A catalyst for catalyzing aromatization of light gasoline and preparation method thereof
By using alumina and stepped-pore ZSM-5 molecular sieve composite carriers and low-temperature phosphating technology, the problems of difficulty in preparing nano-ZSM-5 molecular sieves, high cost of precious metals and insufficient preparation of Ni2P catalysts have been solved, and efficient, sulfur-tolerant light gasoline has been achieved. Aromatization catalyst suitable for industrial applications.
Patent Information
- Application Number
- CN202010781382.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-06
AI Technical Summary
It is difficult to prepare nanometer ZSM-5 molecular sieves in existing light gasoline aromatization catalysts. The cost of precious metals is high and the sulfur resistance is poor. The preparation technology of supported highly dispersed Ni2P catalysts has difficulties in temperature control and reactor clogging problems.
A composite carrier composed of alumina and stepped pore ZSM-5 molecular sieve is used. Ni2+ species are impregnated at low temperature and phosphated outside the device to avoid high-temperature roasting and decomposition of organic phosphating agents, ensuring high dispersion and pure phase transformation of Ni2P.
It achieves high-efficiency aromatization performance of the catalyst, reduces costs and risks of sulfur poisoning, avoids reactor blockage and pore residual problems, and is suitable for industrial production.
Abstract
Description
Technical Field
[0001] The invention relates to the field of aromatization catalysts, and in particular to a catalyst for catalyzing aromatization of light gasoline and a preparation method thereof. Background Art
[0002] FCC gasoline accounts for about 65% of the gasoline pool in my country, and the content of sulfur and olefins is relatively high. The gasoline quality upgrade of the VIA / B stage in China limits the olefin content to no more than 18 / 15v% on the basis of maintaining the sulfur content of 10mg / kg. According to the requirement of the US gasoline quality standard that limits olefins to no more than 10v%, it is speculated that the trend of gasoline quality upgrade in the future is to continue to reduce the olefin content and reduce the octane loss. At present, the FCC gasoline cleaning technology that can simultaneously achieve deep desulfurization, significantly reduce olefins and reduce octane loss is hydrogenation reforming technology, such as GARDES-II technology, MPHG-II technology and PHG-M technology. The common feature of this technology is that the full-fraction gasoline needs to be cut into light gasoline fraction and heavy gasoline fraction first, and the light gasoline fraction and heavy gasoline fraction are etherified and hydrogenated respectively. Finally, the etherified light gasoline fraction and the heavy gasoline fraction after hydrogenation reforming are blended to obtain a blending component that meets the current gasoline quality standards. However, with the implementation of ethanol standard gasoline (E10) in the future, refineries will switch from producing motor gasoline to producing ethanol gasoline blending components, and the light gasoline etherification unit will not be able to perform the task of reducing olefins and restoring octane number of gasoline.
[0003] Light gasoline aromatization can undertake the task of reducing olefins and restoring octane number of gasoline in the future because it can convert olefins in FCC light gasoline into high-octane aromatics. Among aromatization catalysts, ZSM-5 molecular sieves are widely used, and the main problems are low gasoline yield and poor catalyst stability. At present, the aromatization selectivity and stability of ZSM-5 molecular sieve catalysts are mainly improved by optimizing the mass transfer efficiency of ZSM-5 molecular sieves and modifying the metal surface. CN201410628681.6 provides a method for preparing a catalytic cracking light gasoline aromatization catalyst; the preparation method of the catalyst mainly includes modification of nano ZSM-5 molecular sieves, preparation of carriers, preparation of catalysts, etc. The nano ZSM-5 molecular sieve has short pores and high mass transfer efficiency. After surface modification by rare earth or one or two metals of cobalt, molybdenum, nickel, gallium, and zinc, the low-carbon olefins in catalytic cracking light gasoline can be reduced to the maximum extent and the octane number can be guaranteed not to be reduced or even increased. However, due to the small crystal size of the nano ZSM-5 molecular sieve, it is difficult to separate during the preparation process, which is not conducive to industrial production. CN 02133112.X provides a catalytic gasoline aromatization catalyst and its application process. Based on the weight percentage of the catalyst, the composition is: the content of precious metals is 0.1m% to 1.0m%; the content of K-type zeolite is 50.0m% to 90.0m%; the content of K2O is 1.0m% to 5.0m%; the balance is a binder. The catalyst aromatizes the catalytic gasoline after hydrodesulfurization, which can achieve the purpose of reducing the olefin content and reducing the octane number loss, but contains precious metals such as platinum and palladium, which increases the catalyst cost and is prone to sulfur poisoning.
