A water-soluble polyaniline / MXene composite flexible ammonia sensor and preparation method thereof

By induced synthesis of water-soluble polyaniline and MXene composite materials in traditional NH3 sensors, the problems of high temperature, poor safety and low sensitivity of traditional NH3 sensors are solved, and the room temperature with high sensitivity and stability are achieved NH3 sensor, suitable for wearable devices and industrial applications.

CN113984849BActive Publication Date: 2024-12-06DONGGUAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111272592.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-12-06
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Traditional NH3 sensors have problems such as high operating temperature, poor safety, large energy consumption, low sensitivity and poor stability, and are not suitable for the needs of wearable electronic devices. The processing performance of a single polyaniline material also limits its application.

Method used

The PANI:PSS/MXene composite material was prepared by induced by induced synthesis of water-soluble polyaniline (PANI) nanoparticles using polymer polyelectrolyte sodium styrene sulfonate (PSS) as a template and composited with MXene nanosheets, and PANI:PSS/MXene composite material was prepared and in situ deposition was carried out. On the polymer flexible substrate, a room temperature flexible NH3 sensor was prepared with high sensitivity and good stability.

Benefits of technology

It realizes high sensitivity detection (sensitivity up to 0.56) and good stability, and is low-cost and suitable for industrial mass production. The sensors exhibit high selectivity and good durability at room temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003329201140000011
    Figure HDA0003329201140000011
  • Figure HDA0003329201140000012
    Figure HDA0003329201140000012
  • Figure HDA0003329201140000021
    Figure HDA0003329201140000021
Patent Text Reader

Abstract

The present invention relates to a water-soluble polyaniline / MXene composite flexible ammonia sensor and a preparation method thereof, and belongs to the field of nano-functional material preparation. A water-soluble polyaniline / MXene composite flexible ammonia sensor, the ammonia sensor is composed of a polymer flexible substrate and a PANI:PSS / MXene composite film deposited on the substrate, and the polyaniline / MXene composite flexible ammonia sensor is prepared by the following method: aniline, PSS, and MXene nanosheets are sequentially added to hydrochloric acid to obtain a mixed solution; ammonium persulfate solution is added dropwise to the mixed solution, and the polymer flexible substrate is quickly added to react at room temperature to obtain. The flexible NH3 sensor polymer substrate does not require electrodes, has low cost, is easy to process, and is conducive to industrial mass production. The flexible sensor prepared by the present invention has a sensitivity of up to 0.56 to 1ppm NH3 at room temperature, good stability, and high selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a water-soluble polyaniline / MXene composite flexible ammonia sensor and a preparation method thereof, and belongs to the field of nano functional material preparation. Background Art

[0002] With the rapid development of modern society, gas sensors play an increasingly important role in industrial production, environmental monitoring, disease diagnosis, and military counter-terrorism. Ammonia (NH3), as a typical colorless toxic pollutant gas, exists in many aspects of human life. Low concentrations of NH3 can cause damage to human eyes and respiratory tract, and high concentrations of NH3 can cause people to faint or even die. NH3 is also a human metabolite and can be used as a marker to monitor the health of various organs in the human body, such as the liver, duodenum, and cavity. In addition, NH3 can also be used as a marker to detect the freshness of food and monitor the atmosphere at a specific fire scene. Therefore, the development of high-performance NH3 sensors is of great significance to human health and the ecological environment.

[0003] Traditional NH3 sensors generally use metal oxides as gas-sensitive materials. Such sensors have the disadvantages of high operating temperature, poor safety and high energy consumption, and are not suitable for wearable electronic devices that are increasingly in demand. Polyaniline (PANI), as a conductive polymer, has the advantages of low cost, simple synthesis and room temperature operation, and is considered to be a room temperature NH3 sensitive material with great potential. However, NH3 sensors based on single PANI materials usually have disadvantages such as low sensitivity and poor stability; at the same time, the poor processing performance of PANI further limits the practical application of such sensors. Therefore, it is of great research value to prepare processable water-soluble PANI composite sensitive materials and combine the advantages of different materials to obtain high-performance room temperature flexible NH3 sensors.

