Polypropylene film rolls and metallized polypropylene film rolls
By controlling the hysteresis axis angle and circumference ratio of the polypropylene film roll, the problems of wrinkling and loosening of polypropylene film during transport when it is thin and wide were solved, thus achieving long-term durability and high yield of capacitor elements under high temperature and high voltage.
Patent Information
- Application Number
- CN202080041298.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-08
- Filing Date
- 2020-05-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-05-27
AI Technical Summary
Existing polypropylene films are prone to wrinkling and loosening when transported in thin and wide conditions, resulting in uneven film thickness and making it difficult to maintain the long-term durability and high yield of capacitor components under high temperature and high voltage.
By controlling the hysteresis axis angle difference and circumference ratio of the polypropylene film roll, the high flatness of the polypropylene film is ensured during roll-out, and the high precision is achieved during the metal evaporation process. The resulting capacitor elements exhibit excellent durability and high yield under high temperature and high voltage conditions.
This technology achieves long-term durability and high yield of polypropylene film under high temperature and high voltage conditions, suppresses winding deviation caused by wrinkles and slack, and improves the initial voltage withstand capability and processing accuracy of capacitor elements.
Smart Images

Figure CN113905884B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polypropylene film roll and a metallized polypropylene film roll. Background Art
[0002] In the past, capacitors using resin films have been used in electronic equipment, electrical equipment, and the like as filter capacitors and smoothing capacitors for high voltage capacitors, various switching power supplies, converters, inverters, and the like. In such capacitors, the resin film is used as a dielectric film for capacitors, and the capacitor is formed by, for example, the following methods: (i) a method of making a so-called "metallized film" having a conductive layer such as a metal layer on the dielectric film, for example, by metal evaporation or coating / drying of a metal-containing paste, bonding of metal foil or metal powder, etc.; (ii) laminating the dielectric film without a conductive layer such as a metal layer and other conductors such as a metal foil or a metallized film having a metal layer by the same method as (i). The dielectric film for capacitors is also used as a capacitor for inverter power supply equipment that controls drive motors of electric vehicles and hybrid vehicles, which have been in high demand in recent years.
[0003] For example, polypropylene films used as resin films for capacitors of electric vehicles, hybrid vehicles, etc., have been required to be thinner and have larger electrode areas in recent years due to the miniaturization and higher capacity of capacitors. In addition, in order to reduce costs, it is required to provide a polypropylene film roll in which the processing width of the film is widened and a thin film is finely processed with a wider width.
[0004] However, since polypropylene film is highly flexible, wrinkles and sagging are easily generated when the film is transported in a thin and wide width. The reduction in the flatness of the film during transport causes the thickness of the deposited film to become non-uniform in the deposition step.
[0005] As a technology for suppressing wrinkles in polypropylene film during transportation, for example, Patent Document 1 discloses a polypropylene film roll, which is a film roll formed by winding a polypropylene film around a core, wherein the average hardness of the outermost layer of the roll is 84.0 to 94.0°, and the hardness deviation of the outermost layer of the roll in the width direction is within ±2.0°.
[0006] Patent Document 2 discloses a polypropylene film roll for capacitors, which is a polypropylene film wound around a core, and specifies the difference R between the maximum and minimum values of the roll diameter in the width direction and the difference H between the diameters at both ends of the roll.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2018 / 034182
[0010] Patent Document 2: Japanese Patent Application Publication No. 2015-195367 Summary of the invention
[0011] Problems to be solved by the invention
[0012] In Patent Document 1, by controlling the hardness of the polypropylene film roll to a predetermined value, it is possible to prevent problems such as winding deviation, longitudinal wrinkles, and meandering of the film roll during transportation in the vapor deposition step.
[0013] However, although the hardness of the polypropylene film roll is one of the finishing qualities of the film roll, it is a composite characteristic of various components such as the thickness and hardness of the film itself, the material of the core, the wall thickness, the amount of air between the films, the internal stress, and the friction between the film surfaces. In this way, there are many factors that determine the hardness of the roll, and it is very difficult to distinguish the main factors that determine the hardness of the roll. Therefore, the hardness of the roll is nothing more than a standard for obtaining the finishing quality. Therefore, even if the average value, distribution, deviation, etc. of the hardness of the roll are controlled, it is impossible to fully eliminate the wrinkles and relaxation during processing, and the resulting capacitor element is not necessarily a capacitor element with excellent electrical characteristics.
[0014] Patent Document 2 states that the difference R between the maximum and minimum values of the film roll diameter in the width direction and the difference H in diameter at both ends of the film roll are controlled to predetermined values, respectively, so that the occurrence frequency of winding deviation and other faults can be prevented. However, even if the above R and H of the film roll are controlled, the wrinkle suppression effect and relaxation suppression effect during processing of the film obtained from the film roll, and the electrical characteristics of the obtained capacitor element at high temperature and high voltage are not necessarily excellent.
[0015] Under such circumstances, the main purpose of the invention of the first embodiment is to provide a polypropylene film roll, which can be subjected to metal vapor deposition processing with high precision while maintaining high flatness for the polypropylene film rolled out from the polypropylene film roll, and the obtained capacitor element has excellent initial withstand voltage and long-term durability under high temperature and high voltage, and winding deviation caused by wrinkles and relaxation of the film is also suppressed, so that the capacitor element can be manufactured with a high yield. In addition, the purpose of the invention of the first embodiment is also to provide a metallized polypropylene film roll using the capacitor film roll.
[0016] In addition, the main purpose of the invention of the second embodiment is to provide a polypropylene film roll, which can be used to perform metal vapor deposition processing with high precision while maintaining high flatness on the polypropylene film rolled out from the polypropylene film roll, and the obtained capacitor element has excellent long-term durability under high temperature and high voltage, and the winding deviation caused by wrinkles and slack of the film and the reduction in yield due to cutting are also suppressed, so that the capacitor element can be manufactured with a high yield. In addition, the purpose of the invention of the second embodiment is also to provide a metallized polypropylene film roll using the capacitor film roll.
[0017] Means for solving problems
[0018] The inventors of the present invention have conducted in-depth research to solve the above-mentioned problems of the invention of the first embodiment. As a result, it was found that, in a polypropylene film roll formed by winding a polypropylene film around a core, (1A) the difference between the maximum value and the minimum value of the slow axis angle of the polypropylene film measured under prescribed conditions is set to less than 5°, and (2A) when the circumference is measured at the two end positions, the central position, and the positions at intervals of 50 mm from the central position toward the two end positions of the polypropylene film roll, the ratio ΔX of the difference (Xmax-Xmin) between the maximum value Xmax and the minimum value Xmin of the circumference to the average value Xave of the circumference is set to less than 0.2%, thereby making it possible to perform metal vapor deposition processing on the polypropylene film rolled out from the polypropylene film roll while maintaining high flatness, and the obtained capacitor element has excellent initial withstand voltage and long-term durability under high temperature and high voltage, and can also suppress winding deviation caused by wrinkling and relaxation of the polypropylene film, so that the capacitor element can be manufactured with a high yield.
[0019] In addition, the present inventors have conducted intensive studies in order to solve the above-mentioned problems of the invention according to the second embodiment. As a result, it was found that in a polypropylene film roll obtained by winding a polypropylene film having a thickness of 20 μm or less and a width of 200 mm or more around a core, under the conditions specified in (1B), the shortest distance ΔL from the midpoint of a straight line connecting both ends of a peeling line, i.e., a boundary line for peeling the polypropylene film from the polypropylene film roll, to the peeling line is set to 20 mm or less, and (2B) when the circumference length is measured at both end positions, a central position, and positions at intervals of 50 mm from the central position toward the both end positions of the polypropylene film roll, the ratio ΔX of the difference between the maximum value Xmax and the minimum value Xmin of the circumference length (Xmax-Xmin) to the average value Xave of the circumference length is set to 0.2% or less, the polypropylene film rolled out from the polypropylene film roll can be subjected to metal vapor deposition processing with high precision while maintaining high flatness, and the obtained capacitor element has excellent long-term durability at high temperature and high voltage. In addition, winding deviation due to wrinkling and sag of the polypropylene film and reduction in yield due to cutting are suppressed, and capacitor elements can be manufactured with high yield.
[0020] The present invention has been completed through further research based on the above findings.
[0021] That is, the present invention includes the following aspects.
[0022] Solution 1. A polypropylene film roll, which is formed by winding a polypropylene film around a core, wherein the polypropylene film roll satisfies the following physical properties (1A) and (2A),
[0023] (1A) The difference between the maximum and minimum values of the slow axis angle obtained by the following methods (a) to (c) is less than 5°.
[0024] (a) When the total length in the width direction of the polypropylene film is defined as 100%, nine samples for measurement of 50 mm x 50 mm are cut out, centered at positions every 10% from both ends of the polypropylene film.
[0025] (b) The width direction of the measurement sample is set to 0°, and the acute angle formed by the width direction of the measurement sample and the slow axis is measured as the slow axis angle.
[0026] (c) The difference between the maximum value and the minimum value of the slow axis angle measured in (b) among the nine samples for measurement is determined.
[0027] (2A) When the circumferential length is measured at the two end positions, the center position, and positions at intervals of 50 mm from the center position toward the two end positions of the polypropylene film roll, the ratio ΔX of the difference between the maximum value Xmax and the minimum value Xmin of the circumferential length, i.e., Xmax-Xmin, to the average value Xave of the circumferential length is less than 0.2%.
[0028] Scheme 2. A polypropylene film roll according to Scheme 1, wherein the deformation rate (ε1) in the long side direction, the deformation rate (ε2) in the width direction, and the deformation rate (ε3) in the diagonal direction of the polypropylene film at a stress of 25 MPa are respectively in the range of greater than 0.6% and less than 1.5%.
[0029] Solution 3. The polypropylene film roll according to Solution 1 or 2, wherein the width of the polypropylene film is 200 mm or more.
[0030] Aspect 4. The polypropylene film roll according to any one of aspects 1 to 4, wherein the polypropylene film has a thickness of 6.0 μm or less.
[0031] Scheme 5. A polypropylene film roll, which is formed by winding a polypropylene film around a core,
[0032] The polypropylene film has a thickness of less than 20 μm and a width of more than 200 mm.
[0033] The polypropylene film satisfies the following physical properties (1B) and (2B),
[0034] (1B) when the polypropylene film is unrolled from the polypropylene film roll at an unwinding tension of 3 N / m and a speed of 2 m / min under an environment of a temperature of 23° C. and a humidity of 60%, the shortest distance ΔL from the middle point of a straight line connecting both ends of a peeling line to the peeling line is less than 20 mm, the peeling line being a boundary line at which the polypropylene film is peeled from the polypropylene film roll,
[0035] (2B) When the circumferential length is measured at the two end positions, the center position, and positions at intervals of 50 mm from the center position toward the two end positions of the polypropylene film roll, the ratio ΔX of the difference (Xmax-Xmin) between the maximum value Xmax and the minimum value Xmin of the circumferential length to the average value Xave of the circumferential length is less than 0.2%.
[0036] Scheme 6. A polypropylene film roll according to Scheme 5, wherein when the hardness is measured at the two end positions, the center position, and positions at intervals of 50 mm from the center position toward the two end positions of the polypropylene film roll, the average hardness value Mave is greater than 88° and less than 96°, and the difference ΔM between the maximum hardness value Mmax and the minimum hardness value Mmin is less than 4°.
[0037] Scheme 7. A polypropylene film roll according to Scheme 5 or 6, wherein the deformation rate (ε1) in the long side direction, the deformation rate (ε2) in the width direction, and the deformation rate (ε3) in the diagonal direction of the polypropylene film at a stress of 25 MPa are respectively in the range of greater than 0.6% and less than 1.5%.
[0038] Scheme 8. The polypropylene film roll according to any one of schemes 5 to 7, wherein the surface roughness of at least one surface of the polypropylene film has a center line average roughness (Ra) of 0.04 μm to 0.08 μm, and a maximum height (Rz) of 0.3 μm to 0.9 μm.
[0039] Aspect 9. The polypropylene film roll according to any one of aspects 1 to 8, wherein the polypropylene film has a winding length of 10,000 m or more.
[0040] Aspect 10. The polypropylene film roll according to any one of aspects 1 to 9, wherein the polypropylene film roll is used to produce a metallized polypropylene film for a capacitor by laminating a metal film on one side or both sides of the polypropylene film.
[0041] A metallized polypropylene film roll, wherein a metal film is laminated on one or both sides of the polypropylene film in the polypropylene film roll according to any one of Aspects 1 to 10.
[0042] Effects of the Invention
[0043] According to the invention of the first embodiment, a polypropylene film roll can be provided, which can perform metal vapor deposition processing with high precision on the polypropylene film rolled out from the polypropylene film roll while maintaining high flatness, and the obtained capacitor element has excellent initial withstand voltage and long-term durability under high temperature and high voltage, and winding deviation caused by wrinkles and relaxation of the film is also suppressed, so that the capacitor element can be manufactured with a high yield. In addition, according to the invention of the first embodiment, a metallized polypropylene film roll using the capacitor film roll can also be provided.
[0044] In addition, according to the invention of the second embodiment, a polypropylene film roll can be provided, which can perform metal vapor deposition processing with high precision on the polypropylene film rolled out from the polypropylene film roll while maintaining high flatness, and the obtained capacitor element has excellent long-term durability under high temperature and high voltage, and the winding deviation caused by wrinkles and slack of the film and the reduction of the yield rate due to cutting are also suppressed, so that the capacitor element can be manufactured with a high yield rate. In addition, according to the invention of the second embodiment, a metallized polypropylene film roll using the capacitor film roll can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a schematic diagram for explaining a method of measuring the shortest distance ΔL from the midpoint of a straight line connecting both ends of a peeling line, which is a boundary line where the polypropylene film is peeled from the polypropylene film roll, to the peeling line.
[0046] Figure 2 This is a schematic diagram for explaining a method for producing a polypropylene film roll. DETAILED DESCRIPTION
[0047] The polypropylene film roll according to the first embodiment of the present invention is characterized in that a polypropylene film is wound around a core and satisfies the following physical properties (1A) and (2A).
[0048] (1A) The difference between the maximum and minimum values of the slow axis angle obtained by the following methods (a) to (c) is less than 5°.
[0049] (a) When the total length in the width direction of the polypropylene film is defined as 100%, nine samples for measurement of 50 mm x 50 mm are cut out, centered at positions every 10% from both ends of the polypropylene film.
[0050] (b) The width direction of the measurement sample is set to 0°, and the acute angle formed by the width direction of the measurement sample and the slow axis is measured as the slow axis angle.
[0051] (c) The difference between the maximum value and the minimum value of the slow axis angle measured in (b) above among the nine measurement samples was determined.
[0052] (2A) When the circumferential length is measured at the two end positions, the center position, and positions at intervals of 50 mm from the center position toward the two end positions of the above-mentioned polypropylene film roll, the ratio ΔX of the difference between the maximum value Xmax and the minimum value Xmin of the circumferential length (Xmax-Xmin) to the average value Xave of the circumferential length is less than 0.2%.
[0053] The polypropylene film roll of the first embodiment satisfies the physical properties of (1A) and (2A) above, and can perform metal vapor deposition processing on the polypropylene film rolled out from the polypropylene film roll with high precision while maintaining high flatness. The resulting capacitor element has excellent initial withstand voltage and long-term durability under high temperature and high voltage. In addition, winding deviation caused by wrinkling and relaxation of the film is also suppressed, and capacitor elements can be manufactured with a high yield.
[0054] The polypropylene film roll according to the second embodiment is characterized in that a polypropylene film having a thickness of 20 μm or less and a width of 200 mm or more is wound around a core and that the polypropylene film satisfies the following physical properties (1B) and (2B).
[0055] (1B) When the polypropylene film is unrolled from the polypropylene film roll at a unwinding tension of 3 N / m and a speed of 2 m / min under an environment of a temperature of 23°C and a humidity of 60%, the shortest distance ΔL from the midpoint of a straight line connecting the two ends of a peeling line, i.e., a boundary line at which the polypropylene film is peeled off from the polypropylene film roll, to the peeling line is less than 20 mm.
[0056] (2B) When the circumferential length of the polypropylene film roll is measured at the two end positions, the center position, and the positions with an interval of 50 mm from the center position toward the two end positions, the ratio ΔX of the difference (Xmax-Xmin) between the maximum value Xmax and the minimum value Xmin of the circumferential length to the average value Xave of the circumferential length is less than 0.2%.
