thickness direction of the separation active layer (more specifically, a method of measuring the mass of the microscope image output by the method described in [Examples] of the present disclosure) is 0 to 60%. In one embodiment, in the method for manufacturing a forward osmosis membrane module, after providing the separation active layer, a heat treatment step is performed, and a fluid (e.g., liquid or gas) at 55° C. or higher is supplied in a flowing state and in a wet state to at least the separation active layer forming side of the support membrane (e.g., when the separation active layer is provided on the inner surface of the support membrane, at least the inner surface side of the hollow fiber).

[0168] As a heat treatment method, for example, the permeation of a humidified gas (e.g., nitrogen or air containing water) heated by a heat source or the permeation of hot water, and the permeation or exposure of water vapor can be cited. Here, permeation refers to a process in which the separation active layer and the microporous support membrane are contacted with a fluid by supplying a fluid to the forward osmosis membrane. As a preferred permeation method, for example, in the case of a hollow fiber-shaped forward osmosis membrane, a method in which the fluid is contacted with the surface side and back side and the inside of the separation active layer, and the pores of the microporous support membrane by supplying a fluid to the inside or outside of the hollow fiber or both sides thereof can be cited.

[0169] Here, the heat treatment in the "heat treatment step" of the present embodiment refers to a treatment at a temperature of at least 55° C. In addition, the "flowing state" of the present embodiment refers to a state in which a substance in a solid, liquid or gas moves.

[0170] The heat treatment step in this embodiment is more effective when the separation active layer of the forward osmosis membrane has a uniform thickness. The uniform thickness refers to a state in which the coefficient of variation of the average thickness of the separation active layer is 0 to 60%. The coefficient of variation is more preferably 0 to 50%, further preferably 0 to 40%, and most preferably 0 to 30%.

[0171] In the present embodiment, it is preferred to supply hot water at 60°C to 100°C to the forward osmosis membrane after the polymer film is formed. Among them, from the perspective of promoting the cross-linking reaction of the polymer film well and having high heat transfer efficiency, it is particularly suitable to use the forward osmosis membrane as a hollow fiber and supply hot water at 70°C to 95°C to the polymer film forming side as the inner surface side of the hollow fiber, that is, for the forward osmosis membrane having a separation active layer of a polymer on the inner surface of the microporous hollow fiber support membrane, at least the inner surface side of the hollow fiber is continuously subjected to the flow (more specifically, the permeation) of hot water at 70°C to 95°C. In the case of continuously flowing hot water (for example, permeation), compared with the method of immersing the separation active layer in hot water, it is not easy to cause unnecessary reactions by uniformly transferring heat to the separation active layer and flowing residual monomers in the support membrane, so it is particularly preferred. The water flow time of hot water is preferably 5 minutes to 2 hours. In the case of more than 5 minutes, cross-linking reactions and the like are well performed. If the reaction time exceeds 2 hours, the effect at the temperature will reach equilibrium, so the reaction time is preferably 2 hours or less.

[0172] In other examples of the present embodiment, it is also suitable to use a method of supplying high-temperature water vapor to the forward osmosis membrane. High-temperature water vapor refers in particular to water in a gaseous state of more than 100°C under high pressure conditions. High-temperature water vapor can usually be produced by a pressure autoclave such as an autoclave used in high-pressure steam sterilization. In the promotion of the cross-linking reaction of the polymer of the forward osmosis membrane, from the perspective of promoting the cross-linking reaction of the polymer film well, not significantly damaging the support membrane or the polymer film, and extremely reducing the back diffusion of salts, it is suitable to use, for example, a method of supplying water vapor of 100°C to 170°C to a forward osmosis membrane having a separation active layer of a polymer film on the inner surface of a microporous hollow fiber support membrane, and in particular a method of supplying water vapor of 100°C to 150°C. The time for supplying water vapor of the set temperature to the forward osmosis membrane is preferably 1 minute to 2 hours. In the case of more than 1 minute, cross-linking reactions can be carried out well. In addition, if it exceeds 2 hours, the effect at this temperature will reach equilibrium, so it is preferably less than 2 hours.

[0173] In addition, when at least one of the first monomer and the second monomer contains a reactive compound having more than three reactive groups and the above-mentioned heat treatment in a wet state is applied to the three-dimensional high molecular polymer film formed thereby, the above-mentioned effect can be more significantly manifested, resulting in improved strength and durability of the forward osmosis membrane and reduced salt back diffusion, which is particularly preferred.

[0174] The pure water referred to in the present disclosure refers to water having an electrical conductivity of 100 μS / cm or less and an organic matter concentration of 10 mass ppm or less, and can be produced by distillation, ion exchange, reverse osmosis, or the like.