[0004] A large number of research results show that supported highly dispersed nickel phosphide (Ni2P) catalysts not only have similar properties to precious metal "platinum" such as hydrorefining, dehydrogenation, and hydroisomerization, but are also cheap and have good sulfur resistance. At present, the preparation method of supported highly dispersed Ni2P catalysts with the most promising industrial application prospects is to use hypophosphite (H2PO2 - ), the reduction reaction between phosphine (PH3) and divalent nickel ions. CN200810234685.0 through H2PO2 - and Ni 2+ The solid phase reaction was carried out at a relatively low temperature to obtain a supported Ni2P catalyst with high active component dispersion and good catalytic activity. - When heated, it undergoes disproportionation reaction to generate PH3, P, PO3 2- PO4 3- , low-cost PH3 and Ni 2+ A reduction reaction occurs to generate Ni2P, but the reaction temperature is too high, H2PO2 - The disproportionation reaction is very fast, and the generated PH3 does not have time to react with Ni 2+reaction, it is possible to generate some nickel phosphates (such as NiP4O 11 ); Residual PO3 2- PO4 3- Species such as nickel and tantalum will occupy part of the pores of the catalyst. CN201510232332.7 discloses a supported Ni2P catalyst and a phosphating preparation method thereof, wherein the supported Ni2P catalyst is prepared by first loading a nickel salt on a carrier to obtain supported nickel oxide, and then phosphating the supported nickel oxide catalyst in a reactor to convert the nickel oxide into Ni2P in situ. The prepared catalyst has a high Ni2P loading, good dispersion, high purity, and good hydrogenation performance. However, the valence state and aggregation of the supported nickel oxide in the invention are not well controlled. During the phosphating process, it is not easy to convert all the nickel oxide species into pure phase Ni2P, and the organic phosphating agent used will produce elemental P during the thermal decomposition process in the device, resulting in blockage of the reactor system. Summary of the invention
[0005] In view of the problems that the nano ZSM-5 molecular sieve used in the above-mentioned light gasoline aromatization catalyst is not conducive to industrial production due to its small grain size, the precious metals used are expensive and have poor sulfur resistance, and the preparation technology of supported highly dispersed Ni2P catalyst is insufficient, the purpose of the present invention is to provide a Ni2P catalyst for catalyzing the aromatization of light gasoline and a preparation method thereof, the carrier of the catalyst is a composite carrier composed of alumina and stepped pore ZSM-5 molecular sieve, and the active metal component of the catalyst is Ni2P.
[0006] The step-pore ZSM-5 molecular sieve used in the present invention not only has good diffusion and mass transfer performance, but also avoids the problem that the nano ZSM-5 molecular sieve is difficult to separate and unfavorable for industrial production due to small crystal grains. Preferably, in the composite carrier composed of the step-pore ZSM-5 molecular sieve and alumina, the content of the step-pore ZSM-5 molecular sieve is 60-80wt%, the content of alumina is 20-40wt%, and the more preferred dry basis mass ratio of the step-pore ZSM-5 molecular sieve to alumina is 3.0-4.0.