[0004] The composite of PANI and two-dimensional nanomaterials is one of the effective methods to improve the NH3 sensitivity of single PANI materials. As a new type of two-dimensional nanomaterial, MXene has the characteristics of excellent conductivity, rich surface functional groups and large specific surface area, which has attracted widespread attention in the field of gas sensors. Summary of the invention

[0005] The present invention uses polymer polyelectrolyte sodium polystyrene sulfonate (PSS) as a template to induce the synthesis of water-soluble PANI nanoparticles (PANI:PSS), which are then composited with MXene nanosheets to prepare a new NH3 sensitive material PANI:PSS / MXene; by in situ depositing PANI:PSS / MXene onto a cheap polymer flexible substrate, a room-temperature flexible NH3 sensor with high sensitivity, good stability and high selectivity based on the composite material is prepared.

[0006] The object of the present invention is to provide a water-soluble polyaniline / MXene composite flexible ammonia sensor and a preparation method thereof.

[0007] A water-soluble polyaniline / MXene composite flexible ammonia sensor, the ammonia sensor is composed of a polymer flexible substrate and a PANI:PSS / MXene composite film deposited on the substrate, wherein:

[0008] The polyaniline / MXene composite flexible ammonia sensor is prepared according to the following method: 30 to 150 μL of aniline, PSS, and MXene nanosheets are sequentially added to 80 ml of 0.5 M hydrochloric acid, wherein the mass ratio of PSS to aniline is 1:1 to 1:9, and the mass of MXene nanosheets is 2.0 to 40 wt % of aniline, and stirred at 900 to 2000 rpm for 1 h at room temperature to obtain a mixed solution; ammonium persulfate solution is added dropwise to the mixed solution, and a polymer flexible substrate is quickly added to react at room temperature for 8 to 24 h; the flexible substrate with the PANI:PSS / MXene composite film deposited is taken out, washed with deionized water, and dried at room temperature to obtain a mixed solution, wherein the ammonium persulfate solution is prepared by dissolving 200 to 600 mg of ammonium persulfate in 5 ml of 0.5 M hydrochloric acid.

[0009] Preferably, the MXene nanosheets are prepared by the following method: 8 g of LiF is added to 100 ml of 6-9 M hydrochloric acid and stirred to dissolve; after sufficient dissolution, a MAX powder selected from Ti3AlC2, Ti2AlC, Ti4AlN3, Ti2AlN, Nb4AlC3, Nb2AlC, V2AlC, Ta2AlC, Mo2TiAlC2, Mo2Ti2AlC3, and MoYAlC is slowly added, and the mixture is stirred and reacted at 20-60° C. for 24-168 h, with a mass ratio of MAX powder to LiF of 1:1-1:3; after the reaction is completed, the mixture is centrifuged and washed with deionized water for 5-10 times, the centrifuged product is dispersed with deionized water, the dispersion is ultrasonically treated for 1-6 h, and then freeze-dried to obtain MXene nanosheets.

[0010] Preferably, the polymer flexible substrate is a PET, PI or PDMS substrate.

[0011] Furthermore, the substrate needs to be pretreated, and the specific steps are: cut the flexible PET, PI or PDMS substrate into a width of 5 to 15 mm and a length of 5 to 20 mm, ultrasonically wash it with deionized water, acetone, and ethanol respectively, with an ultrasonic frequency of 25 to 80 KHZ, and treat the substrate with oxygen plasma for 5 to 30 minutes after drying.

[0012] Another object of the present invention is to provide a method for preparing the above-mentioned water-soluble polyaniline / MXene composite flexible ammonia sensor.

[0013] A method for preparing a water-soluble polyaniline / MXene composite flexible ammonia sensor comprises the following process steps:

[0014] (1) Cut the flexible PET, PI or PDMS substrate into pieces with a width of 5 to 15 mm and a length of 5 to 20 mm, and wash them with deionized water, acetone, and ethanol ultrasonically at a frequency of 25 to 80 kHz. After drying, treat the substrate with oxygen plasma for 5 to 30 min and set aside for use.

[0015] (2) Add 8 g of LiF to 100 ml of 6-9 M hydrochloric acid and stir to dissolve; after sufficient dissolution, slowly add one MAX powder selected from Ti3AlC2, Ti2AlC, Ti4AlN3, Ti2AlN, Nb4AlC3, Nb2AlC, V2AlC, Ta2AlC, Mo2TiAlC2, Mo2Ti2AlC3, and MoYAlC, and stir to react at 20-60 °C for 24-168 h. The mass ratio of MAX powder to LiF is 1:1-1:3. After the reaction, centrifuge and wash with deionized water for 5-10 times. The centrifuged product is dispersed with deionized water. The dispersion is ultrasonically treated for 1-6 h and then freeze-dried to obtain MXene nanosheets.