[0175] Example

[0176] The present invention will be specifically described below based on examples, but the present invention is not limited to the examples.

[0177] [Example 1]

[0178] [Manufacturing of microporous support membrane]

[0179] Polyethersulfone (PES; manufactured by BASF, trade name Ultrason) and terminal hydroxylated polyethersulfone were dissolved in N-methyl-2-pyrrolidone (manufactured by Wako Pure Chemical Industries, Ltd.) to prepare a hollow fiber spinning stock solution with a polymer concentration of 18.5% by mass. At this time, the ratio of polyethersulfone to terminal hydroxylated polyethersulfone was 55:45. The above stock solution was filled in a wet hollow fiber spinning machine equipped with a double spinneret, extruded into a coagulation tank filled with water, and hollow fibers were formed by phase separation. The obtained hollow fibers were wound in a winding machine. The outer diameter of the obtained hollow fibers was 1.0 mm and the inner diameter was 0.70 mm. The water permeability was 2,392 kg / (m 2 × hr) / 100 kPa. The hollow fiber was used as a microporous hollow fiber support membrane.

[0180] [Manufacturing of supporting membrane modules]

[0181] 1750 microporous hollow fiber support membranes were filled into a 5 cm diameter, 50 cm long cylindrical plastic shell to produce an effective membrane with an inner surface area of ​​1.65 m 2 of, Figure 1 Support membrane assembly shown.

[0182] [Coating of separation active layer]

[0183] An aqueous solution (first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (second solution) containing 0.17% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and then 70°C hot water was circulated through the inner side of the hollow fiber at a flow rate of 1.5 L / min for 30 minutes, and further washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly.

[0184] [Measurement of water permeability F1 and salt reverse diffusion amount R1 of forward osmosis membrane module]

[0185] The tank of 100L loaded with 60L pure water is connected to the inner conduit (hollow fiber inner side) of the obtained forward osmosis membrane assembly by piping, and the pure water is circulated (raw liquid) by pump. A conductivity meter is equipped in the tank to measure the movement of salt in the pure water. On the other hand, the tank of 100L loaded with 60L of 3.5 mass % sodium chloride aqueous solution is connected to the outer conduit (hollow fiber outer side) by piping, and the sodium chloride aqueous solution is circulated (driving solution) by pump. The tanks of the inside and outside are respectively arranged on a balance, and the movement of water is measured. The flow rate of pure water is 2.2L / minute, the flow rate of sodium chloride aqueous solution is 8.8L / minute and is operated simultaneously, and the movement of water and salt after 60 minutes is measured respectively. In the determination, the driving solution of saturated concentration is added little by little in the dilute driving solution, thus set to keep the initial concentration, and measured at 25 ° C. These operations were performed at least five times, and the average values ​​thereof were used to calculate the water permeation rate F1 and the salt reverse diffusion rate R1 of the forward osmosis membrane according to equations (1) and (2).

[0186] R=G / (M×H) ···Formula (1)

[0187] Here, G is the amount of solute that permeates from the draw solution side to the feed solution side (g), and M is the effective surface area of ​​the forward osmosis membrane (m 2 ), and H is time (hr).

[0188] F=L / (M×H) ···Formula (2)

[0189] Here, L is the amount of water permeating from the feed solution side to the draw solution side (kg), and M is the effective surface area of ​​the forward osmosis membrane (m 2), and H is time (hr).

[0190] The results are shown in Table 1.

[0191] [Measurement of Salt Permeability R2 / F2 of Forward Osmosis Membrane Module]

[0192] The tank of 100L of the 20 mass % sodium chloride aqueous solution of 60L is connected with the inner conduit of the forward osmosis membrane assembly obtained by pipe arrangement, and the sodium chloride aqueous solution is circulated (the raw liquid 2 in the table) by pump. On the other hand, the tank of 100L of the 35 mass % magnesium chloride aqueous solution of 60L is connected with the outer conduit by pipe arrangement, and the magnesium chloride aqueous solution is circulated (the driving solution 2 in the table) by pump. The tank of the inside and the outside is respectively arranged on a balance, and the moving amount of water is measured. If the flow rate of sodium chloride aqueous solution is 2.2L / minute, the flow rate of magnesium chloride aqueous solution is 8.8L / minute and is operated simultaneously, the moving amount of water and each salt after 60 minutes is measured respectively. In the determination, the driving solution of saturated concentration is added a little bit in the driving solution of dilution, thus set to keep initial concentration, measured at 25 ℃. In order to calculate the amount of salt migration, an inductively coupled plasma-mass spectrometry (ICP-MS) device, model "iCAP Q" manufactured by Thermo Fisher Scientific, Inc. was used to analyze the cations (Mg from magnesium chloride as the solute of the draw solution). 2+ ions) were measured. These operations were performed at least 5 times, and the average values ​​were used to calculate the water permeation F2 and the salt reverse diffusion R2 of the forward osmosis membrane according to equations (1) and (2). R2 was divided by F2 to calculate the salt permeability R2 / F2. The results are shown in Table 1.