[0057] The polypropylene film roll involved in the second embodiment satisfies the above-mentioned thickness and width, and further satisfies the above-mentioned physical properties (1B) and (2B), so that the polypropylene film rolled out from the polypropylene film roll can be subjected to metal vapor deposition processing with high precision while maintaining high flatness. The obtained capacitor element has excellent long-term durability under high temperature and high voltage. In addition, the winding deviation caused by wrinkling and relaxation of the film and the reduction in yield due to cutting are also suppressed, so that the capacitor element can be manufactured with a high yield.
[0058] The following is a detailed description of the polypropylene film roll involved in the first embodiment and the second embodiment, the metallized polypropylene film roll using the polypropylene film roll, and the capacitor element. It should be noted that in this specification, "~" in the numerical range refers to above and below. That is, the expression α~β means above α and below β, or above β and below α, including α and β as a range. In addition, in this specification, the "mass %" indicating the content rate of each component indicates the ratio of the content when the amorphous thermoplastic resin film is set to 100 mass %, unless otherwise specified.
[0059] In addition, in this specification, the expression "capacitor" includes concepts such as "capacitor", "capacitor element" and "film capacitor". In addition, sometimes "polypropylene film" is abbreviated as "film", "polypropylene film roll" is abbreviated as "film roll", "metallized polypropylene film" is abbreviated as "metallized film", and "metallized polypropylene film roll" is abbreviated as "metallized film roll". In addition, in the polypropylene film roll of the first embodiment and the second embodiment, the polypropylene film is not a microporous film and therefore does not have a plurality of pores. In addition, the polypropylene film may be composed of multiple layers of two or more layers, but is preferably composed of a single layer.
[0060] <1A. Polypropylene film roll according to first embodiment>
[0061] The polypropylene film roll according to the first embodiment is characterized in that a polypropylene film is wound around a core and satisfies the above-mentioned physical properties (1A) and (2A).
[0062] The physical property of (1A) is a physical property related to the slow phase axis angle of the polypropylene film. The biaxially stretched polypropylene film is stretched in a first direction and a second direction orthogonal thereto. The polypropylene film is oriented in the plane by biaxial stretching, so it has birefringence. In the plane of the polypropylene film, the direction with the largest refractive index becomes the direction where the speed of light travels slowly (phase delay), so it is called the slow phase axis.
[0063] For example, in the sequential biaxial stretching method, first, the cast green sheet is stretched in the flow direction (MD direction), and then the sheet is stretched in the transverse direction (TD direction (width direction)). In this case, regarding the slow axis of the biaxially stretched polypropylene film, there is a tendency that the refractive index in the transverse direction of the second direction is greater than the refractive index in the flow direction of the first direction. Here, the transverse direction of the second direction is the slow axis.
[0064] In the transverse (TD) stretching, when the stretching is performed completely in the transverse direction (when the stretching is performed completely in the direction orthogonal to the flow direction), the lag axis angle defined in this specification is 0°. However, in reality, Poisson shrinkage stress, mechanical external force, thermoplasticity of the film, etc. act during stretching, and it is impossible to stretch completely in the transverse (TD direction), and there is a tendency for the lag axis angle to be greater than 0°. In addition, in the sequential biaxial stretching method, there is a tendency for the lag axis angle to be larger at both ends of the biaxially stretched film.
[0065] In the first embodiment, it can be said that the smaller the difference between the maximum and minimum values of the above-mentioned slow axis angle, the smaller the deviation of the orientation of the optical orientation axis in the two orthogonal directions of the flow direction (MD direction) of the first direction and the transverse direction (TD direction) of the second direction. Therefore, when the metallized film is produced, the shrinkage in the oblique direction during heating becomes less, and it is easy to achieve uniform heat shrinkage in the first direction and the second direction. As a result, wrinkles and relaxation during processing can be suppressed, and the film can be used appropriately.
[0066] The difference between the maximum and minimum values of the lag axis angle in the first embodiment is not the anisotropy of the optical orientation intensity represented by birefringence, etc., that is, it is not the size and direction of the orientation itself, but represents the angle formed by the maximum and minimum values of the second direction and the lag axis, that is, the variation range of the lag axis angle in the width direction. In the first embodiment, it is preferred to control the above difference to be smaller in the roll width direction (processing width direction). The reason why the above difference is preferably controlled to be smaller is that even if a certain mechanical processing strength is given to the polypropylene as a soft raw material based on the orientation strength of biaxial stretching, the thermal dimensional change caused by the metal vapor deposition process cannot be fully reduced. Instead, the deviation of the orientation direction in the roll width direction is suppressed, and the variation contributes to the uniformity of the shrinkage direction in the in-plane direction, so that a metallized film with less uneven vapor deposition film can be obtained.
[0067] The capacitor element thus obtained has excellent initial withstand voltage and long-term durability under high temperature and high voltage. In addition, the polypropylene film roll can be used as a roll that significantly eliminates winding deviation caused by wrinkles and slack during processing, has excellent yield of capacitor elements, and is cost-effective.
[0068] In the polypropylene film roll involved in the first embodiment, the difference between the maximum and minimum values of the lag axis angle of the polypropylene film is set to less than 5°, and the physical property (2A) described later is also satisfied (the ratio ΔX of the circumferential length of the polypropylene film roll is set to less than 0.2%), so that the polypropylene film rolled out from the polypropylene film roll can be subjected to metal vapor deposition processing with high precision while maintaining high flatness, and the deviation of the film thickness of the metal film can be suppressed. Furthermore, the capacitor element obtained from the polypropylene film has excellent initial withstand voltage and long-term durability under high temperature and high voltage. In addition, the winding deviation caused by the wrinkling and relaxation of the film is also suppressed, and the capacitor element can be manufactured with a high yield.
[0069] Although the difference between the maximum and minimum values of the lag axis angle is less than 5°, the metal vapor deposition process is carried out with high precision while maintaining higher flatness for the polypropylene film rolled out from the polypropylene film roll, and the initial withstand voltage of the capacitor element and the long-term durability under high temperature and high voltage are further improved, and the winding deviation caused by the wrinkles and relaxation of the polypropylene film is suppressed, and the capacitor element is manufactured with a higher yield. From the point of view, it is preferably 4.5° or less, more preferably 4.0° or less, and further preferably 3.0° or less. It should be noted that the lower limit of the difference between the maximum and minimum values of the lag axis angle is 0°.
[0070] The difference between the maximum value and the minimum value of the slow axis angle of the polypropylene film can be measured by the method described in Examples.
[0071] When the circumference of the physical property (2A) is measured at the two end positions, the center position, and positions at intervals of 50 mm from the center position toward the two end positions of the polypropylene film roll, the ratio ΔX ((Xmax-Xmin) / Xave) of the difference between the maximum value Xmax and the minimum value Xmin of the circumferential length (Xmax-Xmin) to the average value Xave of the circumferential length is less than 0.2%.
[0072] In the polypropylene film roll of the first embodiment, the ratio ΔX of the circumference length can be 0.2% or less, but from the above viewpoint, it is preferably 0.19% or less, more preferably 0.18% or less, and further preferably 0.17% or less. In addition, the lower limit of the ratio ΔX of the circumference length can be, for example, 0.00%, 0.01%, etc.
[0073] The ratio ΔX of the circumferential length of the polypropylene film roll can be measured by the method described in Examples.
[0074] In addition, regarding the peeling line formed when the polypropylene film is unwound from the polypropylene film roll according to the first embodiment under predetermined conditions, the shortest distance ΔL from the middle point of the straight line connecting the two ends of the peeling line to the peeling line is preferably 20 mm or less. Figure 1 As shown in the schematic diagram of , the peeling line S is the boundary line between the portion of the polypropylene film 1 peeled off from the polypropylene film roll 10 and the portion that is not peeled off. Generally speaking, when the polypropylene film is rolled out from the polypropylene film roll, the peeling line is not straight in the width direction x, but is formed in a manner of describing an arc (an arc of the peeling line S toward the rolling-out direction L) from one end to the other end of the width direction x of the polypropylene film (that is, from one end x1 of the peeling line to the other end x2). The thinner the thickness of the polypropylene film roll and the wider the width, the larger the shortest distance ΔL of the peeling line. It should be noted that when the polypropylene film roll is visually confirmed from above, the peeled portion and the unpeeled portion of the transparent polypropylene film roll have different appearances across the boundary line, so the peeling line can be identified visually.
[0075] The shortest distance ΔL of the peeling line of the polypropylene film roll can be measured by the method described in Examples.
[0076] From the above viewpoints, in the polypropylene film roll involved in the first embodiment, the shortest distance ΔL of the peeling line is preferably 20 mm or less, more preferably 17 mm or less, further preferably 14 mm or less, and particularly preferably 10 mm or less. In addition, the lower limit of the shortest distance ΔL of the peeling line can be, for example, 0 mm, 2 mm, etc.
[0077] In addition, from the above-mentioned viewpoints, in the polypropylene film roll involved in the first embodiment, the deformation rate (ε1) in the longitudinal direction (MD), the deformation rate (ε2) in the width direction (TD) and the deformation rate (ε3) in the diagonal direction (45°) of the polypropylene film when the stress is 25 MPa are preferably in the range of 0.6 to 1.5%, more preferably in the range of 0.6 to 1.4%, and further preferably in the range of 0.6 to 1.3%.
[0078] The deformation rate of the polypropylene film is a value measured on the polypropylene film unwound from the polypropylene film roll, and can be specifically measured by the method described in Examples.
[0079] In the polypropylene film roll according to the first embodiment, the thickness of the polypropylene film is, for example, 6.0 μm or less. For a polypropylene film roll wound with a thin polypropylene film, from the viewpoint of appropriately satisfying the physical properties of (1A) and (2A) above, it is preferably 4.0 μm or less, more preferably 3.0 μm or less, further preferably 2.8 μm or less, and particularly preferably 2.5 μm or less. Furthermore, from the viewpoint of appropriately satisfying the physical properties of (1A) and (2A) above, it is preferably 0.5 μm or more, more preferably 1.0 μm or more, and further preferably 1.5 μm or more.
[0080] In the polypropylene film roll involved in the first embodiment, the width of the polypropylene film can be 200 mm or more. However, from the viewpoint of appropriately satisfying the physical properties of (1A) and (2A) above, for a polypropylene film roll wound with a wider polypropylene film, the width is preferably 400 mm or more, more preferably 600 mm or more, and the preferred range is 600 to 1200 mm, and further 600 to 1000 mm.
[0081] In the polypropylene film roll of the first embodiment, the winding length of the polypropylene film is not particularly limited, and may be, for example, 10000 m or more, more preferably 30000 m or more. The upper limit of the winding length of the polypropylene film may be, for example, 100000 m.
[0082] The polypropylene film wound around the polypropylene film roll according to the first embodiment is preferably a biaxially stretched polypropylene film. From the viewpoint of appropriately satisfying the physical properties of (1A) and (2A) above, the preferred stretching ratio (longitudinal stretching ratio, transverse stretching ratio) of the biaxially stretched polypropylene film and the tenter inlet speed ratio in the sequential biaxial stretching method are as described in the column <2. Method for producing a polypropylene film roll> described later.
[0083] As described later, the physical properties of (1A) and (2A) are affected by the stretching conditions of the polypropylene film, etc. The physical properties of (1A) and (2A) can be adjusted by adjusting the stretching temperature and stretching ratio when stretching in the flow direction (hereinafter, also referred to as "longitudinal stretching temperature" and "longitudinal stretching ratio", respectively), the stretching temperature, stretching ratio and stretching angle when stretching in the width direction (hereinafter, also referred to as "transverse stretching temperature", "transverse stretching ratio" and "transverse stretching angle", respectively), the tenter inlet speed ratio in the sequential biaxial stretching method, etc. It should be noted that examples of preferred stretching conditions in the first embodiment will be described later in the column <2A. Method for manufacturing a polypropylene film roll involved in the first embodiment>. In addition, in this specification, "longitudinal" and "flow direction" are synonymous, and "transverse" and "width direction" are synonymous.
[0084] The polypropylene film wound by the polypropylene film roll involved in the first embodiment contains a polypropylene resin as a resin. Preferably, the main component of the polypropylene film is a polypropylene resin, and more preferably, the resin component constituting the film is a polypropylene resin. It should be noted that the above-mentioned "main component" refers to a resin as a main component containing 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and particularly preferably 99% by mass or more in terms of solid content in the polypropylene film. The polypropylene resin contained in the polypropylene film is described in detail below.
[0085] <Polypropylene resin>
[0086] The polypropylene resin is not particularly limited as long as a polypropylene film roll having the physical properties of (1A) and (2A) can be obtained, and a wide range of resins that can be used to form polypropylene films can be used. Examples of the polypropylene resin include propylene homopolymers such as isotactic polypropylene and syndiotactic polypropylene; copolymers of propylene and ethylene; long-chain branched polypropylene; ultra-high molecular weight polypropylene, etc., preferably propylene homopolymers, among which isotactic polypropylene is more preferably exemplified from the viewpoint of heat resistance, and further preferably isotactic polypropylene obtained by homopolymerizing polypropylene in the presence of an olefin polymerization catalyst. The polypropylene resin may be used alone or in combination of two or more.
[0087] The weight average molecular weight (Mw) of the polypropylene resin is preferably 250,000 to 450,000. If such a polypropylene resin is used, appropriate resin fluidity is obtained during biaxial stretching, and the thickness of the cast green sheet is easily controlled. For example, it is easy to obtain an extremely thin biaxially stretched polypropylene film suitable for small and high-capacity capacitors, so it is preferred. In addition, it is difficult to produce uneven thickness of the cast green sheet and the biaxially stretched polypropylene film, so it is preferred.
[0088] The molecular weight distribution (Mw / Mn) calculated as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the polypropylene resin is preferably 7 or more and 12 or less. In addition, the molecular weight distribution (Mw / Mn) is more preferably 7.1 or more, further preferably 7.5 or more, and particularly preferably 8 or more. Further, the molecular weight distribution (Mw / Mn) is more preferably 11 or less, and further preferably 10 or less. If such a polypropylene resin is used, appropriate resin fluidity can be obtained during biaxial stretching, and an extremely thin biaxially stretched polypropylene film without uneven thickness can be easily obtained, so it is preferred. In addition, from the viewpoint of the voltage resistance of the biaxially stretched polypropylene film, such a polypropylene resin is also preferred.
[0089] The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) of the polypropylene resin can be measured using a gel permeation chromatography (GPC) device. More specifically, for example, HLC-8121GPC-HT (trade name), a high temperature GPC measuring machine with a built-in differential refractometer (RI) manufactured by Tosoh Corporation, can be used for measurement. Mw and Mn are measured, for example, as follows. As a GPC column, three TSKgel GMHHR-H(20)HT manufactured by Tosoh Corporation are connected and used, the column temperature is set to 140°C, and trichlorobenzene as an eluent is allowed to flow at a flow rate of 1.0 ml / 10 minutes to obtain the measured values of Mw and Mn. A standard curve related to the molecular weight M is prepared using standard polystyrene manufactured by Tosoh Corporation, and the measured values are converted into polystyrene values to obtain Mw and Mn.
[0090] The melt flow rate (MFR) of the polypropylene resin at 230°C and a load of 2.16 kg is not particularly limited, but from the viewpoint of the stretchability of the obtained film, it is preferably 7 g / 10 minutes or less, and more preferably 6 g / 10 minutes or less. In addition, from the viewpoint of improving the thickness accuracy of the polypropylene film, it is preferably 0.3 g / 10 minutes or more, and more preferably 0.5 g / 10 minutes or more. It should be noted that the above MFR can be measured according to JIS K 7210-1999.
[0091] The meso pentad fraction ([mmmm]) of the polypropylene resin is preferably 94% or more, more preferably 95% or more, and further preferably more than 96%. In addition, the above-mentioned meso pentad fraction of the polypropylene resin is preferably 98.5% or less, more preferably 98.4% or less, and further preferably 98% or less. The above-mentioned meso pentad fraction of the polypropylene resin is preferably 94% or more and 99% or less, more preferably 95% or more and 98.5% or less. By using such a polypropylene resin, the crystallinity of the resin is moderately improved by moderately high stereoregularity, and the initial withstand voltage and long-term withstand voltage are improved. On the other hand, the desired stretchability can be obtained by a moderate solidification (crystallization) speed when molding the cast green sheet.