[0016] (3) 30-150 μL of aniline, PSS, and MXene nanosheets were added to 80 ml of 0.5 M hydrochloric acid in sequence, wherein the mass ratio of PSS to aniline was 1:1-1:9, and the mass of MXene nanosheets was 2.0-40 wt% of aniline, and stirred at 900-2000 rpm for 1 h at room temperature to obtain a mixed solution; ammonium persulfate solution was added dropwise to the mixed solution, and then quickly added to a polymer flexible substrate, and reacted at room temperature for 8-24 h; the flexible substrate with the PANI:PSS / MXene composite film deposited was taken out, washed with deionized water, and then dried at room temperature to obtain a mixed solution, wherein the ammonium persulfate solution was prepared by dissolving 200-600 mg of ammonium persulfate in 5 ml of 0.5 M hydrochloric acid.

[0017] The beneficial effects of the present invention are as follows: the water-soluble PANI synthesized by inducing the polymer polyelectrolyte PSS as a template has a nano-microsphere structure, and the nano-microsphere PANI is distributed on the surface of the MXene nanosheet. The introduction of the nano-microsphere structure effectively increases the contact area between the composite material and NH3 and the diffusion and penetration of the gas, and improves the MH3 sensitivity of the PANI:PSS / MXene composite material; the introduction of the MXene nanosheet effectively improves the conductivity of the water-soluble PANI, and the rich surface functional groups on its surface increase the NH3 adsorption active sites of the PANI:PSS / MXene composite material, which helps to improve the sensitivity of the sensor; PSS is not only a template agent for PANI, but also a dopant for PANI, which improves the stability of the sensor. The flexible NH3 sensor polymer substrate does not require electrodes, has low cost, is easy to process, and is conducive to industrial mass production. The flexible sensor prepared by the present invention has a sensitivity of up to 0.56 to 1 ppm NH3 at room temperature, and has good stability and high selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a SEM image of Ti3C2MXene nanosheets prepared in Example 3 of the present invention.

[0019] Figure 2 This is the SEM image of the PANI:PSS / MXene composite material in Example 3 of the present invention.

[0020] Figure 3 Sensitivity diagram of the flexible NH3 sensors prepared in Examples 1 to 5 of the present invention and Comparative Example 1 to 1 ppm NH3 at room temperature. (Sensitivity S: S=∆R / R o , where ∆R is the resistance difference between the sensor in NH3 and air, R o is the resistance value of the sensor in air).

[0021] Figure 4 3 is the sensitivity change curve of the flexible NH3 sensor prepared in Example 3 of the present invention to 1-10 ppm NH3 at room temperature. DETAILED DESCRIPTION

[0022] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0023] The test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0024] Example 1

[0025] (1) The flexible PET was cut into pieces with a width of 10 mm and a length of 20 mm, and ultrasonically washed with deionized water, acetone, and ethanol at an ultrasonic frequency of 25 kHz. After drying, the substrate was treated with oxygen plasma for 5 min and set aside for use.

[0026] (2) 8 g of LiF was added to 100 ml of 6 M hydrochloric acid and stirred to dissolve. After sufficient dissolution, 8 g of Ti3AlC2 powder was slowly added and stirred at 20°C for 24 h. After the reaction was completed, the mixture was centrifuged and washed with deionized water for 5 times. The centrifuged product was dispersed with deionized water. The dispersion was ultrasonically treated for 1 h and then freeze-dried to obtain Ti3C2MXene nanosheets.

[0027] (3) 96.7 μL of aniline, 32.9 mg of PSS, and MXene nanosheets were added to 80 ml of 0.5 M hydrochloric acid in sequence (the mass of MXene nanosheets was 2.0 wt% of aniline). The mixture was stirred vigorously at 900 rpm for 1 h at room temperature. Then, ammonium persulfate solution (200 mg of ammonium persulfate dissolved in 5 ml of 0.5 M hydrochloric acid) was added dropwise to the mixture and quickly added to the prepared flexible substrate. The mixture was reacted at room temperature for 8 h. The flexible substrate on which the PANI:PSS / MXene composite sensitive material was deposited was taken out, washed with deionized water, and dried at room temperature. Thus, a flexible NH3 sensor based on PANI:PSS / MXene sensitive material was prepared.

[0028] (4) The prepared flexible NH3 sensor was connected to a CHI 760E electrochemical workstation and placed in an atmosphere of air and 1 ppm NH3 for current signal testing. The current change was converted into response change using mathematical methods, and the sensitivity of the sensor was calculated to be 0.32.