[0193] [Scanning electron microscope observation of separation active layer, average thickness, and measurement of coefficient of variation]

[0194] The forward osmosis membrane modules obtained in each embodiment and comparative example were disassembled, and one hollow fiber was sampled from three locations, namely, the center in the radial direction of the module, the position of 50% of the radius, and the outermost periphery. Each hollow fiber was divided into three equal parts along the length direction to obtain nine samples. These hollow fiber samples were frozen and cut to prepare hollow fiber cross-section samples.

[0195] Here, the preparation of samples by freeze-fracture was performed as follows.

[0196] The hollow fiber was immersed in ethanol (manufactured by Wako Pure Chemical Industries, Ltd.), sealed in gelatin capsule No. 00 (manufactured by Wako Pure Chemical Industries, Ltd.) together with ethanol, and then immersed in liquid nitrogen for 5 minutes for freezing. The hollow fiber was cut together with the frozen capsule using a chisel and a hammer. And the cut product obtained was freeze-dried to obtain a hollow fiber cross-section sample for scanning electron microscope observation. The above cross-section samples were observed by scanning electron microscope respectively. The scanning electron microscope observation was carried out using model S-4800 manufactured by Hitachi, Ltd., under the conditions of accelerating voltage 1.0kV, WD5mm reference ±0.7mm, and emission current set to 10±1μA. The microscope image was printed on paper using a printer, the separation active layer portion was cut, and its mass was measured using a precision balance. The mass was converted into the thickness (μm) of the separation active layer using a pre-made calibration curve. And the average value of the 9 samples was taken as the average thickness of the separation active layer, and the coefficient of variation was calculated. The results are shown in Table 1.

[0197] [Simulated sap concentration]

[0198] Magnesium chloride was added to a 10 mass % sucrose aqueous solution, and the Mg content of the solution was adjusted to 2+ The ion concentration is diluted in a manner of 40 mass ppm to make a simulated sap (raw solution). A 1000L tank to which 300L of the raw solution is added is connected to the inner conduit of the forward osmosis membrane assembly obtained by the same method by using a pipe, and a pump is used to circulate the simulated sap. In addition, a 1000L tank to which 500L of a 20 mass % magnesium chloride aqueous solution is added is connected to the outer conduit by using a pipe, and a magnesium chloride aqueous solution (drive solution) is circulated by a pump. Graduations are drawn on the inner and outer tanks in a manner that the amount of internal liquid can be calculated in advance by the liquid level, and the amount of water moved is measured according to the movement of the liquid level of the raw liquid tank. Calculated according to the amount of water moved from the raw liquid to the drive solution, the operation is stopped when about 5 times of concentration is performed (when the raw liquid reaches 60L), and the amount of water and each salt moved is measured respectively. In the determination, a saturated concentration of the drive solution is added little by little to the diluted drive solution, and thus it is set to maintain the initial concentration and is measured at 25°C. In order to calculate the amount of salt migration, the cations (Mg from magnesium chloride as the solute of the draw solution) were measured using an inductively coupled plasma-mass spectrometer (ICP-MS), model “iCAP Q” manufactured by Thermo Fisher Scientific. 2+ ions).

[0199] [Evaluation of Mg concentration after simulated sap concentration: practical application]

[0200] After the concentration of the simulated sap, the obtained forward osmosis membrane module was washed with water for more than 5 hours, and the simulated sap was concentrated again by the same method. The concentration of the simulated sap by 5 times was repeated 5 times.

[0201] As a practical standard, the simulated sap was concentrated five times and the Mg content diffused from the draw solution into the raw material solution was evaluated according to the following criteria AA to C. 2+ The results are shown in Table 1.

[0202] AA: Mg in the concentrated raw material solution 2+ When the ion concentration is less than 500 mass ppm

[0203] A: Mg in the concentrated raw material solution 2+ When the ion concentration is 500 mass ppm or more and less than 1500 mass ppm

[0204] B: Mg in the concentrated raw material solution 2+ When the ion concentration is 1500 mass ppm or more and less than 2500 mass ppm

[0205] C: Mg in the concentrated raw material solution 2+ When the ion concentration is 2500 mass ppm or more

[0206] It should be noted that, in the case of ideal concentration and the driving solution not diffusing into the raw material solution, Mg 2+ The ion concentration was 200 mass ppm.