[0007] The Ni2P used in the present invention not only has the hydrogenation / dehydrogenation performance similar to "platinum", but also is cheap and has good sulfur resistance. According to the scheme of the present invention, it is preferred that the content of Ni2P in the catalyst is 0.2-20.0wt% in terms of NiO based on the total weight of the catalyst.
[0008] The present invention will contain Ni 2+ After the impregnation solution of the species is impregnated into the above composite support, it is preferred that high-dispersion Ni 2+ Species, this is Ni 2+ The complete phosphating of species laid the foundation for highly dispersed Ni2P.
[0009] The present invention is highly dispersed Ni 2+ During the phosphating process of species, the PH3 generated outside the device by organic or inorganic phosphating agents is used to treat highly dispersed Ni 2+ The species undergoes phosphation reaction and is completely converted into highly dispersed pure phase Ni2P, which avoids the problem of organic phosphine clogging the reactor system due to the production of elemental P during the decomposition process in the reactor and the residual PO3 in the catalyst pores during the decomposition of hypophosphite. 2- PO4 3- The problem of species.
[0010] The present invention also aims to provide a method for preparing a catalyst for catalyzing aromatization of light gasoline, the method mainly comprising the following steps:
[0011] (1) Preparation of alumina and stepped pore ZSM-5 molecular sieve composite carrier
[0012] The step-pore ZSM-5 molecular sieve is mixed with alumina raw powder, and an extrusion aid and a peptizing solvent aqueous solution are added respectively. After kneading, molding, drying and calcining, an alumina and step-pore ZSM-5 molecular sieve composite carrier is obtained.
[0013] (2) Alumina and step-pore ZSM-5 molecular sieve composite carrier loaded with highly dispersed Ni 2+ Species
[0014] According to the water absorption rate of the composite carrier and the Ni 2+ Species metal content, configure Ni containing suitable concentration 2+ The impregnation solution of the species is impregnated into the carrier, and after aging and drying, high-temperature calcination is not required to directly obtain a highly dispersed Ni on the carrier of the composite carrier of alumina and stepped pore ZSM-5 molecular sieve. 2+ Species.
[0015] (3) Preparation of highly dispersed Ni2P catalyst
[0016] The above-mentioned highly dispersed Ni 2+ The alumina and stepped pore ZSM-5 molecular sieve composite carrier of the species is placed in a fixed bed reactor, and phosphating reaction is carried out under hydrogen conditions by using PH3 produced outside the reactor by an organic phosphating agent or an inorganic phosphating agent, and finally a catalyst for catalyzing aromatization of light gasoline is obtained.
[0017] Preferably, in step (1), the average pore size, BET specific surface area, and silicon / aluminum atomic ratio of the step-pore ZSM-5 molecular sieve are 2-20 nm, 300-500 m 2 / g, 5:1-100:1;
[0018] In step (1), preferably, the alumina raw powder can be a commonly used aluminum source, such as pseudo-boehmite powder, aluminum hydroxide powder, SB powder, etc.;
[0019] In step (1), preferably, during the molding process, the dry weight ratio of the stepped pore ZSM-5 molecular sieve to alumina can be controlled to be 3.0-3.7:1; based on the total dry weight of the catalyst carrier, the weight contents of the extrusion aid and the peptizer are 6-8wt% and 3-4wt%, respectively; the extrusion aid can be sesbania powder, polyacrylamide, graphite, lubricating oil, etc., and the peptizer can be nitric acid, hydrochloric acid, acetic acid, citric acid, etc.;
[0020] In step (1), preferably, after drying at 120-150° C. for about 3-5 hours and calcining at 500-550° C. for about 3-5 hours, a composite carrier of alumina and stepped pore ZSM-5 molecular sieve is obtained;