[0029] Example 2

[0030] (1) The flexible PET substrate was cut into pieces with a width of 10 mm and a length of 20 mm. The pieces were ultrasonically cleaned with deionized water, acetone, and ethanol at an ultrasonic frequency of 80 kHz. After drying, the substrate was treated with oxygen plasma for 30 min and set aside for use.

[0031] (2) 8 g of LiF was added to 100 ml of 9 M hydrochloric acid and stirred to dissolve. After sufficient dissolution, 2.7 g of Ti3AlC2 powder was slowly added and stirred at 20 °C for 168 h. After the reaction, the mixture was centrifuged and washed with deionized water for 10 times. The centrifuged product was dispersed with deionized water. The dispersion was ultrasonically treated for 6 h and then freeze-dried to obtain Ti3C2MXene nanosheets.

[0032] (3) 96.7 μL of aniline, 32.9 mg of PSS, and MXene nanosheets were added to 80 ml of 0.5 M hydrochloric acid in sequence (the mass of MXene nanosheets was 5.0 wt% of aniline). The mixture was stirred vigorously at 2000 rpm for 1 h at room temperature. Then, ammonium persulfate solution (600 mg of ammonium persulfate dissolved in 5 ml of 0.5 M hydrochloric acid) was added dropwise to the mixture and quickly added to the prepared flexible substrate. The mixture was reacted at room temperature for 24 h. The flexible substrate on which the PANI:PSS / MXene composite sensitive material was deposited was taken out, washed with deionized water, and dried at room temperature. Thus, a flexible NH3 sensor based on PANI:PSS / MXene sensitive material was prepared.

[0033] (4) The prepared flexible NH3 sensor was connected to a CHI 760E electrochemical workstation and placed in an atmosphere of air and 1 ppm NH3 for current signal testing. The current change was converted into response change using mathematical methods, and the sensitivity of the sensor was calculated to be 0.42.

[0034] Example 3

[0035] (1) The flexible PET substrate was cut into pieces with a width of 10 mm and a length of 20 mm. The pieces were ultrasonically cleaned with deionized water, acetone, and ethanol at a frequency of 40 kHz. After drying, the substrate was treated with oxygen plasma for 10 min and set aside for use.

[0036] (2) 8 g of LiF was added to 100 ml of 8 M hydrochloric acid and stirred to dissolve. After sufficient dissolution, 4 g of Ti3AlC2 powder was slowly added and stirred at 40 °C for 48 h. After the reaction, the mixture was centrifuged and washed with deionized water for 8 times. The centrifuged product was dispersed with deionized water. The dispersion was ultrasonically treated for 2 h and then freeze-dried to obtain Ti3C2MXene nanosheets.

[0037] (3) 96.7 μL of aniline, 32.9 mg of PSS, and MXene nanosheets were added to 80 ml of 0.5 M hydrochloric acid in sequence (the mass of MXene nanosheets was 10 wt% of aniline). The mixture was stirred vigorously at 1000 rpm for 1 h at room temperature. Then, ammonium persulfate solution (314 mg of ammonium persulfate dissolved in 5 ml of 0.5 M hydrochloric acid) was added dropwise to the mixture and quickly added to the prepared flexible substrate. The mixture was reacted at room temperature for 12 h. The flexible substrate on which the PANI:PSS / MXene composite sensitive material was deposited was taken out, washed with deionized water, and dried at room temperature. Thus, a flexible NH3 sensor based on PANI:PSS / MXene sensitive material was prepared.

[0038] (4) The prepared flexible NH3 sensor was connected to a CHI 760E electrochemical workstation and placed in an atmosphere of air and 1 ppm NH3 for current signal testing. The current change was converted into response change using mathematical methods, and the sensitivity of the sensor was calculated to be 0.56.

[0039] Example 4

[0040] (1) The flexible PET substrate was cut into pieces with a width of 10 mm and a length of 20 mm. The pieces were ultrasonically cleaned with deionized water, acetone, and ethanol at a frequency of 40 kHz. After drying, the substrate was treated with oxygen plasma for 10 min and set aside for use.

[0041] (2) 8 g of LiF was added to 100 ml of 9 M hydrochloric acid and stirred to dissolve. After sufficient dissolution, 8 g of Ti3AlC2 powder was slowly added and stirred at 45 °C for 72 h. After the reaction was completed, the mixture was centrifuged and washed with deionized water for 8 times. The centrifuged product was dispersed with deionized water. The dispersion was ultrasonically treated for 2 h and then freeze-dried to obtain Ti3C2MXene nanosheets.