[0207] [R1 / F1 evaluation after 20 times of simulated sap concentration: durability]

[0208] After the concentration of the simulated sap, the forward osmosis membrane module was washed with water for more than 5 hours, and the simulated sap was concentrated again by the same method, and the concentration of the simulated sap was repeated 20 times. As a standard of durability, after the 20th concentration, the forward osmosis membrane module was washed with water, and then R1 / F1 was calculated again by the same method as in Example 1, and evaluated according to the following criteria A to C. The results are shown in Table 1.

[0209] A: When R1 / F1 is less than 0.15

[0210] B: R1 / F1 is greater than 0.15 and less than 0.25

[0211] C: R1 / F1 greater than 0.25

[0212] [Example 2]

[0213] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0214] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface side of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.13% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and then 85°C hot water was circulated through the inner side of the hollow fiber for 30 minutes, and further washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly. The results are shown in Table 1.

[0215] [Example 3]

[0216] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0217] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.15% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and then 95°C hot water was circulated through the inner side of the hollow fiber for 30 minutes, and further washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly. The results are shown in Table 1.

[0218] [Example 4]

[0219] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0220] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution, and then air was circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. Thereafter, a n-hexane solution (the second solution) containing 0.20% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. Thereafter, the remaining n-hexane solution was removed by circulating nitrogen, and then hot water at 70°C was circulated inside the hollow fiber for 30 minutes. The assembly was then placed in an autoclave (ES-315 manufactured by Tomy Seiko) and high-temperature steam at 100°C was supplied for 20 minutes. The assembly was further washed with water at 20°C for more than 30 minutes to obtain a forward osmosis membrane assembly. The results are shown in Table 1.

[0221] [Example 5]

[0222] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0223] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.13% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and the assembly was then loaded into an autoclave (ES-315 manufactured by Tomy Seiko) and high-temperature steam at 121°C was supplied for 20 minutes. The membrane was further washed with water at 20° C. for 30 minutes or longer to obtain a forward osmosis membrane module.

[0224] [Example 6]

[0225] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0226] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution, and then air was circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. Thereafter, a n-hexane solution (the second solution) containing 0.20% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. Thereafter, the remaining n-hexane solution was removed by circulating nitrogen, and then hot water at 70°C was circulated inside the hollow fiber for 30 minutes. The assembly was then placed in an autoclave (ES-315 manufactured by Tomy Seiko) and high-temperature steam at 132°C was supplied for 20 minutes. The assembly was further washed with water at 20°C for more than 30 minutes to obtain a forward osmosis membrane assembly. The results are shown in Table 1.

[0227] [Example 7]

[0228] The evaluation was carried out under the same conditions as in Example 4 except that the microporous support membrane was polyketone hollow fiber. A polyketone hollow fiber membrane module was produced as follows.

[0229] A polyketone having an intrinsic viscosity of 3.0 dl / g obtained by complete alternating copolymerization of ethylene and carbon monoxide was added to a 63% by mass aqueous solution of resorcinol having a polymer concentration of 17% by mass, dissolved with stirring at 80°C for 2 hours, and degassed to obtain a uniform transparent stock solution.

[0230] The above stock solution was filled into a wet hollow fiber spinning machine equipped with a double spinneret at 50°C, extruded into a coagulation tank filled with a 40% by mass methanol aqueous solution, and formed into hollow fibers by phase separation. The obtained hollow fibers were wound in a winding machine. The outer diameter of the obtained hollow fibers was 0.6 mm and the inner diameter was 0.35 mm. 3500 of the obtained microporous hollow fiber support membranes were filled into a cylindrical plastic shell with a diameter of 5 cm and a length of 50 cm to produce an effective membrane with an inner surface area of ​​1.65 m 2 of Figure 1 The results are shown in Table 1.

[0231] [Example 8]

[0232] The evaluation was carried out under the same conditions as in Example 4 except that the microporous support membrane was polybenzimidazole hollow fiber. A polybenzimidazole hollow fiber membrane module was produced as follows.

[0233] Polybenzimidazole (PBI; manufactured by Performance Products) was dissolved in DMAc (manufactured by Wako Pure Chemical Industries, Ltd.) and 1.4 mass % LiCl to prepare a hollow fiber spinning stock solution with a polymer concentration of 18 mass %. The stock solution was filled into a wet hollow fiber spinning machine equipped with a double spinneret, extruded into a coagulation tank filled with water, and hollow fibers were formed by phase separation. The obtained hollow fibers were wound in a winding machine. The outer diameter of the obtained hollow fibers was 0.5 mm and the inner diameter was 0.35 mm. The hollow fibers were used as support membranes. 3500 of the obtained microporous hollow fiber support membranes were filled into a cylindrical plastic shell with a diameter of 5 cm and a length of 50 cm to produce an effective membrane with an inner surface area of ​​1.65 m 2 of Figure 1 The results are shown in Table 1.