[0021] In step (2), preferably, the Ni 2+ The impregnation solution of the species is configured by using one or more of nickel sulfate, nickel ammonium sulfate, nickel chloride, nickel bromide, nickel iodide, nickel carbonate, nickel acetate, basic nickel carbonate, nickel oxalate, nickel formate, nickel acetylacetonate, etc.;
[0022] Preferably, in step (2), the Ni-containing +2 Species infusions;
[0023] In step (2), after impregnation, the mixture is aged at room temperature for about 6-8 hours, and dried at 90-120°C for about 4-6 hours to obtain a highly dispersed Ni +2 Species;
[0024] In step (3), the organic phosphorus activating agent preferably comprises one or more of triethyl phosphine, tripropyl phosphine, tributyl phosphine, triisopropyl phosphine, di-tert-butyl phosphine, triphenyl phosphine, trioctyl phosphine, tri-p-tolyl phosphine, diphenylmethyl phosphine, etc.;
[0025] In step (3), the inorganic phosphating agent preferably comprises one or more of hypophosphorous acid, sodium hypophosphite, ammonium hypophosphite, nickel hypophosphite, etc.;
[0026] In step (3), preferably, the concentration of phosphine in hydrogen is 10000-20000 ppm; the hydrogen volume space velocity is 1.0-3.0h -1 ; Phosphating temperature 150-400℃; Phosphating time 12-48h; Phosphating pressure 0.1-1.0MPa.
[0027] Compared with the prior art, the catalyst for catalyzing aromatization of light gasoline and the preparation method thereof provided by the present invention have the following characteristics:
[0028] (1) The step-pore ZSM-5 molecular sieve used in the catalyst not only has good diffusion and mass transfer performance, but also avoids the problem of separation difficulty and disadvantageous industrial production caused by the small crystal size of nano ZSM-5 molecular sieve;
[0029] (2) The Ni2P used in the catalyst not only has “platinum-like” hydrogenation / dehydrogenation performance, but is also cheap and has good sulfur resistance;
[0030] (3) Preparation of catalyst First, Ni-containing 2+ After the impregnation solution of the species is impregnated into the above composite carrier, high-dispersion Ni 2+ Species, and then the PH3 generated outside the device by organic or inorganic phosphating agent is used to treat the highly dispersed Ni 2+ The species undergoes phosphation reaction, which completely converts them into highly dispersed pure phase Ni2P, avoiding the problem of organic phosphine clogging the reactor system due to the production of elemental P during the decomposition process in the reactor and the residual PO3 in the catalyst pores during the decomposition of hypophosphite. 2- PO4 3- The problem of species. DETAILED DESCRIPTION
[0031] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0032] Example 1
[0033] Catalyst A prepared in this example contains, based on the weight of the catalyst, 5.0 wt% NiO, 74.4 wt% mesoporous-macroporous ZSM-5 molecular sieve, and 20.6 wt% alumina.
[0034] Weigh 375 g of the above-mentioned stepped pore ZSM-5 molecular sieve (self-made, with a specific surface area of 344 m 2 / g, average pore size 3.5nm, silicon / aluminum atomic ratio 20:1), 150g of pseudo-boehmite powder HC-07 (produced by Shandong Xingdu Chemical Co., Ltd., the prepared alumina loses about 30wt% of water), and 32.5g of field sesbania powder are mixed evenly, and then 16.9g of concentrated nitric acid (65wt%) and 180g of deionized water are added. After sufficient kneading, the strips are extruded into 1.7mm clover-shaped strips in an extruder, dried at 120°C for about 4 hours, calcined at 550°C for about 4 hours, cooled, cut into strips, and sieved to obtain 450g of a 3-10mm long alumina and stepped pore ZSM-5 molecular sieve composite carrier.
[0035] Then, according to the water absorption rate of the carrier (42wt%), the content of the target catalyst NiO (5.0wt%), and the amount of the carrier used, an aqueous solution containing 62.45g of nickel sulfate was prepared, and an equal volume of the aqueous solution was impregnated on 450g of the composite carrier. After aging at room temperature for about 8 hours and drying at 120°C for about 4 hours, the highly dispersed NiO supported on the composite carrier of alumina and the stepped pore ZSM-5 molecular sieve was +2 Species.