[0092] The meso pentad fraction ([mmmm]) is an index of stereoregularity that can be obtained by high-temperature nuclear magnetic resonance (NMR) measurement. Specifically, for example, the measurement can be performed using a high-temperature Fourier transform nuclear magnetic resonance apparatus (high-temperature FT-NMR), JNM-ECP500 manufactured by JEOL Ltd. 13C (125 MHz) can be used as the observation nucleus, 135° C. can be used as the measurement temperature, and o-dichlorobenzene (ODCB: a mixed solvent of ODCB and deuterated ODCB (mixing ratio = 4 / 1)) can be used as the solvent for dissolving the polypropylene resin. The measurement method based on high-temperature NMR can be performed with reference to, for example, the method described in “New Edition of Polymer Analysis Handbook, compiled by the Japan Analytical Chemistry and Polymer Analysis Research Council, Kinokuniya Bookstore, 1995, page 610”.
[0093] The measurement mode can be set to single pulse proton broadband decoupling, the pulse width can be set to 9.1μsec (45° pulse), the pulse interval can be set to 5.5sec, the number of accumulations can be set to 4500 times, and the displacement standard can be set to CH3(mmmm)=21.7ppm. The pentad fraction representing the stereoregularity is calculated as a percentage based on the integral value of the intensity of each signal of the combination of the pentad (mmmm and mrrm, etc.) from the unit group "meso (m)" arranged in the same direction and the unit group "racemic (r)" arranged in different directions. The signals from mmmm and mrrm, etc. can be attributed, for example, with reference to "T.Hayashi et al., Polymer, Vol. 29, p. 138 (1988)" and the like.
[0094] As for the above-mentioned polypropylene resin as the main component of the polypropylene film roll involved in the first embodiment, a linear polypropylene resin can be cited. The linear polypropylene resin can be used alone, or two or more kinds can be mixed and used. Among them, it is preferred to use the following linear polypropylene resin A, and / or, the following linear polypropylene resin B. It is particularly preferred to use the following linear polypropylene resin A and the following linear polypropylene resin B in combination. The following linear polypropylene resin A and the following linear polypropylene resin B are preferably homopolypropylene resins. As a combination of the following linear polypropylene resin A and the following linear polypropylene resin B, the following resin A-1 and the following resin B-1, the following resin A-2 and the following resin B-2, and the following resin A-3 and the following resin B-3 can be cited as a preferred combination. However, in the present invention, the above-mentioned polypropylene resin is not limited to the following resins.
[0095] <Linear polypropylene resin A>
[0096] (Linear Polypropylene Resin A-1)
[0097] A linear polypropylene resin having a melt flow rate (MFR) at 230°C of 4.0 to 10.0 g / 10 min.
[0098] (Linear Polypropylene Resin A-2)
[0099] A linear polypropylene resin having a weight average molecular weight Mw of 340,000 or less.
[0100] (Linear Polypropylene Resin A-3)
[0101] A linear polypropylene resin having a molecular weight distribution Mw / Mn of 8.8 or more.
[0102] <Linear polypropylene resin B>
[0103] (Linear Polypropylene Resin B-1)
[0104] A linear polypropylene resin having a melt flow rate (MFR) at 230°C of less than 4.0 g / 10 min.
[0105] (Linear Polypropylene Resin B-2)
[0106] A linear polypropylene resin having a weight average molecular weight Mw exceeding 340,000.
[0107] (Linear Polypropylene Resin B-3)
[0108] A linear polypropylene resin having a molecular weight distribution Mw / Mn of less than 8.8.
[0109] When the linear polypropylene resin A and the linear polypropylene resin B are used in combination, the content ratio preferably contains 55% by weight or more of the linear polypropylene resin A and 45% by weight or less of the linear polypropylene resin B, more preferably contains 60 to 85% by weight of the linear polypropylene resin A and 40 to 15% by weight of the linear polypropylene resin B, and particularly preferably contains 60 to 80% by weight of the linear polypropylene resin A and 40 to 20% by weight of the linear polypropylene resin B.
[0110] (additive)
[0111] The polypropylene film may further contain additives. "Additives" are generally additives used in polypropylene resins, and there are no particular restrictions as long as a polypropylene film can be obtained. The additives include, for example, necessary stabilizers such as antioxidants, chlorine absorbers, and ultraviolet absorbers, lubricants, plasticizers, flame retardants, antistatic agents, colorants, etc. The polypropylene resin used to make the polypropylene film may contain such additives in an amount that does not adversely affect the polypropylene film.
[0112] (core)
[0113] The polypropylene film roll according to the present embodiment is formed by winding a polypropylene film around a core. The core is cylindrical or cylindrical, and the polypropylene film is wound along the circumferential direction of the core.
[0114] As for the material of the core, there is no particular limitation as long as the polypropylene film roll satisfies the physical properties of (1A) and (2A) above, and examples thereof include plastics with little deformation, fiber reinforced plastics, paper, metals (iron, SUS, aluminum, etc.), etc. Among them, fiber reinforced plastics are preferred from the perspective of being lightweight and high-strength and easily satisfying the physical properties of (1A) and (2A) above. Examples of fiber reinforced plastic cores include cores obtained by molding carbon fibers, glass fibers, etc. into a cylindrical shape, impregnating the cylindrical shape with a curable resin such as an unsaturated polyester resin, and curing the cylindrical shape.
[0115] The size of the core can be set according to the size of the intended polypropylene film roll. The outer diameter of the circular cross section of the core may be, for example, about 50 to 500 mm, more preferably about 100 to 300 mm.
[0116] The polypropylene film wound by the polypropylene film roll of the first embodiment has high initial withstand voltage and excellent long-term withstand voltage. Moreover, since it can be very thin, it is easy to show high electrostatic capacitance. Therefore, it can be extremely suitable for small and high-capacity capacitors of 5μF or more, preferably 10μF or more, and more preferably 20μF or more.
[0117] The method for manufacturing the polypropylene film roll according to the first embodiment is not particularly limited as long as it is a method for obtaining a polypropylene film roll satisfying the physical properties of (1A) and (2A) above. The preferred method for manufacturing the polypropylene film roll according to the first embodiment is described in detail in the column <2A. Method for manufacturing the polypropylene film roll according to the first embodiment>.
[0118] <2A. Method for producing polypropylene film roll according to first embodiment>
[0119] The method for producing the polypropylene film roll is not limited to the following method, and an example thereof includes a method including the following steps 1 to 5 in order.
[0120] (1) Step 1 of heating and melting a resin composition containing a polypropylene raw material resin
[0121] (2) Step 2 of extruding the heated and molten resin composition
[0122] (3) Cooling and solidifying the extruded resin composition to obtain a cast green sheet;
[0123] (4) Step 4 of stretching the cast green sheet in the flow direction and the width direction to obtain a biaxially stretched polypropylene film
[0124] (5) Step 5 of cutting (slitting) the biaxially stretched polypropylene film into a predetermined width and winding the polypropylene film around a core to obtain a polypropylene film roll;
[0125] Hereinafter, the method for producing the polypropylene film roll will be described in detail.
[0126] (Manufacture of polypropylene raw material resin)
[0127] The polypropylene raw material resin that can be included in the polypropylene film can be produced using a generally known polymerization method. The method for producing the polypropylene resin is not particularly limited as long as the produced polypropylene resin can be used to finally obtain a polypropylene film. As such a polymerization method, for example, a gas phase polymerization method, a bulk polymerization method, and a slurry polymerization method can be exemplified.
[0128] The total ash content caused by the polymerization catalyst residues contained in the polypropylene raw resin is preferably as small as possible in order to improve the electrical properties of the polypropylene film. The total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and particularly preferably 30 ppm or less based on the polypropylene resin (100 parts by weight). In addition, the total ash content in the polypropylene film is preferably 0.1 ppm or more, more preferably 1 ppm or more, and further preferably 5 ppm or more based on the polypropylene resin.
[0129] (Steps 1 to 3: Production of Cast Green Sheet)
[0130] The “cast green sheet” as a sheet before stretching for producing a biaxially stretched polypropylene film can be produced, for example, through the above-mentioned steps 1 to 3 using the polypropylene raw material resin produced as described above.
[0131] The polypropylene resin pellets as the resin composition, the polypropylene resin pellets after dry mixing (and / or polymer powder), or the mixed polypropylene resin pellets prepared by melt kneading in advance are supplied to an extruder, heated and melted (step 1), and after passing through a filter, heated and melted to preferably 170° C. to 320° C., more preferably 200° C. to 300° C., and melt-extruded from a T-die (step 2), and cooled and solidified using at least one metal roller maintained at preferably 92° C. to 105° C., thereby forming a cast green sheet (step 3).
[0132] From the viewpoint of appropriately imparting the physical properties of (1A) and (2A) to the polypropylene film roll involved in the first embodiment, the surface temperature of the metal roller when molding the cast green sheet is preferably 92 to 97°C, more preferably 93 to 96°C, and further preferably 94 to 95°C. If the surface temperature of the metal roller is within these preferred ranges, the β crystal percentage can be within the preferred range, and fine roughness can be formed on the film surface. If it is lower than 92°C, the film surface becomes smooth, the sliding is poor, and there is a tendency to produce wrinkles on the roller of the processing machine. On the other hand, if it exceeds 97°C, the film surface is excessively roughened, so when the film is unrolled from the film roll, winding deviation is likely to occur, and the film has a tendency to meander on the roller of the processing machine. It should be noted that the β crystal percentage is measured by an X-ray method, and is preferably 1% or more and 50% or less, more preferably 5% or more and 30% or less, and further more preferably about 5% or more and 20% or less. It should be noted that this value is a value when a β crystal nucleating agent is not contained. The above-mentioned range of the β crystal percentage is preferred because it is easy to satisfy both capacitor characteristics and element winding processability.
[0133] The β crystal percentage can be obtained by measuring the X-ray diffraction intensity, and can be calculated by the method described in "A. Tu rner-Jonesetal., Makromol. Chem., Vol. 75, p. 134 (1964)", which is called the K value. That is, the ratio of the β crystal is expressed by the ratio of the sum of the heights of the three diffraction peaks from the α crystal to the one diffraction peak from the β crystal.
[0134] The thickness of the cast green sheet is not particularly limited as long as a polypropylene film can be obtained, but is preferably 0.05 mm to 2 mm, and more preferably 0.1 mm to 1 mm.
[0135] (Step 4: Production of biaxially stretched polypropylene film)
[0136] In step 4, the cast green sheet is produced by stretching the cast green sheet in the flow direction and the width direction. The stretching is performed by biaxial stretching for biaxial orientation in the longitudinal direction and the transverse direction. The stretching method may be a simultaneous or sequential biaxial stretching method, and a sequential biaxial stretching method is preferred.
[0137] As a sequential biaxial stretching method, for example, a cast green sheet is first maintained at a temperature of about 135 to 147°C (longitudinal stretching temperature), stretched to 3 to 74.00 to 4.95 times (longitudinal stretching ratio) in the flow direction by passing it between rollers with a speed difference, and immediately cooled to room temperature. Next, the stretched film is introduced into a tenter, stretched to about 7 to 11 times (transverse stretching ratio) in the width direction at a temperature of 150°C or more (transverse stretching temperature) at a tenter inlet speed ratio of 0.98 to 1.014 times, and then relaxed and heat-set (heat-set temperature is about 158 to 168°C), and wound up with a take-up roller at the tenter outlet at a speed of about 1.01 to 1.20 times the tenter speed. The wound film can be cut into the desired product width after being aged in an atmosphere of about 20 to 45°C.
[0138] In the above-mentioned manufacturing process, the longitudinal stretching temperature, the longitudinal stretching ratio, the transverse stretching temperature, the transverse stretching ratio, the tenter inlet speed ratio, the molecular weight distribution of the polypropylene resin, the resin temperature during melting, the MFR of the cast film, the relaxation rate in the width direction after transverse stretching, the relaxation temperature, the thermal fixing temperature, etc. are parameters that affect the physical properties of the above-mentioned (1A) and (2A), and they are appropriately adjusted. Among these parameters, the longitudinal stretching ratio and the tenter inlet speed ratio are the parameters that have a great influence on the physical properties of the above-mentioned (1A) and (2A), respectively. Regarding a part of these parameters, an example of the adjustment range thereof is shown below. However, in the first embodiment, as the above-mentioned parameters, they are not limited to the following ranges.
[0139] <Longitudinal stretching temperature>
[0140] From the viewpoint of easily having the desired physical properties of the first embodiment, the longitudinal stretching temperature is preferably 135 to 147° C., more preferably 137 to 147° C., and further preferably 140 to 145° C. The reason why the longitudinal stretch ratio affects the slow axis angle is that the longitudinal stretched film after longitudinal stretching has plasticity under the influence of the longitudinal stretching temperature, and the tension generated by the above-mentioned tenter inlet speed ratio acts to affect the orientation of the polymer molecular chains.
[0141] <Longitudinal stretch ratio>
[0142] From the viewpoint of being easy to possess the desired physical properties of the first embodiment, the longitudinal stretching ratio is preferably 4.00 to 4.95 times, more preferably 4 to 4.9 times, and further preferably 4.2 to 4.8 times. If the longitudinal stretching ratio is in the preferred range, film breakage is suppressed in the transverse stretching process during film making, and productivity is excellent. In addition, the mechanical strength of the obtained film is moderately high and the processability is excellent. If it is less than 4.0 times, there is a tendency for the deformation rate (elongation change) to increase when force is applied, and wrinkles are easily generated due to the tension of the processing machine. On the other hand, if it exceeds 4.95 times, since the deformation rate is small, the film roll has poor followability during winding, and there is a tendency to unevenly involve air. Therefore, the film is deformed at a location where the air layer between the overlapping films is large during winding, and wrinkles and relaxation are easily generated at specific locations during processing.
[0143] <Transverse stretching temperature>
[0144] From the viewpoint of easily having the desired physical properties of the first embodiment, the transverse stretching temperature is preferably 150° C. or higher, more preferably 155° C. or higher and 165° C. or lower, further preferably 155° C. or higher and lower than 160° C., and particularly preferably 155° C. or higher and 159° C. or lower. It should be noted that in order to make the transverse stretching temperature within the above range, the tenter temperature can be set within the above range.
[0145] <Transverse stretching ratio>
[0146] From the viewpoint of easily obtaining the desired physical properties of the first embodiment, the transverse stretching ratio is preferably 7 to 11 times, more preferably 8 to 11 times, and even more preferably 9 to 11 times.
[0147] <Speed ratio at stenter entrance>
[0148] The slow axis angle of the biaxially stretched polypropylene film is affected by the ratio of the tenter inlet speed to the longitudinally stretched film obtained by stretching in the flow direction (tenter inlet speed ratio). From the viewpoint of being easy to have the desired physical properties of the first embodiment, the tenter inlet speed ratio (tenter inlet speed / MD film speed) is preferably 0.98 or more and 1.014 or less, more preferably 1.00 or more and 1.014 or less, further preferably 1.001 or more and 1.013 or less, further preferably 1.002 or more and 1.012 or less, and particularly preferably 1.003 to 1.010. By adjusting the ratio to 1.014 or less, the tension of the longitudinally stretched film can be suppressed to a low level without bending, and the variation range (maximum-minimum) of the slow axis angle in the width direction can be appropriately suppressed to a small value. As a reason for the influence on the slow axis angle, it can be considered that the tension generated by the tenter inlet speed ratio is propagated to the longitudinally stretched film in the longitudinal stretching process, thereby affecting the orientation of the polymer molecular chain. There is a tendency that: if the tenter inlet speed ratio (tenter inlet speed / longitudinal stretching film speed) is increased (raised), the variation range (maximum-minimum) of the lag axis angle in the width direction becomes larger; if the above ratio is reduced (lowered), the variation range (maximum-minimum) of the lag axis angle in the width direction becomes smaller.
[0149] In addition, the ratio ΔX of the circumferential length has a tendency to change according to the longitudinal stretching ratio and the tenter inlet speed ratio. If the longitudinal stretching ratio or the tenter inlet speed ratio is excessively increased, there is a tendency to increase. When the film roll is wound, the difference in circumferential length becomes larger because the air layer is unevenly wound and the local winding is harder. The reason is that if the longitudinal stretching ratio or the tenter inlet speed ratio is excessively increased, there is a tendency for the deformation rate after biaxial stretching to become smaller. Therefore, when the cut film is wound, the film's followability to the roller becomes worse (difficult to stretch), and there is a tendency to unevenly draw in air. Therefore, deviations occur in the parts where the air layer between the wound overlapping films is large, and the difference in circumferential length becomes larger.
[0150] By such a stretching step, a biaxially stretched polypropylene film can be produced. It is preferable to give the surface of the biaxially stretched polypropylene film an appropriate surface roughness that improves winding suitability and also improves capacitor characteristics.