[0234] [Example 9]

[0235] The evaluation was carried out under the same conditions as in Example 4 except that the microporous support membrane was polysulfone hollow fiber. A polysulfone hollow fiber membrane module was produced as follows.

[0236] Polysulfone (P-3500 manufactured by Amoco) was dissolved in N-methyl-2-pyrrolidone (manufactured by Wako Pure Chemical Industries, Ltd.) at 19% by mass to prepare a hollow fiber spinning solution. The above-mentioned solution was filled into a wet hollow fiber spinning machine equipped with a double spinneret, extruded into a coagulation tank filled with water, and hollow fibers were formed by phase separation. The obtained hollow fibers were wound in a winding machine. The outer diameter of the obtained hollow fibers was 1.0 mm and the inner diameter was 0.70 mm. The hollow fibers were used as microporous hollow fiber support membranes. 1750 microporous hollow fiber support membranes obtained were filled into a cylindrical plastic shell with a diameter of 5 cm and a length of 50 cm to produce an effective membrane with an inner surface area of ​​1.65 m 2 of Figure 1 The results are shown in Table 1.

[0237] [Example 10]

[0238] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Example 4 except that the raw solution 2 in the table was a 10 mass % sodium chloride aqueous solution and the draw solution 2 in the table was a 20 mass % magnesium chloride aqueous solution. The results are shown in Table 1.

[0239] [Example 11]

[0240] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Example 4 except that the raw solution 2 in the table was a 15 mass % potassium chloride aqueous solution and the draw solution 2 in the table was a 35 mass % magnesium chloride aqueous solution. The results are shown in Table 1.

[0241] [Example 12]

[0242] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Example 4 except that the raw solution 2 in the table was a 15 mass % sucrose aqueous solution and the draw solution 2 in the table was a 15 mass % magnesium chloride aqueous solution. The results are shown in Table 1.

[0243] [Example 13]

[0244] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Example 4 except that the raw solution 2 in the table was a 15 mass % sucrose aqueous solution and the draw solution 2 in the table was a 15 mass % sodium chloride aqueous solution. The results are shown in Table 1.

[0245] [Example 14]

[0246] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Example 4 except that the raw solution 2 in the table was pure water and the draw solution 2 in the table was a 35 mass % magnesium chloride aqueous solution. The results are shown in Table 1.

[0247] [Comparative Example 1]

[0248] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0249] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned supporting membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the supporting membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.13% by mass of 1,3,5-triphenylethylene dichloride was then passed through at a flow rate of 1.75 L / min for 3 minutes to coat the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen gas, and the forward osmosis membrane assembly was obtained by washing with water at 20°C for more than 30 minutes. The results are shown in Table 1.

[0250] [Comparative Example 2]

[0251] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0252] An aqueous solution (first solution) containing 2.0 mass % of m-phenylenediamine and 0.15 mass % of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (second solution) containing 0.20 mass % of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and dry nitrogen gas heated to 50°C and with a dew point of -55°C was further circulated in the assembly for 30 minutes, and then washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly. The results are shown in Table 1.

[0253] [Comparative Example 3]

[0254] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0255] An aqueous solution (first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (second solution) containing 0.15% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and dry nitrogen gas heated to 80°C and with a dew point of -55°C was further circulated in the assembly for 2 hours, and then washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly. The results are shown in Table 1.

[0256] [Comparative Example 4]

[0257] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0258] An aqueous solution (first solution) containing 2.0 mass % of m-phenylenediamine and 0.15 mass % of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (second solution) containing 0.14 mass % of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and dry nitrogen gas heated to 100°C and with a dew point of -55°C was further circulated in the assembly for 30 minutes, and then washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly. The results are shown in Table 1.

[0259] [Comparative Example 5]

[0260] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0261] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100 L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.15% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75 L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and then 50°C hot water was circulated through the inner side of the hollow fiber for 30 minutes, and further washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly. The results are shown in Table 1.

[0262] [Comparative Example 6]

[0263] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0264] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 5kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 100L / min for 1 hour to remove the remaining first solution. A 0.20% by mass n-hexane solution (the second solution) containing 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.75L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and then 85°C hot water was circulated through the inner side of the hollow fiber for 30 minutes, and further washed with water at 20°C for more than 30 minutes, thereby obtaining a forward osmosis membrane assembly. The results are shown in Table 1.

[0265] [Comparative Example 7]

[0266] Evaluation was carried out under the same conditions as in Example 1 except that the separation active layer was applied as follows.