[0036] The high-density Ni +2 The species were placed in a fixed bed reactor, and the PH3 produced by sodium hypophosphite outside the reactor was used. The concentration of phosphine in hydrogen was 12000ppm, the phosphating temperature was 300℃, the phosphating pressure was 0.5MPa, and the hydrogen volume space velocity was 2.0h -1 Under the conditions of , after phosphating for 24 hours, a Ni2P catalyst A for catalyzing the aromatization of light gasoline was obtained.
[0037] Example 2
[0038] The catalyst prepared in this example is B, and its preparation steps are the same as those in Example 1, except that the content of Ni2P in the catalyst is: based on the weight of the catalyst, NiO 1.0wt%, 75.8wt% step pore ZSM-5 molecular sieve, and 23.2wt% alumina.
[0039] Example 3
[0040] The catalyst prepared in this example is C, and its preparation steps are the same as those in Example 1, except that the content of Ni2P in the catalyst is: based on the weight of the catalyst, NiO 10.0wt%, 69.6wt% step pore ZSM-5 molecular sieve, and 30.4wt% alumina.
[0041] Example 4
[0042] The catalyst prepared in this example is D, and its preparation steps are the same as those in Example 1, except that the phosphating agent used is ammonium hypophosphite.
[0043] Example 5
[0044] The catalyst prepared in this example is E, and its preparation steps are the same as those in Example 1, except that the phosphating agent used is triphenylphosphine.
[0045] Example 6
[0046] The catalyst prepared in this example is F, and its preparation steps are the same as those in Example 1, except that nickel chloride is used to prepare the Ni +2 Species infusion.
[0047] Example 7
[0048] The catalyst prepared in this example is G, and its preparation steps are the same as those in Example 1, except that the phosphating pressure is 0.2 MPa.
[0049] Example 8
[0050] The catalyst prepared in this embodiment is H. The preparation steps thereof are different from those in Example 1 in that after the impregnation solution is impregnated into the carrier, it is calcined at 550°C for 6 hours to obtain a multivalent Ni supported on a composite carrier of alumina and a stepped pore ZSM-5 molecular sieve. x+ Species.
[0051] Example 9
[0052] In this example, catalytic light gasoline of a certain factory with a temperature below 70° C. was used as a raw material (the contents of saturated hydrocarbons, aromatic hydrocarbons and olefins were 40.5 v%, 0.2 v% and 59.3 v% respectively), and the aromatization performance of catalysts A, B, C, D, E, F, G and H of the present invention on FCC light gasoline was evaluated in a small fixed bed reactor.
[0053] The precursors of the above catalysts were respectively loaded into a small fixed bed reactor, with the catalyst loading being 10 mL. After the reactor was found to be airtight, in-situ phosphating was performed according to the phosphating procedure described in the implementation.
[0054] After phosphating, switch to FCC light gasoline for replacement for 2h, reduce the reaction pressure to 0.1MPa, increase the reaction temperature to 400℃, and maintain the volume space velocity for 3.0h -1 , the hydrogen / oil volume ratio was adjusted to 250, and samples were taken for analysis after 72 hours of reaction.
[0055] Table 1 is the aromatization reaction data of FCC light gasoline over the catalysts A, B, C, D, E, F, G, and H of the present invention. + The conversion rate of olefins is 61.3-66.0v%, the increase of aromatics is 7.3-11.2v%, and the product C5 + The liquid yield is 83.2-88.7% by volume, which indicates that FCC light gasoline can be effectively aromatized over the catalyst of the present invention.