[0151] (Step 5: Slitting and winding onto a core)
[0152] In step 5, the biaxially stretched polypropylene film obtained in step 4 is cut (slit) into a predetermined width and wound around a core to obtain a polypropylene film roll. Figure 2As shown in the schematic diagram of , the biaxially stretched polypropylene film of step 4 is wound into a roll to prepare a pre-cut film roll. Next, the film is unrolled from the pre-cut film roll, cut in the unrolling direction using a cutter (slitting section), and the cut polypropylene film is wound around a core to obtain a polypropylene film roll. In step 5, when winding the cut polypropylene film, a method of applying a winding surface pressure to the polypropylene film using a winding device equipped with a pressure roller can be adopted. At this time, the winding tension and winding surface pressure during cutting and the rubber hardness of the pressure roller are parameters that have a great influence on the physical properties of the above-mentioned (1A) and (2A), respectively.
[0153] From the viewpoint of appropriately imparting the physical properties of (1A) and (2A) to the polypropylene film roll of the first embodiment and appropriately setting the shortest distance ΔL to 20 mm or less, the winding tension in step 5 is preferably 30 to 75 N / m, more preferably 40 to 70 N / m, further preferably 50 to 65 N / m, and particularly preferably 50 to 60 N / m. In addition, the winding surface pressure in step 5 is preferably 200 to 440 N / m, more preferably 250 to 420 N / m, further preferably 300 to 400 N / m, and extremely preferably 320 to 400 N / m.
[0154] The unwinding tension in step 5 is set to match the winding tension and is preferably 30 to 70 N / m, more preferably 30 to 65 N / m, and even more preferably 35 to 60 N / m.
[0155] From the viewpoint of appropriately giving the above-mentioned physical properties of (1A) and (2A) to the polypropylene film roll of the first embodiment, and then appropriately setting the shortest distance ΔL to less than 20 mm, the rubber hardness of the contact roller used in process 5 is preferably 35° to 65°, more preferably 40° to 60°, and further preferably 40° to 55°. If the rubber hardness is in the preferred range, the surface rubber is appropriately deformed to match the shape of the film roll, so the surface pressure during winding is easily applied uniformly in the width direction. As a result, the air layer inside the obtained film roll is uniformized, so when the film is rolled out, the difference in the peeling position in the width direction becomes smaller. If the rubber hardness is lower than 35°, the surface rubber is excessively deformed relative to the shape of the film roll, so the air layer inside the obtained film roll becomes less and is wound harder. Therefore, adhesion is easily generated between the overlapping films wound, and the difference in the peeling position in the width direction becomes larger when the film is rolled out. If the rubber hardness exceeds 65°, it is difficult for the surface rubber to follow the shape of the film roll, the surface pressure during winding becomes uneven in the width direction, and it is easy to be wound hard locally. Inside the obtained film roll, since there is uneven air layer in the width direction, when the film is unwound, there is a tendency for the difference in the peeling position in the width direction to become larger.
[0156] <1B. Polypropylene film roll according to second embodiment>
[0157] The polypropylene film roll according to the second embodiment is characterized in that a polypropylene film having a thickness of 20 μm or less and a width of 200 mm or more is wound around a core and satisfies the above-mentioned physical properties (1B) and (2B).
[0158] Regarding the physical property (1B) above, for the peeling line formed when the polypropylene film is unwound from the polypropylene film roll according to the second embodiment under specified conditions, the shortest distance ΔL from the middle point of the straight line connecting the two ends of the peeling line to the peeling line is 20 mm or less. Figure 1 As shown in the schematic diagram of , the peeling line S is the boundary line between the portion where the polypropylene film 1 is peeled off from the polypropylene film roll 10 and the portion that is not peeled off. Usually, when the polypropylene film is rolled out from the polypropylene film roll, the peeling line is not straight in the width direction x, but is formed in a manner of describing an arc (an arc of the peeling line S toward the rolling-out direction L) from one end to the other end of the width direction x of the polypropylene film (that is, from one end x1 of the peeling line to the other end x2). The thinner the thickness of the polypropylene film roll and the wider the width, the greater the shortest distance ΔL of the peeling line. It should be noted that when the polypropylene film roll is visually confirmed from above, the portion where the transparent polypropylene film roll is peeled off and the portion that is not peeled off have different appearances across the boundary line, so the peeling line can be identified visually.
[0159] The shortest distance ΔL of the peeling line of the polypropylene film roll can be measured by the method described in Examples.
[0160] In the polypropylene film roll involved in the second embodiment, the shortest distance ΔL of the peeling line is set to be less than 20 mm, and the physical property (2B) described later is also satisfied (the ratio ΔX of the circumferential length of the polypropylene film roll is set to be less than 0.2%), so that the polypropylene film rolled out from the polypropylene film roll can be subjected to metal vapor deposition processing with high precision while maintaining high flatness, and the deviation of the film thickness of the metal film is suppressed. Furthermore, the capacitor element obtained from the polypropylene film has excellent long-term durability at high temperature and high voltage. In addition, the winding deviation caused by the wrinkles and slack of the film and the reduction of the yield due to cutting are also suppressed, and the capacitor element can be manufactured with a high yield.
[0161] From the viewpoint that the polypropylene film rolled out from the polypropylene film roll can be subjected to metal vapor deposition processing with high precision while maintaining higher flatness, the long-term durability of the capacitor element under high temperature and high voltage can be further improved, and further, the winding deviation caused by the wrinkles and relaxation of the polypropylene film and the reduction of the yield rate caused by cutting can be suppressed, and the capacitor element can be manufactured with a higher yield rate, in the polypropylene film roll involved in the second embodiment, the shortest distance ΔL of the peeling line can be 20 mm or less, but preferably 17 mm or less, more preferably 14 mm or less, and further preferably 10 mm or less. In addition, the lower limit of the shortest distance ΔL of the peeling line can be, for example, 0 mm, 2 mm, etc.
[0162] When the circumference of the polypropylene film roll is measured at the two end positions, the center position, and positions at intervals of 50 mm from the center position toward the two end positions, the physical property (2B) above has a ratio ΔX ((Xmax-Xmin) / Xave) of the difference (Xmax-Xmin) between the maximum value Xmax and the minimum value Xmin of the circumferential length to the average value Xave of the circumferential length of less than 0.2%.
[0163] In the polypropylene film roll involved in the second embodiment, the ratio ΔX of the circumference length can be 0.2% or less, but from the above viewpoint, it is preferably 0.19% or less, more preferably 0.18% or less, and further preferably 0.17% or less. In addition, the lower limit of the ratio ΔX of the circumference length can be, for example, 0.00%, 0.01%, etc.
[0164] The ratio ΔX of the circumferential length of the polypropylene film roll can be measured by the method described in Examples.
[0165] From the above viewpoints, in the polypropylene film roll of the second embodiment, when the hardness is measured at the two end positions, the central position, and the positions at intervals of 50 mm from the central position toward the two end positions of the polypropylene film roll, the average value Mave of the hardness is preferably 88 to 96°, and the difference ΔM between the maximum value and the minimum value Mmin of the hardness is less than 4°. With respect to Mave, it is more preferably 96 to 86°, and more preferably 94 to 88°. With respect to ΔM, it is more preferably 3° or less, and more preferably 2° or less. With respect to the lower limit of ΔM, for example, 0° can be cited.
[0166] The average value Mave of the hardness of the polypropylene film roll and the difference ΔM between the maximum value Mmax and the minimum value Mmin of the hardness can be measured by the methods described in Examples.
[0167] In addition, from the above-mentioned viewpoints, in the polypropylene film roll involved in the second embodiment, the deformation rate (ε1) in the longitudinal direction (MD), the deformation rate (ε2) in the width direction (TD) and the deformation rate (ε3) in the diagonal direction (45°) of the polypropylene film when the stress is 25 MPa are preferably in the range of 0.6 to 1.5%, more preferably in the range of 0.6 to 1.4%, and further preferably in the range of 0.6 to 1.3%.
[0168] The deformation rate of the polypropylene film is a value measured on the polypropylene film unwound from the polypropylene film roll, and can be specifically measured by the method described in Examples.
[0169] In addition, from the above-mentioned viewpoints, the ratio of the deformation rate (ε1) to the deformation rate (ε2) (ε2 / ε1), and the ratio of the deformation rate (ε3) to the deformation rate (ε1) (ε3 / ε1) are preferably in the range of 0.5 to 1.0, more preferably in the range of 0.7 to 1.0, and further preferably in the range of 0.8 to 0.9.
[0170] In addition, from the above viewpoints, in the polypropylene film roll involved in the second embodiment, the surface roughness of at least one side of the polypropylene film is preferably 0.04 to 0.08 μm in centerline average roughness (Ra) and 0.3 to 0.9 μm in maximum height (Rz). Regarding the centerline average roughness (Ra), it is more preferably 0.05 to 0.08 μm, and more preferably 0.05 to 0.07 μm. In addition, regarding the maximum height (Rz), it is more preferably 0.3 to 0.8 μm, and more preferably 0.4 to 0.8 μm. The surface roughness of both sides of the polypropylene film may also have the above values.
[0171] The surface roughness (center line average roughness (Ra) and maximum height (Rz)) of the polypropylene film is a value measured for the polypropylene film unwound from a polypropylene film roll, and can be specifically measured by the method described in Examples.
[0172] In the polypropylene film roll of the second embodiment, the difference between the maximum and minimum values of the slow axis angle obtained by the following methods (a) to (c) is preferably 5° or less. (a) When the total length in the width direction of the polypropylene film is set to 100%, 9 pieces of 50 mm × 50 mm measurement samples are cut out with the center at positions every 10% from both ends.
[0173] (b) The width direction of the measurement sample is set to 0°, and the acute angle formed by the width direction of the measurement sample and the slow axis is measured as the slow axis angle.
[0174] (c) The difference between the maximum value and the minimum value of the slow axis angle measured in (b) above among the nine measurement samples was determined.
[0175] This physical property is a physical property related to the slow phase axis angle of the polypropylene film. The biaxially stretched polypropylene film is stretched in a first direction and a second direction orthogonal thereto. The polypropylene film is oriented inwardly by biaxial stretching, so it has birefringence. In the polypropylene film plane, the direction with the largest refractive index becomes the direction with the slow forward speed of light (phase delay), so it is called the slow phase axis.
[0176] For example, in the sequential biaxial stretching method, first, the cast green sheet is stretched in the flow direction (MD direction), and then the sheet is stretched in the transverse direction (TD direction (width direction)). In this case, regarding the slow axis of the biaxially stretched polypropylene film, there is a tendency that the refractive index in the transverse direction of the second direction is greater than the refractive index in the flow direction of the first direction. Here, the transverse direction of the second direction is the slow axis.
[0177] In the transverse (TD) stretching, when the stretching is performed completely in the transverse direction (when the stretching is performed completely in the direction orthogonal to the flow direction), the lag axis angle defined in this specification is 0°. However, in reality, Poisson shrinkage stress, mechanical external force, thermoplasticity of the film, etc. act during stretching, and it is impossible to stretch completely in the transverse (TD direction), and there is a tendency for the lag axis angle to be greater than 0°. In addition, in the sequential biaxial stretching method, there is a tendency for the lag axis angle to be larger at both ends of the biaxially stretched film.
[0178] In the second embodiment, it can be said that the smaller the difference between the maximum and minimum values of the above-mentioned slow axis angle, the smaller the deviation of the orientation of the optical orientation axis relative to the two orthogonal directions of the flow direction (MD direction) of the first direction and the transverse direction (TD direction) of the second direction. Therefore, when the metallized film is produced, the oblique shrinkage during heating becomes less, and it is easy to achieve uniform heat shrinkage in the first direction and the second direction. As a result, wrinkles and relaxation during processing can be suppressed, and the film can be used appropriately.
[0179] The difference between the maximum and minimum values of the lag axis angle in the second embodiment is not the anisotropy of the optical orientation intensity represented by birefringence, etc., that is, it is not the size and direction of the orientation itself, but the angle formed by the maximum and minimum values of the second direction and the lag axis, that is, the variation range of the lag axis angle in the width direction. In the second embodiment, it is preferred to control the above difference to be smaller in the roll width direction (processing width direction). The reason why the above difference is preferably controlled to be smaller is that even if a certain mechanical processing strength is given to the polypropylene as a soft raw material based on the orientation strength of biaxial stretching, the thermal dimensional change caused by the metal vapor deposition process cannot be fully reduced. Instead, the deviation of the orientation direction in the roll width direction is suppressed, and the variation contributes to the uniformity of the shrinkage direction in the in-plane direction, so that a metallized film with less uneven vapor deposition film can be obtained.
[0180] The capacitor element thus obtained has excellent long-term durability at high temperature and high voltage. In addition, the polypropylene film roll can be used in which the winding deviation caused by wrinkles and slack during processing is significantly eliminated, the yield rate of the capacitor element is excellent, and the cost is also appropriate.
[0181] In the polypropylene film roll involved in the second embodiment, the difference between the maximum and minimum values of the lag axis angle of the polypropylene film is set to less than 5°, and the physical property (2B) described later is also satisfied (the ratio ΔX of the circumferential length of the polypropylene film roll is set to less than 0.2%), so that the polypropylene film rolled out from the polypropylene film roll can be subjected to metal vapor deposition processing with high precision while maintaining high flatness, and the deviation of the film thickness of the metal film is suppressed. Furthermore, the capacitor element obtained from the polypropylene film has excellent initial withstand voltage and long-term durability under high temperature and high voltage. In addition, the winding deviation caused by the wrinkles and relaxation of the film is also suppressed, and the capacitor element can be manufactured with a high yield.
[0182] From the viewpoint that the polypropylene film rolled out from the polypropylene film roll can be subjected to metal vapor deposition processing with high precision while maintaining higher flatness, the initial withstand voltage of the capacitor element and the long-term durability under high temperature and high voltage can be further improved, and further, the winding deviation caused by the wrinkles and relaxation of the polypropylene film and the reduction of the yield rate due to cutting can be suppressed to manufacture the capacitor element with a higher yield rate, preferably 4.5° or less, more preferably 4.0° or less, and further preferably 3.0° or less can be cited. In addition, the lower limit of the difference between the maximum value and the minimum value of the lag axis angle is 0°.
[0183] The difference between the maximum value and the minimum value of the slow axis angle of the polypropylene film can be measured by the method described in Examples.
[0184] In the polypropylene film roll according to the second embodiment, the thickness of the polypropylene film is, for example, 6.0 μm or less. For a polypropylene film roll wound with a thin polypropylene film, from the viewpoint of appropriately satisfying the physical properties of (1B) and (2B) above, it is preferably 4.0 μm or less, more preferably 3.0 μm or less, further preferably 2.8 μm or less, and particularly preferably 2.5 μm or less. Furthermore, from the viewpoint of appropriately satisfying the physical properties of (1B) and (2B) above, it is preferably 0.5 μm or more, more preferably 1.0 μm or more, and further preferably 1.5 μm or more.
[0185] In the polypropylene film roll involved in the second embodiment, the width of the polypropylene film can be 200 mm or more. From the viewpoint of appropriately satisfying the physical properties of (1B) and (2B) mentioned above, the width of the polypropylene film roll wound with a wide polypropylene film is preferably 400 mm or more, more preferably 600 mm or more, and the preferred range is 600 to 1200 mm, and further 600 to 1000 mm.
[0186] In the polypropylene film roll of the second embodiment, the winding length of the polypropylene film is not particularly limited, and is, for example, 10000 m or more, more preferably 30000 m or more. The upper limit of the winding length of the polypropylene film is, for example, 100000 m.
[0187] The polypropylene film wound around the polypropylene film roll according to the second embodiment is preferably a biaxially stretched polypropylene film. From the viewpoint of appropriately satisfying the physical properties of (1B) and (2B) above, the preferred stretch ratios (longitudinal stretch ratio, transverse stretch ratio) of the biaxially stretched polypropylene film are as described in the column <2B. Method for producing polypropylene film roll according to the second embodiment> described later.
[0188] As described later, the physical properties of (1B) and (2B) above are affected by the stretching conditions of the polypropylene film, etc. The physical properties of (1B) and (2B) above can be adjusted by adjusting the stretching temperature and stretching ratio when stretching along the flow direction (hereinafter, also referred to as "longitudinal stretching temperature" and "longitudinal stretching ratio", respectively), the stretching temperature, stretching ratio and stretching angle when stretching along the width direction (hereinafter, also referred to as "transverse stretching temperature", "transverse stretching ratio" and "transverse stretching angle", respectively), etc. It should be noted that examples of preferred stretching conditions in the second embodiment will be described later in the column <2B. Method for manufacturing a polypropylene film roll according to the second embodiment>. In addition, in this specification, "longitudinal" and "flow direction" are synonymous, and "transverse" and "width direction" are synonymous.