[0267] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.15% by mass of sodium lauryl sulfate was passed through the inner surface side of the hollow fiber of the above-mentioned support membrane assembly for 40 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 5kPaG while the inner side of the hollow fiber was wetted by the first solution. The air was then circulated at a flow rate of 100L / min for 10 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.15% by mass of 1,3,5-triphenylethylene dichloride was then passed through at a flow rate of 1.75L / min for 3 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and the hollow fiber membrane assembly was then immersed in hot water at 95°C for 30 minutes, and further washed with water at 20°C for more than 30 minutes to obtain a forward osmosis membrane assembly. The results are shown in Table 1.

[0268] [Comparative Example 8]

[0269] An aqueous solution containing 2.2% by mass of m-phenylenediamine, 0.10% by mass of sodium lauryl sulfate, 2.2% by mass of triethylamine, and 4.4% by mass of camphorsulfonic acid is brought into contact with a flat membrane-like support membrane composed of a polysulfone porous body and a non-woven fabric. The excess solution is then removed. A n-hexane solution containing 0.19% by mass of 1,3,5-benzene trimesoyl chloride is brought into contact with the surface of the support membrane for 3 minutes. It is then kept in a dryer at 120°C for 5 minutes to form a separation active layer on the support membrane to obtain a composite reverse osmosis membrane. The composite reverse osmosis membrane is further immersed in hot water at 85°C for 30 minutes. A 1.6m 2 The reverse osmosis membrane assembly was prepared. With reference to Example 1, the flow rate was set in the same manner as in Example 1, and the evaluation was performed under the same other conditions. At this time, the raw material solution was supplied to the separation active layer side, and the driving solution was supplied to the support membrane side, thereby performing the treatment by the forward osmosis method. The results are shown in Table 1.

[0270] Since Comparative Example 8 is a flat membrane, the column of the coefficient of variation related to the average thickness of the hollow fibers is indicated as "-" (not evaluated) in the table.

[0271] [Comparative Example 9]

[0272] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Comparative Example 4 except that the raw solution 2 in the table was a 15 mass % sucrose aqueous solution and the draw solution 2 in the table was a 15 mass % magnesium chloride aqueous solution. The results are shown in Table 1.

[0273] [Comparative Example 10]

[0274] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Comparative Example 1 except that the raw solution 2 in the table was a 15 mass % sucrose aqueous solution and the draw solution 2 in the table was a 15 mass % sodium chloride aqueous solution. The results are shown in Table 1.

[0275] [Comparative Example 11]

[0276] In the measurement of the salt permeability R2 / F2 of the forward osmosis membrane module, the evaluation was carried out under the same conditions as in Comparative Example 1 except that the raw material solution 2 in the table was pure water and the draw solution 2 in the table was a 35 mass % magnesium chloride aqueous solution. The results are shown in Table 1.

[0277] [Comparative Example 12]

[0278] An aqueous solution containing 2.0% by mass of m-phenylenediamine and 0.10% by mass of sodium lauryl sulfate was brought into contact with a flat membrane-like support membrane composed of an acetylated cellulose ether porous body and a nonwoven fabric. The excess solution was then removed. A n-hexane solution containing 0.20% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was brought into contact with the surface of the support membrane for 3 minutes. The membrane was then kept in a dryer at 120°C for 5 minutes to form a separation active layer on the support membrane to obtain a composite membrane. A 1.0 m 2 The membrane module was evaluated in the same manner as in Comparative Example 8. At this time, the raw material solution was supplied to the separation active layer side and the driving solution was supplied to the support membrane side, and the treatment was performed by the forward osmosis method. The results are shown in Table 1.

[0279] Since Comparative Example 12 is a flat membrane, the column of the coefficient of variation related to the average thickness of the hollow fibers is indicated as "-" (not evaluated) in the table.

[0280] [Comparative Example 13]

[0281] Cellulose triacetate, N-methyl-2-pyrrolidone, ethylene glycol, and benzoic acid are uniformly dissolved to prepare a hollow fiber spinning solution. The above-mentioned solution is filled into a spinning machine equipped with a three-partition nozzle, extruded into a water tank containing N-methyl-2-pyrrolidone, and a hollow fiber is formed by phase separation. The obtained hollow fiber is wound in a winding machine. The outer diameter of the obtained hollow fiber is 0.15mm and the inner diameter is 0.07mm. The hollow fibers are bundled and made into a membrane assembly. With reference to Example 1, the flow rate is set in the same manner as in Example 1 according to the pressure applied to the inside and outside of the hollow fiber, and the evaluation is carried out under the same conditions. At this time, the raw material solution is supplied to the dense layer side located at the periphery of the hollow fiber, and the driving solution is supplied to the inside of the hollow fiber, and the forward osmosis method is used for treatment.