[0042] (3) 96.7 μL of aniline, 32.9 mg of PSS, and MXene nanosheets were added to 80 ml of 0.5 M hydrochloric acid in sequence (the mass of MXene nanosheets was 20 wt% of aniline). The mixture was stirred vigorously at 1200 rpm at room temperature for 1 h. Then, ammonium persulfate solution (314 mg of ammonium persulfate dissolved in 5 ml of 0.5 M hydrochloric acid) was added dropwise to the mixture and quickly added to the prepared flexible substrate. The mixture was reacted at room temperature for 12 h. The flexible substrate on which the PANI:PSS / MXene composite sensitive material was deposited was taken out, washed with deionized water, and dried at room temperature. Thus, a flexible NH3 sensor based on PANI:PSS / MXene sensitive material was prepared.

[0043] (4) The prepared flexible NH3 sensor was connected to a CHI 760E electrochemical workstation and placed in an atmosphere of air and 1 ppm NH3 for current signal testing. The current change was converted into response change using mathematical methods, and the sensitivity of the sensor was calculated to be 0.37.

[0044] Example 5

[0045] (1) The flexible PET substrate was cut into pieces with a width of 10 mm and a length of 20 mm. The pieces were ultrasonically cleaned with deionized water, acetone, and ethanol at a frequency of 40 kHz. After drying, the substrate was treated with oxygen plasma for 10 min and set aside for use.

[0046] (2) 8 g of LiF was added to 100 ml of 9 M hydrochloric acid and stirred to dissolve. After sufficient dissolution, 8 g of Ti3AlC2 powder was slowly added and stirred at 60 °C for 24 h. After the reaction was completed, the mixture was centrifuged and washed with deionized water for 9 times. The centrifuged product was dispersed with deionized water. The dispersion was ultrasonically treated for 2 h and then freeze-dried to obtain Ti3C2MXene nanosheets.

[0047] (3) 96.7 μL of aniline, 32.9 mg of PSS, and MXene nanosheets were added to 80 ml of 0.5 M hydrochloric acid in sequence (the mass of MXene nanosheets was 40 wt% of aniline), and the mixture was stirred vigorously at 1100 rpm at room temperature for 1 h. Then, ammonium persulfate solution (314 mg of ammonium persulfate dissolved in 5 ml of 0.5 M hydrochloric acid) was added dropwise to the mixture, and the prepared flexible substrate was quickly added to react at room temperature for 12 h. The flexible substrate with the PANI:PSS / MXene composite sensitive material deposited was taken out, washed with deionized water, and dried at room temperature. Thus, a flexible NH3 sensor based on PANI:PSS / MXene sensitive material was prepared.

[0048] (4) The prepared flexible NH3 sensor was connected to a CHI 760E electrochemical workstation and placed in an atmosphere of air and 1 ppm NH3 for current signal testing. The current change was converted into response change using mathematical methods, and the sensitivity of the sensor was calculated to be 0.34.

[0049] Comparative Example 1

[0050] (1) The flexible PET substrate was cut into pieces with a width of 10 mm and a length of 20 mm. The pieces were ultrasonically cleaned with deionized water, acetone, and ethanol at a frequency of 50 kHz. After drying, the substrate was treated with oxygen plasma for 10 min and set aside for use.

[0051] (2) 96.7 μL of aniline and 32.9 mg of PSS were added to 80 ml of 0.5 M hydrochloric acid in sequence and stirred vigorously at 1000 rpm at room temperature for 1 h. Then, ammonium persulfate solution (314 mg of ammonium persulfate dissolved in 5 ml of 0.5 M hydrochloric acid) was added dropwise to the mixture and quickly added to the prepared flexible substrate. The mixture was reacted at room temperature for 12 h. The flexible substrate on which the PANI:PSS composite sensitive material was deposited was taken out, washed with deionized water and dried at room temperature. Thus, a flexible NH3 sensor based on PANI:PSS sensitive material was prepared.

[0052] (3) The prepared flexible NH3 sensor was connected to a CHI 760E electrochemical workstation and placed in an atmosphere of air and 1 ppm NH3 for current signal testing. The current change was converted into response change using mathematical methods, and the sensitivity of the sensor was calculated to be 0.28.