[0189] The polypropylene film wound by the polypropylene film roll involved in the second embodiment contains a polypropylene resin as a resin. It is preferred that the main component of the polypropylene film is a polypropylene resin, and more preferably the resin component constituting the film is a polypropylene resin. It should be noted that the above-mentioned "main component" refers to a resin as a main component containing 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and particularly preferably 99% by mass or more in terms of solid content in the polypropylene film. The polypropylene resin contained in the polypropylene film is described in detail below.
[0190] <Polypropylene resin>, <Linear polypropylene resin A>, <Linear polypropylene resin B>, (additive), and (core)
[0191] In the second embodiment, the polypropylene resin is not particularly limited as long as a polypropylene film roll having the physical properties of (1B) and (2B) can be obtained, and a wide range of polypropylene resins that can be used to form a polypropylene film can be used. Regarding the polypropylene resin of the second embodiment, the description of <Polypropylene Resin>, <Linear Polypropylene Resin A>, <Linear Polypropylene Resin B> and (Additives) described in the above-mentioned first embodiment is cited and omitted. In addition, the polypropylene film roll involved in the second embodiment is formed by winding a polypropylene film on a core. The description of the core in the second embodiment is also cited and omitted by referring to the description of (Core) described in the above-mentioned first embodiment.
[0192] The polypropylene film wound by the polypropylene film roll involved in the second embodiment has high initial withstand voltage and excellent long-term withstand voltage. Moreover, since it can be made very thin, it is easy to show high electrostatic capacitance. Therefore, it can be extremely suitable for small and high-capacity capacitors of 5μF or more, preferably 10μF or more, and more preferably 20μF or more.
[0193] The method for producing the polypropylene film roll according to the second embodiment is not particularly limited as long as it is a method for obtaining a film roll satisfying the physical properties of (1B) and (2B) above. The preferred method for producing the polypropylene film roll according to the second embodiment is described in the column <2B. Method for producing the polypropylene film roll according to the second embodiment>.
[0194] <2B. Method for producing polypropylene film roll according to second embodiment>
[0195] The method for producing the polypropylene film roll according to the second embodiment is not limited to the following method, but similarly to the first embodiment, for example, a method including the following steps 1 to 5 in order can be exemplified.
[0196] (1) Step 1 of heating and melting a resin composition containing a polypropylene raw material resin
[0197] (2) Step 2 of extruding the heated and molten resin composition
[0198] (3) Cooling and solidifying the extruded resin composition to obtain a cast green sheet;
[0199] (4) Step 4 of stretching the cast green sheet in the flow direction and the width direction to obtain a biaxially stretched polypropylene film
[0200] (5) Step 5 of cutting (slitting) the biaxially stretched polypropylene film into a predetermined width and winding the polypropylene film around a core to obtain a polypropylene film roll;
[0201] Hereinafter, the method for producing the polypropylene film roll will be described in detail.
[0202] (Manufacture of polypropylene raw material resin)
[0203] The polypropylene raw material resin that can be contained in the polypropylene film can be produced using a generally known polymerization method. The method for producing the polypropylene resin is as described in the first embodiment.
[0204] In the second embodiment, the description about the total ash content is the same as that of the first embodiment.
[0205] (Steps 1 to 3: Production of Cast Green Sheet)
[0206] The “cast green sheet” as a sheet before stretching for producing a biaxially stretched polypropylene film can be produced, similarly to the first embodiment, by using the polypropylene raw material resin produced as described above and passing through the above steps 1 to 3.
[0207] The polypropylene resin pellets as the resin composition, the polypropylene resin pellets after dry mixing (and / or polymer powder), or the mixed polypropylene resin pellets produced by preliminarily melt-kneading are supplied to an extruder, heated and melted (step 1), and after passing through a filter, heated and melted to preferably 170° C. to 320° C., more preferably 200° C. to 300° C., and melt-extruded from a T-die (step 2), and cooled and solidified by at least one metal roller maintained at preferably 92° C. to 105° C., more preferably 93° C. to 97° C., thereby forming a cast green sheet (step 3).
[0208] From the viewpoint of appropriately imparting the physical properties of (1B) and (2B) described above to the polypropylene film roll involved in the second embodiment, the surface temperature of the metal roller when molding the cast green sheet is preferably 92 to 97°C, more preferably 93 to 96°C, and further preferably 94 to 95°C. If the surface temperature of the metal roller is within these preferred ranges, the β crystal percentage can be within the preferred range, and fine roughness can be formed on the film surface. If it is lower than 92°C, the film surface becomes smooth, the sliding is poor, and there is a tendency to produce wrinkles on the roller of the processing machine. On the other hand, if it exceeds 97°C, the film surface is excessively roughened, so when the film is unwound from the film roll, winding deviation is likely to occur, and the film has a tendency to meander on the roller of the processing machine. It should be noted that the β crystal percentage is measured by an X-ray method, and is preferably 1% or more and 50% or less, more preferably 5% or more and 30% or less, and further more preferably about 5% or more and 20% or less. It should be noted that this value is a value when a β crystal nucleating agent is not contained. The above-mentioned range of the β crystal percentage is preferred because it is easy to satisfy both physical properties of capacitor characteristics and element winding processability.
[0209] The description about the β crystal percentage is as described in the first embodiment.
[0210] The thickness of the cast green sheet is not particularly limited as long as a polypropylene film can be obtained, but is preferably 0.05 mm to 2 mm, and more preferably 0.1 mm to 1 mm.
[0211] (Step 4: Production of biaxially stretched polypropylene film)
[0212] In step 4, the cast green sheet is produced by stretching the cast green sheet in the flow direction and the width direction. The stretching is performed by biaxial stretching for biaxial orientation in the longitudinal direction and the transverse direction. The stretching method may be a simultaneous or sequential biaxial stretching method, and a sequential biaxial stretching method is preferred.
[0213] As a sequential biaxial stretching method, for example, the cast green sheet is first maintained at a temperature of about 135 to 147°C (longitudinal stretching temperature), stretched to 4.00 to 4.95 times (longitudinal stretching ratio) in the flow direction through rollers with a speed difference, and immediately cooled to room temperature. Next, the stretched film is introduced into a tenter, stretched to about 7 to 11 times (lateral stretching ratio) in the width direction at a temperature of more than 150°C (lateral stretching temperature), and then relaxed and heat-set (heat-set temperature is about 158 to 168°C) and wound. The wound film can be cut into the desired product width after being aged in an atmosphere of about 20 to 45°C.
[0214] In the above-mentioned manufacturing process, the longitudinal stretching temperature, the longitudinal stretching ratio, the transverse stretching temperature, the transverse stretching ratio, the molecular weight distribution of the polypropylene resin, the resin temperature during melting, the MFR of the cast film, the relaxation rate in the width direction after the transverse stretching, the relaxation temperature, the thermal fixing temperature, etc. are parameters that affect the physical properties of the above-mentioned (1B) and (2B), and they are appropriately adjusted. Among these parameters, the longitudinal stretching ratio is a parameter that has a great influence on the physical properties of the above-mentioned (1B) and (2B). About a part of these parameters, an example of its adjustment range is shown below. However, in the second embodiment, as the above-mentioned parameters, it is not limited to the following range.
[0215] <Longitudinal stretching temperature>
[0216] From the viewpoint of easily obtaining the desired physical properties of the second embodiment, the longitudinal stretching temperature is preferably 135 to 147°C, more preferably 137 to 147°C, and even more preferably 140 to 145°C.
[0217] <Longitudinal stretch ratio>
[0218] From the viewpoint of being easy to possess the desired physical properties of the second embodiment, the longitudinal stretching ratio is preferably 4.00 to 4.95 times, and more preferably 4.20 to 4.80 times. If the longitudinal stretching ratio is in the preferred range, film breakage is suppressed in the transverse stretching process during film making, and productivity is excellent. In addition, the mechanical strength of the obtained film is moderately high and the processability is excellent. If it is less than 4.00 times, there is a tendency for the deformation rate (elongation change) to increase when force is applied, and wrinkles are easily generated due to the tension of the processing machine. On the other hand, if it exceeds 4.95 times, since the deformation rate is small, the film roll has poor followability during winding, and there is a tendency to unevenly involve air. Therefore, the film is deformed at a location where the air layer between the overlapping films is large during winding, and wrinkles and relaxation are easily generated at specific locations during processing.
[0219] <Transverse stretching temperature>
[0220] From the viewpoint of easily having the desired physical properties of the second embodiment, the transverse stretching temperature is preferably 150° C. or higher, more preferably 155° C. or higher and 165° C. or lower, further preferably 155° C. or higher and lower than 160° C., and particularly preferably 155° C. or higher and 159° C. or lower. It should be noted that in order to make the transverse stretching temperature within the above range, it is sufficient to set the tenter temperature within the above range.
[0221] <Transverse stretching ratio>
[0222] From the viewpoint of easily obtaining the desired physical properties of the second embodiment, the transverse stretching ratio is preferably 7 to 11 times, more preferably 8 to 11 times, and even more preferably 9 to 11 times.
[0223] By such a stretching step, a biaxially stretched polypropylene film can be produced. It is preferable to give the surface of the biaxially stretched polypropylene film an appropriate surface roughness that improves winding suitability and also improves capacitor characteristics.
[0224] (Step 5: Slitting step and winding step around core)
[0225] In step 5, the biaxially stretched polypropylene film obtained in step 4 is cut (slit) into a predetermined width. Figure 2As shown in the schematic diagram of , the biaxially stretched polypropylene film of step 4 is wound into a roll to prepare a pre-cut film roll. Next, the film is unrolled from the pre-cut film roll, and the cut polypropylene film is wound around a core while being cut along the unwinding direction using a cutter (slitting section) to obtain a polypropylene film roll. In step 5, when winding the cut polypropylene film, a method of applying a winding surface pressure to the polypropylene film using a winding device equipped with a pressure roller can be adopted. At this time, the winding tension and the winding surface pressure during cutting and the rubber hardness of the pressure roller are parameters that have a great influence on the physical properties of the above-mentioned (1B) and (2B), respectively.
[0226] From the viewpoint of appropriately imparting the physical properties of (1B) and (2B) to the polypropylene film roll of the second embodiment, the winding tension in step 5 is preferably 30 to 75 N / m, more preferably 40 to 70 N / m, further preferably 50 to 65 N / m, and particularly preferably 50 to 60 N / m. In addition, the winding surface pressure in step 5 is preferably 200 to 440 N / m, more preferably 250 to 420 N / m, further preferably 300 to 400 N / m, and extremely preferably 320 to 400 N / m.
[0227] The unwinding tension in step 5 is set to match the winding tension and is preferably 30 to 70 N / m, more preferably 30 to 65 N / m, and even more preferably 35 to 60 N / m.
[0228] From the viewpoint of appropriately imparting the physical properties of (1B) and (2B) described above to the polypropylene film roll of the second embodiment, the rubber hardness of the contact roller used in step 5 is preferably 35° to 65°, more preferably 40° to 60°, and further preferably 40° to 55°. If the rubber hardness is in the preferred range, the surface rubber is appropriately deformed to match the shape of the film roll, so the surface pressure during winding is easily applied uniformly in the width direction. As a result, the air layer inside the obtained film roll is uniformized, so when the film is rolled out, the difference in the peeling position in the width direction becomes smaller. If the rubber hardness is lower than 35°, the surface rubber is excessively deformed relative to the shape of the film roll, so the air layer inside the obtained film roll becomes less and the film is wound harder. Therefore, adhesion is easily generated between the overlapping films wound, and the difference in the peeling position in the width direction becomes larger when the film is rolled out. If the rubber hardness exceeds 65°, it is difficult for the surface rubber to follow the shape of the film roll, the surface pressure during winding becomes uneven in the width direction, and it is easy to be wound harder locally. Since the air layer is uneven in the width direction inside the obtained film roll, there is a tendency for the difference in the peeling position in the width direction to become large when the film is unwound.
[0229] <3.Metalized polypropylene film roll>
[0230] The first embodiment and the second embodiment also provide, in one mode thereof, a metallized polypropylene film roll having a metal film on one or both sides of the polypropylene film, and a metallized polypropylene film rolled out from the metallized polypropylene film roll. The metallized polypropylene film roll and the metallized polypropylene film of the first embodiment and the second embodiment are described in detail below. The capacitor obtained by winding the metallized polypropylene film of the first embodiment and the second embodiment has excellent initial withstand voltage and long-term durability under high temperature and high voltage.
[0231] In order to be processed into a capacitor, the polypropylene film may be provided with electrodes on one side or both sides. Such electrodes are not particularly limited as long as the capacitor targeted by the first embodiment and the second embodiment can be obtained, and electrodes generally used for manufacturing capacitors can be used. Examples of electrodes include metal foil, paper metalized on at least one side, and plastic film.
[0232] The capacitor is further required to be small and lightweight, so it is preferred to directly metallize one or both sides of the film of the first embodiment and the second embodiment to form an electrode. The metal used can be, for example, zinc, lead, silver, chromium, aluminum, copper, and nickel, etc., a variety of mixtures thereof, and alloys thereof, but if the environment, economy, and capacitor performance are taken into consideration, zinc and aluminum are preferred.
[0233] As a method for directly metallizing the surface of the polypropylene film, for example, a vacuum evaporation method and a sputtering method can be exemplified, and there is no particular limitation as long as the capacitor targeted by the first embodiment and the second embodiment can be obtained. From the viewpoints of productivity and economy, the vacuum evaporation method is preferred. As a vacuum evaporation method, a general crucible type or a wire type can be exemplified, and there is no particular limitation as long as the capacitor targeted by the first embodiment and the second embodiment can be obtained, and the best method can be appropriately selected.
[0234] From the perspective of the electrical characteristics of the capacitor, the film resistance of the metal vapor-deposited film is preferably about 1 to 100Ω / □. From the perspective of self-healing characteristics, the film resistance is expected to be high even within this range, and the film resistance is more preferably 5Ω / □ or more, and more preferably 10Ω / □ or more. In addition, from the perspective of safety as a capacitor, the film resistance is more preferably 50Ω / □ or less, and more preferably 30Ω / □ or less. The film resistance of the metal vapor-deposited film can be measured, for example, by a four-terminal method known to those skilled in the art during metal vapor deposition. The film resistance of the metal vapor-deposited film can be adjusted, for example, by adjusting the output of the evaporation source to adjust the evaporation amount.
[0235] When a metal vapor-deposited film is formed on one side of the film, an insulating edge is formed by not vapor-depositing a certain width from one end of the film so that the film becomes a capacitor when it is wound. Furthermore, in order to firmly bond the metallized polypropylene film to the metal sprayed electrode, it is preferred to form an edge thickening structure at the end opposite to the insulating edge. The film resistance of the edge thickening is generally about 1 to 8Ω / □, preferably about 1 to 5Ω / □. The thickness of the metal film is not particularly limited, but is preferably 1 to 200nm.
[0236] The edge pattern of the formed metal vapor-deposited film is not particularly limited, but from the viewpoint of improving the safety of the capacitor, a pattern including so-called special edges such as a fisheye pattern and a T-shaped edge pattern is preferred. If a metal vapor-deposited film is formed on one side of a polypropylene film with a pattern including special edges, the safety of the obtained capacitor is improved, and it is also effective from the perspective of suppressing the destruction and short circuit of the capacitor, so it is preferred.
[0237] As a method for forming the edge, a known method such as a tape method in which a mask is formed using a tape during vapor deposition and an oil method in which a mask is formed by applying oil can be used without any limitation.
[0238] The metallized film of the first embodiment can be processed into a capacitor of the first embodiment described later by winding along the long side direction of the film. That is, the metallized film of the first embodiment is set as a pair of two sheets, and the metal vapor-deposited film and the polypropylene film are alternately stacked and wound in an overlapping manner. Then, a capacitor is obtained by forming a pair of metal-sprayed electrodes on both end surfaces by metal spraying to form a film capacitor.
[0239] <4.Capacitor>
[0240] The present invention provides, in one embodiment, a capacitor including the metallized polypropylene film of the first embodiment and the second embodiment. The capacitors of the first embodiment and the second embodiment will be described in detail below.