[0282] Comparative Example 13 is an asymmetric membrane composed of a single substance rather than a composite membrane, and therefore the column of coefficient of variation related to the average thickness of the hollow fibers is indicated as "-" (not evaluated) in the table.

[0283] [Example 15]

[0284] The evaluation was carried out under the same conditions as in Example 5 except that the microporous support membrane was made of polysulfone hollow fiber.

[0285] [Example 16]

[0286] The evaluation was carried out under the same conditions as in Example 6 except that the microporous support membrane was made of polysulfone hollow fiber.

[0287] [Example 17]

[0288] Evaluation was carried out under the same conditions as in Example 9 except that the coating of the separation active layer was performed as follows.

[0289] An aqueous solution (the first solution) containing 2.5% by mass of m-phenylenediamine and 0.10% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 30 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 70 L / min for 3 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.18% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.5 L / min for 10 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. The remaining n-hexane solution was then removed by circulating nitrogen, and then 85°C hot water was circulated inside the hollow fiber for 30 minutes. The assembly was then loaded into an autoclave (ES-315 manufactured by Tomy Seiko) and high-temperature steam at 125°C was supplied for 60 minutes. The membrane was further washed with water at 20° C. for 30 minutes or longer to obtain a forward osmosis membrane module.

[0290] [Example 18]

[0291] Evaluation was carried out under the same conditions as in Example 9 except that the coating of the separation active layer was performed as follows.

[0292] An aqueous solution (the first solution) containing 2.0% by mass of m-phenylenediamine and 0.17% by mass of sodium lauryl sulfate was passed through the inner surface of the hollow fiber of the above-mentioned support membrane assembly for 20 minutes. The liquid was then discharged, and the outer side of the support membrane assembly was depressurized and maintained at 90 kPaG while the inner side of the hollow fiber was wetted by the first solution. Air was then circulated at a flow rate of 110 L / min for 2 minutes to remove the remaining first solution. A n-hexane solution (the second solution) containing 0.21% by mass of 1,3,5-trimethylbenzenecarboxylic acid chloride was then passed through at a flow rate of 1.9 L / min for 2 minutes, thereby coating the inner surface of the hollow fiber with a separation active layer by interfacial polymerization. Thereafter, the remaining n-hexane solution was removed by circulating nitrogen, and then 85°C hot water was circulated inside and outside the hollow fiber for 30 minutes, and then the assembly was placed in an autoclave (ES-315 manufactured by Tomy Seiko) and high-temperature steam at 121°C was supplied for 20 minutes. Further, water washing was performed with 20°C water for more than 24 hours to obtain a forward osmosis membrane assembly. The results are shown in Table 1.

[0293] In any forward osmosis membrane module, the membrane performance R1 / F1 after concentrating the simulated sap multiple times changes from the initial R1 / F1. On the other hand, in the forward osmosis membrane module of this embodiment, by setting the initial F1 and R1 to be within a specific range, even if the simulated sap is used multiple times for concentrating a raw liquid having a liquid property similar to that used in an actual concentration operation, concentration with suppressed diffusion of the driving solution can be performed, and thus the forward osmosis membrane module has high practicality.

[0294] Furthermore, according to the comparison of the membrane performance R1 / F1 after the concentration operation, the forward osmosis membrane module according to one embodiment of the present invention can maintain the membrane performance within a desired range even after being used multiple times, and has high durability.

[0295] As one of the methods for producing such a forward osmosis membrane, it is particularly effective to bring a wet and high-temperature liquid or gas into contact in a flowing state.

[0296]

[0297] Explanation of symbols

[0298] 1 Hollow fiber membrane module

[0299] 2 Lateral catheter

[0300] 3 Lateral catheter

[0301] 4 Hollow Fiber

[0302] 5 Adhesive fixing part

[0303] 6 Adhesive fixing part

[0304] 7 Terminal

[0305] 8 Terminal

[0306] 9 Medial catheter

[0307] 10 Medial catheter

Claims

1. A forward osmosis membrane, wherein a separation active layer of a high molecular polymer is provided on the surface of a microporous support membrane, wherein: The microporous support membrane comprises a membrane having at least one selected from the group consisting of polyethersulfone, polysulfone, polyketone, polyetheretherketone, polyphenylene ether, polyvinylidene fluoride, polyacrylonitrile, polyimide, polyimide, polybenzoxazole, polybenzimidazole and polyamide as a main component, The high molecular polymer is a condensation product of one or more first monomers selected from the group consisting of polyfunctional amines and one or more second monomers selected from the group consisting of polyfunctional acyl halides. When pure water as a raw material solution is arranged on the separation active layer side and a 3.5 mass % sodium chloride aqueous solution as a driving solution is arranged on the microporous support membrane side via the forward osmosis membrane, the salt back diffusion amount R1 toward the raw material solution is 0.65 g / (m 2 × hr) or less, and the water permeation F1 toward the draw solution is 3.5 kg / (m 2 ×hr) or above.