[0056] Table 1 Aromatization reaction data of the catalyst of the present invention on FCC light gasoline
[0057] Catalyst of the present invention X, v% <![CDATA[ΔC ar about, in%]]> Y, wt% A 65.4 10.5 85.4 B 63.9 9.6 83.2 C 61.3 7.3 88.7 D 66.5 11.2 86.3 E 65.4 10.7 85.4 F 63.7 11.0 86.0 G 65.9 10.7 85.8 H 66.0 11.0 86.0
[0058] In Table 1: X is C5 + Olefin conversion; ΔC aro is the aromatics increment; Y is the product C5 + Liquid yield.
[0059] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. Use of a catalyst in catalytic aromatization of light gasoline, characterized in that: The catalyst carrier is a composite carrier composed of alumina and stepped pore ZSM-5 molecular sieve, and the active metal component of the catalyst is Ni2P; The average pore size, BET specific surface area, and silicon / aluminum atomic ratio of the step-pore ZSM-5 molecular sieve are 2-20 nm, 300-500 nm, respectively. 2 / g, 5:1-100:1; The preparation method of the catalyst comprises the following steps: (1) Preparation of complex carrier The step-pore ZSM-5 molecular sieve is mixed with alumina raw powder, an extrusion aid and a peptizing solvent aqueous solution are added, and after kneading, molding, drying and calcining, a composite carrier is obtained; (2) Composite carrier loaded with highly dispersed Ni 2+ Species Configuration containing Ni 2+ The impregnation solution of the species is impregnated into the composite carrier, and after aging and drying, high-dispersed Ni is directly obtained without high-temperature calcination. 2+ Species complex carrier; (3) Preparation of Catalyst Highly dispersed Ni 2+ The composite carrier of the species is placed in a fixed bed reactor, and PH3 generated outside the reactor by an organic phosphating agent or an inorganic phosphating agent is used to carry out a phosphating reaction under hydrogen conditions to finally obtain the catalyst.
2. The use according to claim 1, characterized in that: In the composite carrier, the content of the stepped pore ZSM-5 molecular sieve is 60-80wt%, and the content of alumina is 20-40wt%.
3. The use according to claim 2, characterized in that: In the composite carrier, the dry basis mass ratio of the stepped pore ZSM-5 molecular sieve to alumina is 3.0-4.
0.
4. The use according to claim 1, characterized in that: The content of Ni2P in the catalyst is 0.2-20.0 wt% in terms of NiO based on the total weight of the catalyst.
5. The use according to claim 1, characterized in that: The Ni-containing 2+ The impregnation solution of the species is at least one of nickel sulfate, nickel ammonium sulfate, nickel chloride, nickel bromide, nickel iodide, nickel carbonate, nickel acetate, basic nickel carbonate, nickel oxalate, nickel formate, and nickel acetylacetonate.
6. The use according to claim 1, characterized in that: The organic phosphating agent includes at least one of triethyl phosphine, tripropyl phosphine, tributyl phosphine, triisopropyl phosphine, di-tert-butyl phosphine, triphenyl phosphine, trioctyl phosphine, tri-p-tolyl phosphine and diphenylmethyl phosphine.
7. The use according to claim 1, characterized in that: The inorganic phosphating agent includes at least one of hypophosphorous acid, sodium hypophosphite, ammonium hypophosphite, and nickel hypophosphite.
8. The use according to claim 1, characterized in that: The conditions of the phosphating reaction are: the concentration of phosphine in hydrogen is 10000-20000ppm, the volume space velocity of hydrogen is 1.0-3.0h -1 , phosphating temperature 150-400℃, phosphating time 12-48h, phosphating pressure 0.1-1.0MPa.
Citation Information
Patent Citations
Preparation method of nickel phosphide
CN101734633A
Preparation method of catalyst for light gasoline catalytic cracking and aromatization
CN104399518A
Load type nickel phosphide catalyst and pre-phosphating preparation method thereof
CN104841465A
Aromatization catalyst for catalytic gasoline and its use
CN1488728A
Method for controllably preparing supported and non-supported Ni2P under mild conditions
CN102030317A