[0241] In the process of manufacturing the capacitor, the film is wound. For example, the metal film and the polypropylene film in the metallized polypropylene film of the first embodiment and the second embodiment are alternately stacked, and then two pairs of metallized polypropylene films of the first embodiment and the second embodiment are overlapped and wound in such a way that the insulating edge portions are on opposite sides. At this time, it is preferred that the two pairs of metallized films of the first embodiment and the second embodiment are stacked with a gap of 1 to 2 mm. There is no particular limitation on the winding machine used, and for example, an automatic winding machine 3KAW-N2 manufactured by Oto Seisakusho Co., Ltd. can be used.
[0242] When manufacturing flat capacitors, the resulting wound product is usually pressurized after winding. Pressurization promotes the winding of the capacitor and the molding of the component. From the perspective of controlling and stabilizing the interlayer gap, the optimal value of the applied pressure varies depending on the thickness of the polypropylene film, for example, 2 to 20 kg / cm 2 .
[0243] Next, metal is sprayed on both end surfaces of the wound product to provide metal sprayed electrodes, thereby manufacturing a capacitor.
[0244] The capacitor is further subjected to a predetermined heat treatment. That is, the first and second embodiments include a step of subjecting the capacitor to a heat treatment in a vacuum at a temperature of 80 to 125° C. for one hour or more (hereinafter sometimes referred to as “heat aging”).
[0245] In the above-mentioned process of heat treating the capacitor, the temperature of the heat treatment is usually above 80°C, preferably above 90°C. On the other hand, the temperature of the heat treatment is usually below 130°C, preferably below 125°C. By performing the heat treatment at the above-mentioned temperature, the effect of heat aging can be obtained. Specifically, the gap between the films of the capacitor constituting the metallized film based on the first embodiment and the second embodiment is reduced, the corona discharge is suppressed, and the internal structure of the metallized film of the first embodiment and the second embodiment changes and crystallizes. As a result, it can be considered that the voltage resistance is improved. When the temperature of the heat treatment is lower than the specified temperature, the above-mentioned effect brought about by heat aging cannot be fully obtained. On the other hand, when the temperature of the heat treatment is higher than the specified temperature, thermal decomposition, oxidative degradation, etc. sometimes occur in the polypropylene film.
[0246] The method for heat treating the capacitor may be appropriately selected from known methods including, for example, a method using a thermostatic bath in a vacuum atmosphere, a method using high-frequency induction heating, etc. Specifically, a method using a thermostatic bath is preferably used.
[0247] The time for heat treatment is preferably 1 hour or longer, more preferably 10 hours or longer, in order to obtain mechanical and thermal stability, and more preferably 20 hours or shorter in order to prevent molding defects such as heat wrinkles and printing.
[0248] The metallized electrodes of the capacitors subjected to heat aging are usually welded with leads. In order to impart weather resistance, especially to prevent humidity degradation, the capacitors are preferably sealed in a case and potted with epoxy resin.
[0249] The capacitor of the first embodiment is a small and large-capacitance capacitor based on the metallized film of the first embodiment, and has initial withstand voltage and long-term durability under high temperature and high voltage. In addition, the capacitor of the second embodiment is a small and large-capacitance capacitor based on the metallized film of the second embodiment, and has high withstand voltage under high temperature and long-term durability under high temperature and high voltage.
[0250] Example
[0251] The first embodiment is described in detail below with reference to Examples 1A to 14A and Comparative Examples 1A to 13A. However, the first embodiment is not limited to the Examples. It should be noted that, unless otherwise specified, parts and % represent "parts by mass" and "mass %", respectively.
[0252] (Example 1A)
[0253] [Example 1A-1. Production of tape-cast green sheet]
[0254] Polypropylene A1 (PP resin A1) and polypropylene B1 (PP resin B1) were supplied to the extruder at a mass ratio of A1:B1=66:34, and after melting at a resin temperature of 230°C, they were extruded using a T-die, wound on a metal roll whose surface temperature was maintained at 95°C and solidified to produce a cast green sheet (thickness 0.11 mm). PP resin A1 had Mw=320,000, Mw / Mn=9.3, difference (DM)=11.2 ("difference (DM)" refers to the difference obtained by subtracting the differential distribution value when Log(M)=6.0 from the differential distribution value when Log(M)=4.5 in the differential distribution curve of molecular weight), meso pentad fraction [mmmm]=95%, MFR=4.9 g / 10min, and was made from Prime Polymer. In addition, PP resin B1 has Mw=350,000, Mw / Mn=7.7, difference (DM)=7.2, meso pentad fraction [mmmm]=96.5%, MFR=3.8 g / 10 min, and is manufactured by Korea Petrochemical Corporation.
[0255] [Example 1A-2. Preparation of biaxially stretched polypropylene film]
[0256] The obtained cast green sheet was maintained at a temperature of 140°C, stretched in the flow direction (longitudinal stretching) to 4.5 times between rollers with a speed difference, and immediately cooled to room temperature. The stretched film (MD film) obtained by stretching in the flow direction was introduced into the tenter at a tenter inlet speed of 1.010 times relative to its conveying speed (tenter inlet speed ratio of 1.010 times). Then, after being stretched to 10 times in the width direction at a transverse stretching temperature of 160°C, relaxation and heat fixing temperature of 166°C were implemented, and a biaxially stretched polypropylene film with a width of 5000 mm and a thickness of 2.5 μm was pulled at a speed of 1.15 times the tenter speed by the pulling roller at the tenter outlet, and a 78,000m wound pre-cut film roll was obtained.
[0257] [Example 1A-3. Preparation of biaxially stretched polypropylene film roll after cutting]
[0258] like Figure 2 As shown in the schematic diagram, the film is rolled out from the obtained pre-cut film roll and cut in the width direction with a cutting machine. When winding the cut polypropylene film, the following method is adopted: a core made of fiber reinforced plastic is used, and a winding device with a contact pressure roller is used to apply surface pressure to the polypropylene film while winding. The cutting conditions are set to a speed of 300m / min, a roll-out tension of 40N / m, a roll-up tension of 50N / m, and a roll-up surface pressure of 400N / m. The contact pressure roller uses a rubber roller with an outer diameter of 152mm and a surface hardness of 40°, and a plurality of biaxially stretched polypropylene rolls (film rolls after cutting) with a width of 820mm and a length of 75000m are finished. The roll obtained by slitting the position of the end portion of the roll before cutting in the width direction among the plurality of film rolls after cutting with a width of 820mm is referred to as roll 1. Furthermore, among the plurality of 820 mm wide cut film rolls, a roll including the center portion in the width direction of the roll before cutting (if the center portion overlaps with the slit, any roll on both sides of the center portion) is referred to as roll 2.
[0259] [Measurement of roll and film characteristic values]
[0260] <Measurement of the difference between the maximum and minimum values of the slow axis angle>
[0261] The difference between the maximum value and the minimum value of the slow axis angle was determined for each of the biaxially stretched polypropylene films of Roll 1 and Roll 2 by the following methods (a) to (c). The results are shown in Table 2A.
[0262] (a) When the total length in the width direction of the polypropylene film is set to 100%, 9 pieces of 50 mm × 50 mm measurement samples are cut out with the positions at 10% intervals from both ends thereof as the center. That is, if the roll is 820 mm in width, a total of 9 pieces of 50 mm × 50 mm measurement samples are cut out with the positions of (820 / 9) mm, ([820 / 9] × 2) mm, ([820 / 9] × 3) mm, ([820 / 9] × 4) mm, ([820 / 9] × 5) mm, ([820 / 9] × 6) mm, ([820 / 9] × 7) mm, ([820 / 9] × 8) mm, and ([820 / 9] × 9) mm as the center from one end of each roll.
[0263] (b) Next, the width direction of the measurement sample is set to 0°, and the acute angle formed by the width direction of the measurement sample and the slow axis is measured as the slow axis angle. The measuring apparatus and measuring conditions are as follows.
[0264] <Measurement equipment and measurement conditions>
[0265] Measuring device: Delay measuring device RE-100 manufactured by Otsuka Electronics Co., Ltd.
[0266] Light source: Laser light emitting diode (LED)
[0267] Bandpass filter: 550nm (measurement wavelength)
[0268] Measurement interval: 0.1 sec
[0269] Cumulative times: 10 times
[0270] Measurement points: 15 points
[0271] Gain: 10dB
[0272] Measurement environment: temperature 23°C, humidity 60%
[0273] (c) The difference between the maximum value and the minimum value of the slow axis angle measured in the above (b) among the nine measurement samples was determined.
[0274] <Measurement of the ratio ΔX of the circumferential length>
[0275] For roll 1 and roll 2, the circumference was measured at the two end positions, the center position, and the positions at intervals of 50 mm from the center position toward the two end positions. The measurement was performed using a JIS 1 grade ruler. Next, the ratio ΔX ((Xmax-Xmin) / Xave) of the difference between the maximum value Xmax and the minimum value Xmin of the circumference to the average value Xave of the circumference obtained was calculated. The results are shown in Table 4A.
[0276] <The shortest distance ΔL from the middle point of the straight line connecting the two ends of the peeling line to the peeling line>
[0277] like Figure 1 As shown in the schematic diagram, the obtained biaxially stretched polypropylene film roll was placed in a roll-to-roll unwinding / winding device (NT-750 manufactured by NUINTEK) at room temperature of 23°C and humidity of 60%, and the unwinding of the polypropylene film was started under the conditions of unwinding tension of 3N / m and speed of 2m / min. After 1 minute, while unwinding the film, the shortest distance ΔL from the middle point P of the straight line connecting the two ends of the peeling line to the peeling line S was measured. At this time, with respect to the shortest distance ΔL, Figure 1 As shown in the schematic diagram of , for a reference line U (present on the unwinding direction L side relative to the peeling line S) provided along the width direction x of the polypropylene film, the distances (distance in the unwinding direction L) between both ends (ends x1 and x2) of the polypropylene film and the reference line U and the shortest distance from the center position in the width direction x of the reference line U to the peeling line S were measured, and the shortest distance ΔL was indirectly measured. The results are shown in Table 4A.
[0278] <Measurement of thickness of biaxially stretched polypropylene film>
[0279] The thickness of the biaxially stretched polypropylene film unwound from the roll 1 and the roll 2 was measured using a micrometer (JIS-B7502) in accordance with JIS-C2330. The results are shown in Table 1A.
[0280] <Ash content measurement of biaxially stretched polypropylene film>
[0281] The ash content of the biaxially stretched polypropylene films obtained in the above-mentioned Example 1A and the following Examples 2A to 14A was measured. About 200 g of the film was weighed, transferred to a platinum dish, and ashed at 800° C. for 40 minutes. The ash ratio (ppm) was measured from the obtained ash residue. The result was that the ash content of the polypropylene film in any example was 20 ppm.
[0282] <Deformation rate at stress 25MPa>
[0283] A tensile compression tester (manufactured by Minebea Co., Ltd.) was used to perform a tensile test under test conditions (measurement temperature 23°C, test piece length 140mm, test length 100mm, test piece width 15mm, tensile speed 100mm / min). The tensile test was performed in three directions: MD, TD, and diagonal (45°). Then, the deformation rates ε1 (MD), ε2 (TD), and ε3 (diagonal) at 25MPa were obtained using the data processing software built into the tester. The results are shown in Table 3A.
[0284] [Example 1A-4. Fabrication of capacitor]
[0285] Next, the obtained biaxially stretched polypropylene film roll is used to make a capacitor in the following manner. A vacuum vapor deposition machine manufactured by ULVAC Co., Ltd. is used to perform aluminum vapor deposition T-edge vapor deposition pattern on the biaxially stretched polypropylene film with a vapor deposition resistance of 15Ω / □, thereby obtaining a metallized film containing a metal film on one side of the biaxially stretched polypropylene film. After slitting to a width of 60mm, the two metallized films are aligned and wound with 1076 turns at a winding tension of 250g using an automatic winder 3KAW-N2 manufactured by Kaito Seisakusho Co., Ltd. The wound element is pressurized and heat treated at 120°C for 15 hours, and then zinc metal is sprayed on the end surface of the element to obtain a flat capacitor. Leads are welded to the end surface of the flat capacitor and then sealed with epoxy resin.
[0286] [Evaluation of Processability of Capacitor Element]
[0287] <Evaluation of Vapor Deposition Film Unevenness>
[0288] For the metallized film before slitting of the above-mentioned [Example 1A-4. Production of capacitors], after peeling off a piece of the full-width film of one roll from the metallized film before slitting, a 100 mm square film piece is cut out from the central part of the roll width direction of the peeled full-width film. The cut film piece is divided into 100 areas of 10 mm square, and the color values (L* value, a* value, b* value) are measured for the central part of each of the 100 areas using a printing density measuring machine (Model 938 manufactured by X-Rite). It should be noted that the measurement diameter uses a measurement diameter of 8 mm. For each of the L* value, a* value, and b* value, the deviation is calculated using the following formula based on the maximum value, minimum value, and average value at 100. The value with the largest deviation among the deviations of the L* value, a* value, and b* value is evaluated as follows according to the four levels of A to D. The results are shown in Table 5A.
[0289] Deviation of L* value (%) = (maximum L* value - minimum L* value) / average L* value at 100 × 100
[0290] Deviation of a* value (%) = (maximum a* value - minimum a* value) / average a* value at 100 × 100
[0291] Deviation of b* value (%) = (b* maximum value - b* minimum value) / b* average value at 100 × 100
[0292] A: The maximum value among the deviations of L* value, a* value, and b* value is less than 5%
[0293] B: The maximum value among the deviations of L* value, a* value, and b* value is 5% or more and less than 10%
[0294] C: The maximum value among the deviations of L* value, a* value, and b* value is 10% or more and less than 20%
[0295] D: The maximum value among the deviations of L* value, a* value, and b* value is 20% or more
[0296] <Evaluation of Yield of Capacitor Element Manufacturing>
[0297] In the above [Example 1A-4. Production of capacitors], the film during the process of conveying was visually checked, and all wrinkles were considered unqualified. In addition, regarding the winding deviation, the element with a deviation of 0.2 mm or more when observed from the end face of the capacitor element was considered unqualified. 100 elements were made, and the ratio of the number of qualified capacitor elements was calculated as the element yield, and evaluated according to the following criteria. The results are shown in Table 5A.
[0298] A: 100%
[0299] B: 90% or more and less than 100%
[0300] C: 80% or more and less than 90%
[0301] D: less than 80%
[0302] [Evaluation of Initial Withstand Voltage of Capacitor Element]
[0303] The initial electrostatic capacitance (C 0 ) was measured. Next, a DC voltage of 450 V / μm was applied to the capacitor for 10 seconds. Similarly, the electrostatic capacitance (C 1 ), and calculate the capacity change rate before and after the test according to the following formula.
[0304] [Formula 1]
[0305]
[0306] The above-mentioned capacity change rate was measured for five capacitor elements and evaluated according to the following criteria.
[0307] A: All components are -0.5% or more
[0308] B: All components are less than -0.5% and more than -1%
[0309] C: More than one element is less than -1%
[0310] [Evaluation of long-term durability of capacitor elements]
[0311] <Capacitance change rate ΔC>
[0312] The initial electrostatic capacitance (C) before the test of the capacitor element obtained in [Example 1A-4. Preparation of capacitor] was measured using LCR high tester 3522-50 manufactured by Hioki Electric Co., Ltd. 0 ) was measured. Then, the capacitor was continuously loaded with a DC voltage of 300 V / μm per unit thickness for 500 hours in a high temperature tank at 105°C. The capacitance (C 500 ), calculate the capacity change rate (ΔC) before and after the voltage load. Here, the capacity change rate is calculated by the following formula.
[0313] [Formula 2]
[0314]
[0315] The above-mentioned capacity change rate was evaluated based on the average value of five capacitors according to the following criteria. The results are shown in Table 5A.
[0316] A+: -0.5% or more
[0317] A: Less than -0.5% and -1% or more
[0318] B: less than -1% and more than -5%
[0319] C: less than -5% and more than -10%
[0320] D: less than -10%
[0321] (Example 2A)
[0322] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1A, except that the tenter inlet speed ratio was set to 1.007 times, and a capacitor was produced (Table 1A). In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1. The results are shown in Tables 2A to 5A.