2. The forward osmosis membrane according to claim 1, wherein The amount of salt back diffusion R1 toward the raw material liquid is 0.45 g / (m 2 ×hr) or less.

3. The forward osmosis membrane according to claim 1 or 2, wherein The amount of salt back diffusion R1 toward the raw material liquid is 0.30 g / (m 2 ×hr) or less.

4. The forward osmosis membrane according to claim 1 or 2, wherein The water permeation F1 toward the draw solution is 5.0 kg / (m 2 ×hr) or above.

5. The forward osmosis membrane according to claim 1 or 2, wherein The water permeability F1 toward the draw solution is 6.5 kg / (m 2 ×hr) or above.

6. The forward osmosis membrane according to claim 1 or 2, wherein The reverse diffusion amount R1 of the salt toward the raw material liquid is 0.01 g / (m 2 ×hr) or above.

7. The forward osmosis membrane according to claim 1 or 2, wherein The water permeability F1 toward the draw solution is 50 kg / (m 2 ×hr) or less.

8. The forward osmosis membrane according to claim 1 or 2, wherein The value of the ratio R1 / F1 of the amount of salt back diffusion R1 toward the raw solution to the amount of water permeation F1 toward the draw solution is 0.08 or less.

9. The forward osmosis membrane according to claim 1 or 2, wherein The value of the ratio R1 / F1 of the amount of salt back diffusion R1 toward the raw solution to the amount of water permeation F1 toward the draw solution is 0.06 or less.

10. The forward osmosis membrane according to claim 1 or 2, wherein The value of the ratio R1 / F1 of the amount of salt back diffusion R1 toward the raw solution to the amount of water permeation F1 toward the draw solution is 0.04 or less.

11. The forward osmosis membrane according to claim 1 or 2, wherein The microporous support membrane is a membrane containing at least one selected from the group consisting of polyethersulfone, polysulfone, polyketone, and polybenzimidazole as a main component.

12. The forward osmosis membrane according to claim 11, wherein The microporous support membrane is a membrane containing at least one selected from the group consisting of polyethersulfone and polysulfone as a main component.

13. The forward osmosis membrane according to claim 1 or 2, wherein The high molecular polymer is polyamide.

14. The forward osmosis membrane according to claim 1 or 2, wherein The forward osmosis membrane is a hollow fiber.

15. The forward osmosis membrane according to claim 14, wherein The separation active layer is present on the inner surface of the microporous support membrane. 16 . A forward osmosis membrane module incorporating the forward osmosis membrane according to claim 1 .

17. The forward osmosis membrane assembly according to claim 16, wherein: The forward osmosis membrane is a hollow fiber, and the forward osmosis membrane module includes a hollow fiber bundle composed of a plurality of the hollow fibers.

18. The forward osmosis membrane assembly according to claim 17, wherein: In a scanning electron microscope image obtained by photographing a cross section of the separation active layer in the thickness direction, the coefficient of variation of the average thickness of the separation active layer in the radial direction and the longitudinal direction of the hollow fiber bundle is 0 to 60%.

19. A method for manufacturing a forward osmosis membrane module, which is the method for manufacturing a forward osmosis membrane module according to claim 17 or 18, comprising the following steps: a separation active layer forming step of providing a separation active layer on the inner surface of the microporous support membrane; and The heat treatment step is a step of supplying a fluid at 55° C. or higher in a flowing and wet state to at least the inner surface side of the hollow fiber after the separation active layer forming step.

20. The method for manufacturing a forward osmosis membrane module according to claim 19, wherein: The heat treatment step is performed by continuously supplying hot water at a temperature of 70° C. to 95° C. to at least the inner surface side of the hollow fiber.

21. The method for manufacturing a forward osmosis membrane module according to claim 19, wherein: The heat treatment step is performed using steam at a temperature of 100° C. to 150° C.

Citation Information

Patent Citations

  • Forward osmosis treatment system

    JP2016155078A

  • Forward osmosis membrane and method of manufacture

    US20130313185A1

  • Treatment of composite polyamide membranes to improve performance

    WO1999022836A2

  • Composite hollow fiber membrane module and manufacturing method therefor

    WO2016027869A1

  • Method for preparing hollow fiber type forward osmotic membrane

    CN102773024A

Cited By

  • Integrated forward osmosis membrane assembly structure

    CN121869089A