Claims

1. A water-soluble polyaniline / MXene composite flexible ammonia sensor, characterized in that: The ammonia sensor is composed of a polymer flexible substrate and a PANI:PSS / MXene composite film deposited on the substrate, wherein: The polyaniline / MXene composite flexible ammonia sensor is prepared according to the following method: 30 to 150 μL of aniline, PSS, and MXene nanosheets are sequentially added to 80 ml of 0.5 M hydrochloric acid, wherein the mass ratio of PSS to aniline is 1:1 to 1:9, and the mass of MXene nanosheets is 2.0 to 40 wt % of aniline, and stirred at 900 to 2000 rpm for 1 h at room temperature to obtain a mixed solution; ammonium persulfate solution is added dropwise to the mixed solution, and a polymer flexible substrate is quickly added to react at room temperature for 8 to 24 h; the flexible substrate with the PANI:PSS / MXene composite film deposited is taken out, washed with deionized water, and dried at room temperature to obtain a mixed solution, wherein the ammonium persulfate solution is prepared by dissolving 200 to 600 mg of ammonium persulfate in 5 ml of 0.5 M hydrochloric acid.

2. The sensor according to claim 1, characterized in that: The MXene nanosheets are prepared by the following method: adding 8 g of LiF to 100 ml of 6-9 M hydrochloric acid and stirring to dissolve; after sufficient dissolution, slowly adding a MAX powder of Ti3AlC2, Ti2AlC, Ti4AlN3, Ti2AlN, Nb4AlC3, Nb2AlC, V2AlC, Ta2AlC, Mo2TiAlC2, Mo2Ti2AlC3, and MoYAlC, stirring and reacting at 20-60° C. for 24-168 h, wherein the mass ratio of MAX powder to LiF is 1:1-1:3; after the reaction is completed, centrifuging and washing with deionized water are repeated 5-10 times, the centrifuged product is dispersed with deionized water, the dispersion is ultrasonically treated for 1-6 h, and then freeze-dried to obtain MXene nanosheets.

3. The sensor according to claim 1, characterized in that: The polymer flexible substrate is a PET, PI or PDMS substrate.

4. The sensor according to claim 3, characterized in that: The flexible PET, PI or PDMS substrate was cut into pieces with a width of 5 to 15 mm and a length of 5 to 20 mm, and ultrasonically washed with deionized water, acetone, and ethanol at an ultrasonic frequency of 25 to 80 KHZ. After drying, the substrate was treated with oxygen plasma for 5 to 30 min.

5. A method for preparing a water-soluble polyaniline / MXene composite flexible ammonia sensor, characterized in that: The process includes the following steps: (1) Cut the flexible PET, PI or PDMS substrate into pieces with a width of 5 to 15 mm and a length of 5 to 20 mm, and wash them with deionized water, acetone, and ethanol ultrasonically at a frequency of 25 to 80 KHZ. After drying, treat the substrate with oxygen plasma for 5 to 30 min and set aside for use; (2) Add 8 g of LiF to 100 ml of 6-9 M hydrochloric acid and stir to dissolve; after sufficient dissolution, slowly add one MAX powder selected from Ti3AlC2, Ti2AlC, Ti4AlN3, Ti2AlN, Nb4AlC3, Nb2AlC, V2AlC, Ta2AlC, Mo2TiAlC2, Mo2Ti2AlC3, and MoYAlC, and stir to react at 20-60 °C for 24-168 h. The mass ratio of MAX powder to LiF is 1:1-1:

3. After the reaction, centrifuge and wash with deionized water for 5-10 times. The centrifuged product is dispersed with deionized water. The dispersion is ultrasonically treated for 1-6 h and then freeze-dried to obtain MXene nanosheets. (3) 30-150 μL of aniline, PSS, and MXene nanosheets were added to 80 ml of 0.5 M hydrochloric acid in sequence, wherein the mass ratio of PSS to aniline was 1:1-1:9, and the mass of MXene nanosheets was 2.0-40 wt% of aniline. The mixture was stirred at 900-2000 rpm for 1 h at room temperature to obtain a mixed solution. Ammonium persulfate solution was added dropwise to the mixed solution, and the polymer flexible substrate was quickly added to react at room temperature for 8-24 h. The flexible substrate with the PANI:PSS / MXene composite film deposited was taken out, washed with deionized water, and dried at room temperature to obtain a mixed solution. The ammonium persulfate solution was prepared by dissolving 200-600 mg of ammonium persulfate in 5 ml of 0.5 M hydrochloric acid.