[0323] (Example 3A)
[0324] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1A, except that the tenter inlet speed ratio was set to 1.005 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0325] (Example 4A)
[0326] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1A, except that the tenter inlet speed ratio was set to 1.012 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0327] (Example 5A)
[0328] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching ratio was set to 4.0 times, and the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0329] (Example 6A)
[0330] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching ratio was set to 4.9 times, and the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0331] (Example 7A)
[0332] In the preparation of the biaxially stretched polypropylene film, the film thickness was set to 2.3 μm, and the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0333] (Example 8A)
[0334] In the preparation of the biaxially stretched polypropylene film, except that the film thickness was set to 2.0 μm, the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0335] (Example 9A)
[0336] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 8A, except that the tenter inlet speed ratio was set to 1.005 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0337] (Example 10A)
[0338] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 8A, except that the tenter inlet speed ratio was set to 1.012 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0339] (Example 11A)
[0340] In the preparation of the biaxially stretched polypropylene film, except that the film thickness was set to 2.8 μm, the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0341] (Example 12A)
[0342] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching temperature was set to 145° C. and the tenter inlet speed ratio was set to 1.014 times. The film roll was finished in the same manner as in Example 11A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0343] (Example 13A)
[0344] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 10A, except that the roll width after cutting was set to 620 mm, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0345] (Example 14A)
[0346] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 8A, except that the tenter inlet speed ratio was set to 1.001 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0347] (Comparative Example 1A)
[0348] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1A, except that the tenter inlet speed ratio was set to 1.015 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0349] (Comparative Example 2A)
[0350] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1A, except that the tenter inlet speed ratio was set to 1.020 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0351] (Comparative Example 3A)
[0352] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching temperature was set to 150° C., and the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0353] (Comparative Example 4A)
[0354] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching ratio was set to 3.7 times, and the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0355] (Comparative Example 5A)
[0356] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching ratio was set to 5.2 times, and the film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0357] (Comparative Example 6A)
[0358] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching temperature was set to 150° C. and the tenter inlet speed ratio was set to 1.015 times. The film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0359] (Comparative Example 7A)
[0360] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching temperature was set to 150° C. and the tenter inlet speed ratio was set to 1.007 times. The film roll was finished in the same manner as in Example 1A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0361] (Comparative Example 8A)
[0362] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 7A, except that the tenter inlet speed ratio was set to 1.015 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0363] (Comparative Example 9A)
[0364] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 8A, except that the tenter inlet speed ratio was set to 1.015 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0365] (Comparative Example 10A)
[0366] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching temperature was set to 150° C., and the film roll was finished in the same manner as in Comparative Example 9A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0367] (Comparative Example 11A)
[0368] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 11A, except that the tenter inlet speed ratio was set to 1.015 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0369] (Comparative Example 12A)
[0370] In the preparation of the biaxially stretched polypropylene film, the longitudinal stretching temperature was set to 150° C. and the tenter inlet speed ratio was set to 1.020 times. The film roll was finished in the same manner as in Comparative Example 11A to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0371] (Comparative Example 13A)
[0372] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 13A, except that the tenter inlet speed ratio was set to 1.015 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1A. The results are shown in Tables 2A to 5A.
[0373] [Table 1A]
[0374]
[0375] [Table 2A]
[0376]
[0377] [Table 3A]
[0378]
[0379] [Table 4A]
[0380]
[0381] [Table 5A]
[0382]
[0383] The polypropylene film rolls of Examples 1A to 14A are obtained by winding a polypropylene film around a core, (1A) the difference between the maximum and minimum values of the lag axis angle obtained by the above methods (a) to (c) is less than 5°, and (2A) when the circumference is measured at the two end positions, the central position, and the positions at intervals of 50 mm from the central position toward the two end positions of the polypropylene film roll, the ratio ΔX of the difference between the maximum value Xmax and the minimum value Xmin of the circumference to the average value Xave of the circumference is 0.2% or less. From the results shown in Table 5A, it can be seen that the polypropylene film rolls of Examples 1A to 14A can perform metal vapor deposition processing on the polypropylene film rolled out from the polypropylene film roll while maintaining high flatness, and the obtained capacitor element has excellent initial withstand voltage and long-term durability under high temperature and high voltage. In addition, the winding deviation caused by wrinkles and relaxation of the film is also suppressed, and the capacitor element can be manufactured with a high yield. In addition, the electrostatic capacitance of the capacitor element of Examples 1A to 14A was measured, and the result was 75 μF in all cases. Therefore, the electrostatic capacitance of the capacitor element in Examples 1A to 14A was excellent.
[0384] In addition, from the results of Examples 1A to 14A and Comparative Examples 1A to 13A, it can be seen that the above-mentioned physical properties (1A) and (2A) of the polypropylene film roll can be appropriately set by adjusting the thickness and width of the polypropylene film, the surface temperature of the casting metal roller, the stretching ratio, the stretching temperature, the tenter speed ratio, the winding tension during cutting, the winding surface pressure, and the surface hardness of the contact roller.
[0385] The second embodiment will be described in detail below with reference to Examples 1B to 14B and Comparative Examples 1B to 9B. However, the second embodiment is not limited to the examples. It should be noted that, unless otherwise specified, parts and % represent "parts by mass" and "mass %", respectively.
[0386] (Example 1B)
[0387] [Example 1B-1. Production of Cast Green Sheet]
[0388] Polypropylene A1 (PP resin A1) and polypropylene B1 (PP resin B1) were supplied to the extruder at a mass ratio of A1:B1=66:34, and after melting at a resin temperature of 230°C, they were extruded using a T-die, wound on a metal roll whose surface temperature was maintained at 95°C and solidified to produce a cast green sheet (thickness 0.11 mm). PP resin A1 had Mw=320,000, Mw / Mn=9.3, difference (DM)=11.2 ("difference (DM)" refers to the difference obtained by subtracting the differential distribution value when Log(M)=6.0 from the differential distribution value when Log(M)=4.5 in the differential distribution curve of molecular weight), meso pentad fraction [mmmm]=95%, MFR=4.9 g / 10 min, and was made from Prime Polymer. In addition, PP resin B1 has Mw=350,000, Mw / Mn=7.7, difference (DM)=7.2, meso pentad fraction [mmmm]=96.5%, MFR=3.8 g / 10 min, and is manufactured by Korea Petrochemical Corporation.
[0389] [Example 1B-2. Preparation of biaxially stretched polypropylene film]
[0390] The obtained cast green sheet was kept at a temperature of 140°C, passed between rollers with a speed difference, stretched in the flow direction (longitudinal stretching) to 4.5 times, and immediately cooled to room temperature. Next, the stretched film obtained by stretching the cast green sheet in the flow direction was introduced into a tenter, stretched to 10 times in the width direction at a transverse stretching temperature of 158°C, relaxed, and wound up at a heat setting temperature of 166°C, and aged at 35°C to obtain a pre-slitting film roll in which a biaxially stretched polypropylene film with a width of 5000 mm and a thickness of 2.5 μm was wound up for 78,000 m.
[0391] [Example 1B-3. Preparation of biaxially stretched polypropylene film roll after cutting]
[0392] like Figure 2 As shown in the schematic diagram, the film is unwound from the obtained pre-cut film roll and cut in the width direction with a cutter. When winding the cut polypropylene film, the following method is adopted: a fiber reinforced plastic core with an outer diameter of 176 mm is used, and a winding device with a contact pressure roller is used to apply surface pressure to the polypropylene film while winding. The cutting conditions are set to a speed of 300m / min, a roll-out tension of 40N / m, a roll-up tension of 50N / m, and a roll-up surface pressure of 400N / m. The contact pressure roller uses a rubber roller with an outer diameter of 152mm and a surface hardness of 40°, and a biaxially stretched polypropylene roll (film roll after cutting) with a finishing width of 620mm and a length of 75000m.
[0393] [Measurement of roll and film characteristic values]
[0394] <The shortest distance ΔL from the middle point of the straight line connecting the two ends of the peeling line to the peeling line>
[0395] The shortest distance ΔL of the biaxially stretched polypropylene film roll obtained in Example 1B was measured in the same manner as in Examples 1A to 14A and Comparative Examples 1A to 13A. The results are shown in Table 2B.
[0396] <Measurement of the ratio ΔX of the circumferential length>
[0397] For the biaxially stretched polypropylene film roll obtained in Example 1B, the ratio ΔX ((Xmax-Xmin) / Xave) of the difference between the maximum value Xmax and the minimum value Xmin of the circumference (Xmax-Xmin) to the average value Xave of the circumference was calculated in the same manner as in Examples 1A to 14A and Comparative Examples 1A to 13A. The results are shown in Table 2B.
[0398] <Measurement of the difference between the maximum and minimum values of the slow axis angle>
[0399] For the biaxially stretched polypropylene film roll obtained in Example 1B, the difference between the maximum value and the minimum value of the slow axis angle was determined in the same manner as in Examples 1A to 14A and Comparative Examples 1A to 13A. The results are shown in Table 2B.
[0400] <Measurement of coil hardness>
[0401] The roll hardness (surface hardness) was measured using a rubber hardness tester according to JIS K6301 at both ends, the center, and the positions 50 mm apart from the center toward both ends of the obtained biaxially stretched polypropylene film roll. The results of the average value Mave of the hardness and the difference ΔM between the maximum value Mmax and the minimum value Mmin of the hardness are shown in Table 2B.
[0402] <Measurement of thickness of biaxially stretched polypropylene film>
[0403] The thickness of the biaxially stretched polypropylene film unwound from the biaxially stretched polypropylene film roll obtained in Example 1B was measured using a micrometer (JIS-B7502) in accordance with JIS-C2330. The results are shown in Table 1B.
[0404] <Ash content measurement of biaxially stretched polypropylene film>
[0405] The ash content (ppm) of the biaxially stretched polypropylene films obtained in Example 1B and Examples 2B to 14B described below was measured in the same manner as in Examples 1A to 14A. The ash content of the polypropylene films in any of the examples was 20 ppm.
[0406] <Deformation rate at stress 25MPa>
[0407] For the biaxially stretched polypropylene film rolled out from the biaxially stretched polypropylene film roll obtained in Example 1B, the deformation rates ε1 (MD), ε2 (TD) and ε3 (diagonal) at a stress of 25 MPa were determined in the same manner as in Examples 1A to 14A and Comparative Examples 1A to 13A. The results are shown in Table 2B.
[0408] <Measurement of surface roughness>
[0409] The centerline average roughness (Ra) and Rz (Rmax defined in the old JIS) of the biaxially stretched polypropylene film were measured by a contact method using a three-dimensional surface roughness meter (Surfcom1400D-3DF-12 model) manufactured by Tokyo Seimitsu Co., Ltd. according to the method specified in JIS-B0601. The measurement was performed 3 times and the average value was obtained. Ra and Rz were measured using the contact method, and the reliability of the values was confirmed by the non-contact method as required. The results are shown in Table 2B.
[0410] <Evaluation of the yield rate of film rolls after cutting>
[0411] In [Example 1B-3. Preparation of biaxially stretched polypropylene film roll], the film being wound was visually checked, and all those with wrinkles were deemed unqualified. In addition, regarding winding deviation, when observed from the end face of the cut roll, the case where a deviation of more than 2 mm was generated was deemed unqualified. For all the cut rolls, the ratio of the number of cut film rolls that were qualified based on the above criteria was calculated as the cutting yield, and the following criteria were given for evaluation. The results are shown in Table 2B.
[0412] A: 100%
[0413] B: 80% or more and less than 100%
[0414] C: less than 80%
[0415] [Example 1B-4. Fabrication of capacitor]
[0416] Next, the obtained biaxially stretched polypropylene film roll is used to make a capacitor in the following manner. A vacuum vapor deposition machine manufactured by ULVAC Co., Ltd. is used to perform aluminum vapor deposition T-edge vapor deposition pattern on the biaxially stretched polypropylene film with a vapor deposition resistance of 15Ω / □, thereby obtaining a metallized film containing a metal film on one side of the biaxially stretched polypropylene film. After slitting to a width of 60mm, the two metallized films are aligned and wound with 1076 turns at a winding tension of 250g using an automatic winder 3KAW-N2 manufactured by Kaito Seisakusho Co., Ltd. The wound element is pressurized and heat treated at 120°C for 15 hours, and then zinc metal is sprayed on the end surface of the element to obtain a flat capacitor. Leads are welded to the end surface of the flat capacitor and then sealed with epoxy resin.
[0417] [Evaluation of Processability of Capacitor Element]
[0418] <Evaluation of Vapor Deposition Film Unevenness>
[0419] The metallized film before slitting of the above [Example 1B-4. Production of capacitors] was evaluated for vapor deposition unevenness in the same manner as in Examples 1A to 14A and Comparative Examples 1A to 13A, and evaluated in the following four levels of A to D. The results are shown in Table 2B.
[0420] A: The maximum value among the deviations of L* value, a* value, and b* value is less than 5%
[0421] B: The maximum value among the deviations of L* value, a* value, and b* value is 5% or more and less than 10%
[0422] C: The maximum value among the deviations of L* value, a* value, and b* value is 10% or more and less than 20%
[0423] D: The maximum value among the deviations of L* value, a* value, and b* value is 20% or more
[0424] <Evaluation of Yield of Capacitor Element Manufacturing>
[0425] In the above [Example 1B-4. Production of capacitors], the film during the conveying process was visually confirmed, and all wrinkles were considered unqualified. In addition, regarding the winding deviation, the element with a deviation of 0.2 mm or more when observed from the end face of the capacitor element was considered unqualified. 100 elements were made, and the ratio of the number of qualified capacitor elements was calculated as the element yield, and evaluated according to the following criteria. The results are shown in Table 2B.
[0426] A: 100%
[0427] B: 90% or more and less than 100%
[0428] C: 80% or more and less than 90%
[0429] D: less than 80%
[0430] [Evaluation of long-term durability of capacitor elements]
[0431] <Capacitance change rate ΔC>
[0432] For the capacitor element obtained in the above [Example 1B-4. Preparation of capacitor], the capacitance change rate (ΔC) before and after voltage loading was calculated in the same manner as in Examples 1A to 14A and Comparative Examples 1A to 13A, and the average value of 5 capacitors was used for evaluation according to the following criteria. The results are shown in Table 2B.
[0433] A+: -0.5% or more
[0434] A: Less than -0.5% and -1% or more
[0435] B: less than -1% and more than -5%
[0436] C: less than -5% and more than -10%
[0437] D: less than -10%
[0438] (Example 2B)
[0439] In the preparation of the biaxially stretched polypropylene film roll, the surface hardness of the contact roller was set to 55°, and the film roll was finished in the same manner as in Example 1B to prepare a capacitor (Table 1B). In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0440] (Example 3B)
[0441] In the preparation of the biaxially stretched polypropylene film roll, the winding surface pressure was set to 350 N / m, and the film roll was finished in the same manner as in Example 1B to produce a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0442] (Example 4B)
[0443] In the preparation of the biaxially stretched polypropylene film roll, the surface hardness of the contact roller was set to 55° and the winding surface pressure was set to 350 N / m. The film roll was finished in the same manner as in Example 1B to produce a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0444] (Example 5B)
[0445] In the preparation of the biaxially stretched polypropylene film roll, the surface hardness of the contact roller was set to 65° and the winding surface pressure was set to 320 N / m. The film roll was finished in the same manner as in Example 1B to produce a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0446] (Example 6B)
[0447] In the preparation of the biaxially stretched polypropylene film roll, the winding tension was set to 65 N / m, and the film roll was finished in the same manner as in Example 1B to produce a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0448] (Example 7B)
[0449] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1B, except that the film was stretched in the flow direction (longitudinal stretching) to 4.00 times, and a capacitor was prepared. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0450] (Example 8B)
[0451] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1B, except that the film was stretched in the flow direction (longitudinal stretching) to 4.90 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0452] (Example 9B)
[0453] In the preparation of the biaxially stretched polypropylene film, the film roll was stretched to 4.95 times in the flow direction (longitudinal stretching), the winding tension was set to 48 N / m, and the winding surface pressure was set to 390 N / m. The capacitor was produced in the same manner as in Example 1B. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0454] (Example 10B)
[0455] The film roll was finished in the same manner as in Example 1B, except that the film thickness was 2.0 μm, to produce a capacitor. The biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0456] (Example 11B)
[0457] In the preparation of the biaxially stretched polypropylene film roll, the film roll was finished in the same manner as in Example 1B, except that the finishing width of the roll was set to 820 mm. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0458] (Example 12B)
[0459] In the preparation of the biaxially stretched polypropylene film, the surface temperature of the casting metal roll was set to 93° C., and the film roll was finished in the same manner as in Example 1B to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0460] (Example 13B)
[0461] In the preparation of the biaxially stretched polypropylene film, the surface temperature of the casting metal roll was set to 97° C., and the film roll was finished in the same manner as in Example 1B to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0462] (Example 14B)
[0463] The film roll was finished in the same manner as in Example 1B to produce a capacitor, except that the film thickness was set to 2.0 μm, the finished width of the roll was set to 820 m, and the tenter inlet speed ratio was slightly reduced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0464] (Comparative Example 1B)
[0465] In the preparation of the biaxially stretched polypropylene film roll, the surface hardness of the contact roller was set to 65°, and the film roll was finished in the same manner as in Example 1B to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0466] B In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0467] (Comparative Example 2B)
[0468] In the preparation of the biaxially stretched polypropylene film roll, the surface hardness of the contact roller was set to 70°, and the film roll was finished in the same manner as in Example 1B to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0469] (Comparative Example 3B)
[0470] In the preparation of the biaxially stretched polypropylene film roll, the surface hardness of the contact roller was set to 75°, and the film roll was finished in the same manner as in Example 1B to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0471] (Comparative Example 4B)
[0472] In the preparation of the biaxially stretched polypropylene film roll, the winding tension was set to 80 N / m, and the film roll was finished in the same manner as in Example 1B to produce a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0473] (Comparative Example 5B)
[0474] In the preparation of the biaxially stretched polypropylene film roll, the winding surface pressure was set to 450 N / m, and the film roll was finished in the same manner as in Example 1B to produce a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0475] (Comparative Example 6B)
[0476] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1B, except that the film was stretched in the flow direction (longitudinal stretching) to 3.90 times, and a capacitor was produced. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0477] (Comparative Example 7B)
[0478] In the preparation of the biaxially stretched polypropylene film, the film roll was finished in the same manner as in Example 1B, except that the film was stretched in the flow direction (longitudinal stretching) to 5.00 times, and a capacitor was prepared. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0479] (Comparative Example 8B)
[0480] In the preparation of the biaxially stretched polypropylene film, the surface temperature of the casting metal roll was set to 91° C., and the film roll was finished in the same manner as in Example 1B to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0481] (Comparative Example 9B)
[0482] In the preparation of the biaxially stretched polypropylene film, the surface temperature of the casting metal roll was set to 98° C., and the film roll was finished in the same manner as in Example 1B to prepare a capacitor. In addition, the biaxially stretched polypropylene film and the capacitor element were evaluated in the same manner as in Example 1B. The results are shown in Table 2B.
[0483] [Table 1B]
[0484]
[0485] [Table 2B]
[0486]
[0487] The polypropylene film rolls of Examples 1B to 14B are obtained by winding a polypropylene film having a thickness of less than 20 μm and a width of more than 200 mm around a core, wherein (1B) when the polypropylene film is unwound from the polypropylene film roll at a unwinding tension of 3 N / m and a speed of 2 m / min under an environment of a temperature of 23° C. and a humidity of 60%, the shortest distance ΔL from the midpoint of a straight line connecting the two ends of a boundary line for peeling the polypropylene film from the polypropylene film roll to the peeling line is less than 20 mm, and (2B) when the circumference is measured at the two end positions, the central position, and positions at intervals of 50 mm from the central position toward the two end positions of the polypropylene film roll, the ratio ΔX of the difference (Xmax-Xmin) between the maximum value Xmax and the minimum value Xmin of the circumference to the average value Xave of the circumference is less than 0.2%. From the results shown in Table 2B, it can be seen that the polypropylene film rolls of Examples 1B to 14B can perform metal vapor deposition processing with high precision while maintaining high flatness on the polypropylene film rolled out from the polypropylene film roll, and the obtained capacitor elements have excellent long-term durability under high temperature and high voltage. In addition, the winding deviation caused by wrinkles and relaxation of the film and the reduction in yield due to cutting are also suppressed, and capacitor elements can be manufactured with a high yield.
[0488] In addition, from the results of Examples 1B to 14B and Comparative Examples 1B to 9B, it can be seen that the above-mentioned physical properties (1B) and (2B) of the polypropylene film roll can be appropriately set by adjusting the thickness and width of the polypropylene film, the surface temperature of the casting metal roller, the stretch ratio, the winding tension during cutting, the winding surface pressure, and the surface hardness of the contact roller.
[0489] Specifically, for example, in Examples 1B to 4B, the surface temperature of the cast metal roller is set to 94 to 95°C, the longitudinal stretch ratio is set to 4.2 to 4.8 times, the film has a moderate surface roughness and mechanical strength, and excellent processability. In addition, the rubber hardness of the contact roller is 40 to 55°, the surface rubber of the contact roller easily follows the shape of the film roll, and the surface pressure during winding is easily applied uniformly in the width direction. Furthermore, the winding tension is 50 to 60 N / m, and the winding surface pressure is 320 to 400 N / m, and no poor appearance such as buckling, end face deviation, and wrinkles are generated on the film roll. The film rolls of Examples 1B to 4B obtained in this way meet the physical properties of (1B) and (2B) above, and capacitor elements with extremely excellent long-term durability can be manufactured. In addition, there is no generation of wrinkles or uneven evaporation even during processing, and it can be used as a polypropylene film roll that is extremely suitable in terms of cost.
[0490] In addition, in Example 5B, a relatively hard rubber contact roller with a rubber hardness of 65° is used. If the rubber hardness is high, it is difficult for the surface rubber to follow the shape of the film roll. Therefore, in Example 5B, the surface pressure is reduced to 320N / m and adjusted to uniformly contact the width direction of the film roll so that the physical properties of (1B) and (2B) above are satisfied. Similar to Examples 1B to 4B, the long-term durability of the capacitor element made from the film roll of Example 5B is extremely excellent. In addition, even during processing, there is no generation of wrinkles and uneven evaporation, and it can be used as a polypropylene film roll that is extremely suitable in terms of cost.
[0491] On the other hand, Comparative Example 1B is the same as Example 1B except that the rubber hardness is changed to 65°. The surface rubber is difficult to follow the shape of the film roll, and the surface pressure during winding tends to become uneven. The shortest distance ΔL of the film roll obtained in this way becomes larger, resulting in the physical properties of the above (1B) not being satisfied. In addition, the long-term durability of the capacitor element made by the roll is poor. Furthermore, even during processing, the film cannot maintain flatness, wrinkles, and relaxation occur, and satisfactory processability cannot be obtained.
[0492] Comparative Example 2B is the same as Example 1B except that the rubber hardness is changed to 70°. Compared with Comparative Example 1B, the surface rubber is more difficult to follow the shape of the film roll, and the surface pressure during winding is more likely to become uneven. The film roll thus obtained has a tendency to further increase the shortest distance ΔL, and the long-term durability of the capacitor element made from the roll is poor. In addition, even during processing, the film cannot maintain flatness, wrinkles, and sag, and satisfactory processability cannot be obtained.
[0493] Comparative Example 3B is the same as Example 1B except that the rubber hardness is changed to 75°. In Comparative Example 3B, the non-uniformity of the surface pressure is further developed compared with Comparative Examples 1B and 2B, and there is a tendency to be wound harder in the portion with large film thickness. Therefore, both the shortest distance ΔL and the circumferential length difference ΔX become larger. The long-term durability of the capacitor element made by such a roll is extremely poor. Even during processing, the film cannot maintain flatness, wrinkles and sags frequently, and satisfactory processability cannot be obtained.
[0494] In Example 6B, the winding tension is set to 65 N / m, which is greater than that in Example 1B. In Example 6B, the slight difference in film thickness affects the air layer, and the circumferential length difference ΔX is greater than that in Example 1B. However, the physical properties of (1B) and (2B) are satisfied, and a film roll having excellent long-term durability and suitable for processing can be obtained.
[0495] In Comparative Example 4B, the winding tension was set to 80 N / m, which was further increased compared to Example 6B. In Comparative Example 4B, due to the excessive tension, the circumferential length difference ΔX was larger than that of Example 6B, and the physical property (1B) was not satisfied, and both long-term durability and processability could not be satisfied.
[0496] In Comparative Example 5B, the winding surface pressure is set to 450 N / m, making the winding surface pressure greater than that of Example 1B. If the winding surface pressure is too large as in Comparative Example 5B, the surface pressure during winding becomes uneven, and there is a tendency for the winding to be harder locally (especially in the thick part of the film). The shortest distance ΔL and the circumferential length difference ΔX of the film roll obtained in this way become larger, and neither can meet the physical properties of (1B) and (2B) above. The long-term durability of the capacitor element made from such a roll is extremely poor. In addition, even during processing, the film cannot maintain flatness, wrinkles and sags frequently, and the processability is not satisfactory.
[0497] In Examples 7B and 8B, the longitudinal stretch ratio is changed from 4.50 times of Example 1B to 4.00 times or 4.90 times. If the longitudinal stretch ratio is reduced, the deformation rate becomes larger. Therefore, the film is easily stretched due to the tension of the processing machine, and there is a tendency for the shortest distance ΔL to become larger. If the longitudinal stretch ratio is increased, the followability of the film roll during winding is reduced (the deformation rate is reduced), and the film roll is wound harder locally (especially in the thick part of the film), so the circumferential length difference ΔX becomes larger. However, the film rolls of Examples 7B and 8B can meet both long-term durability and processability by satisfying the physical properties of (1B) and (2B) above.
[0498] On the other hand, in Comparative Example 6B, the longitudinal stretching ratio is too small, 3.9 times, and in Comparative Example 7B, the longitudinal stretching ratio is too large, 5.0 times, so the physical properties of (1B) or (2B) mentioned above are not satisfied, and both long-term durability and processability cannot be satisfied.
[0499] In Example 9B, the longitudinal stretch ratio was changed from 4.50 times in Example 1B to 4.95 times. If the longitudinal stretch ratio is increased, the followability of the film roll during winding is reduced (the deformation rate is reduced), and the film roll is wound harder locally (especially in the thick film portion), so the circumferential length difference ΔX becomes larger. However, the film roll of Example 9B can satisfy both long-term durability and processability by satisfying the above-mentioned physical properties (1B) and (2B).
[0500] In Example 10B, the thickness of the film was changed from 2.5 mm in Example 1B to 2.0 μm. A pressure difference was generated between the upper and lower surfaces of the rolled film, and the film was subjected to forces in the floating and descending directions, thereby changing the peeling position. There is a tendency that the thinner the film thickness, the greater the influence. Therefore, compared with Example 1B, in Example 10B, the shortest distance ΔL becomes larger, but by satisfying the above-mentioned physical properties of (1B) and (2B), both long-term durability and processability can be satisfied.
[0501] In Example 11B, the roll width was changed from 620 mm in Example 1B to 820 mm. As the roll width increases, the surface pressure applied to the film roll tends to become uneven, and there is a tendency for the film roll to be partially wound harder. Therefore, there is a tendency for the circumferential length difference ΔX to become larger, but by satisfying the above-mentioned physical properties (1B) and (2B), both long-term durability and processability can be satisfied.
[0502] In Examples 12B and 13B, the surface temperature of the casting metal drum is changed from that of Example 1B. If the temperature is low, the film surface is smoothed, and if the temperature is high, it is roughened. If smoothing progresses, there is a tendency for the shortest distance ΔL to become larger due to sliding when the film is unrolled. If roughening progresses, there is a tendency for the amount of air sucked in during winding to increase and the circumferential length difference ΔX to become larger. In Examples 12B and 13B, by satisfying the above-mentioned physical properties of (1B) and (2B), both long-term durability and processability can be satisfied.
[0503] On the other hand, in Comparative Example 8B, the surface temperature of the casting metal drum was too low, so the film roll could not meet the physical properties of (1B) above, and could not meet both long-term durability and processability. In addition, the slip was poor, and there was a tendency to generate wrinkles on the roller of the processing machine.
[0504] In Comparative Example 9B, the surface temperature of the casting metal drum was too high, so the film roll could not meet the physical properties of (2B) above, and could not meet both long-term durability and processability. In addition, when the film was unwound from the film roll, there was a tendency for winding deviation to occur and the film to meander on the roller of the processing machine.
[0505] In addition, the electrostatic capacitance of the capacitor element of Examples 1B to 14B was measured, and the result was 75 μF in all cases. Therefore, the electrostatic capacitance of the capacitor element in Examples 1B to 14B was excellent.
[0506] Explanation of symbols
[0507] 1 Polypropylene film
[0508] 2 cores
[0509] 10 Polypropylene film rolls
[0510] x1 Stripping wire end
[0511] x2 Other end of stripped wire
[0512] L Roll out direction
[0513] M Circumferential direction
[0514] ΔL The shortest distance from the midpoint of the straight line connecting the two ends of the peel line to the peel line
[0515] P The middle point of the straight line connecting the two ends of the stripping line
[0516] Q From the middle point P to the shortest point of the stripping line
[0517] S Stripping line
[0518] T A straight line connecting the two ends of the stripping line
[0519] U Baseline.
Claims
1. A polypropylene film roll, which is formed by winding a polypropylene film around a core, wherein the polypropylene film roll satisfies the following physical properties (1A) and (2A), (1A) The difference between the maximum and minimum values of the slow axis angle obtained by the following methods (a) to (c) is less than 5°, (a) When the total length in the width direction of the polypropylene film is set to 100%, nine samples for measurement of 50 mm x 50 mm are cut out, centered at positions every 10% from both ends of the polypropylene film, (b) setting the width direction of the measurement sample to 0°, measuring the acute angle between the width direction of the measurement sample and the slow axis as the slow axis angle, (c) finding the difference between the maximum and minimum values of the slow axis angles measured in (b) among the nine samples for measurement, (2A) when the circumference of the polypropylene film roll is measured at the two end positions, the center position, and the positions at intervals of 50 mm from the center position toward the two end positions, the ratio ΔX of the difference between the maximum value Xmax and the minimum value Xmin of the circumference, i.e., Xmax-Xmin, to the average value Xave of the circumference is less than 0.2%, The polypropylene film has a deformation rate ε1 in the longitudinal direction, a deformation rate ε2 in the width direction, and a deformation rate ε3 in the diagonal direction at a stress of 25 MPa, each in a range of 0.6% or more and 1.5% or less.
2. The polypropylene film roll according to claim 1, in, The width of the polypropylene film is greater than 200 mm.
3. The polypropylene film roll according to claim 1 or 2, in, The polypropylene film has a thickness of 6.0 μm or less.
4. The polypropylene film roll according to claim 1 or 2, in, The winding length of the polypropylene film is greater than 10000 m.
5. The polypropylene film roll according to claim 1 or 2, in, The polypropylene film roll is used to manufacture a metallized polypropylene film for capacitors by laminating a metal film on one side or both sides of the polypropylene film.
6. A polypropylene film roll, which is formed by winding a polypropylene film around a core, The polypropylene film has a thickness of less than 20 μm and a width of more than 200 mm. The polypropylene film satisfies the following physical properties (1B) and (2B), (1B) when the polypropylene film is unwound from the polypropylene film roll at an unwinding tension of 3 N / m and a speed of 2 m / min under an environment of a temperature of 23° C. and a humidity of 60%, the shortest distance ΔL from the middle point of a straight line connecting both ends of a peeling line to the peeling line is less than 20 mm, the peeling line being a boundary line at which the polypropylene film is peeled from the polypropylene film roll, (2B) when the circumference of the polypropylene film roll is measured at the two end positions, the center position, and positions at intervals of 50 mm from the center position toward the two end positions, the ratio ΔX of the difference between the maximum value Xmax and the minimum value Xmin of the circumference, i.e., Xmax-Xmin, to the average value Xave of the circumference is less than 0.2%, The polypropylene film has a deformation rate ε1 in the longitudinal direction, a deformation rate ε2 in the width direction, and a deformation rate ε3 in the diagonal direction at a stress of 25 MPa, each in a range of 0.6% or more and 1.5% or less.
7. The polypropylene film roll according to claim 6, in, When the hardness is measured at the two end positions, the central position and the positions 50 mm apart from the central position toward the two end positions of the polypropylene film roll, the average hardness value Mave is greater than 88° and less than 96°, and the difference ΔM between the maximum hardness value Mmax and the minimum hardness value Mmin is less than 4°.
8. The polypropylene film roll according to claim 6 or 7, in, The surface roughness of at least one surface of the polypropylene film has a center line average roughness Ra of 0.04 μm to 0.08 μm, and a maximum height Rz of 0.3 μm to 0.9 μm.
9. The polypropylene film roll according to claim 6 or 7, in, The winding length of the polypropylene film is greater than 10000 m.
10. The polypropylene film roll according to claim 6 or 7, in, The polypropylene film roll is used to manufacture a metallized polypropylene film for capacitors by laminating a metal film on one side or both sides of the polypropylene film. 11 . A metallized polypropylene film roll, wherein a metal film is laminated on one or both sides of the polypropylene film of the polypropylene film roll according to claim 1 .