Electrostatic capacitance input device and manufacturing method thereof, and image display device

A photosensitive film with a photocurable resin layer addresses the challenges of forming a white decorative layer on capacitive touch panels, achieving desired properties with improved yield and reducing device thickness and weight.

CN114089600BActive Publication Date: 2024-12-03FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111494949.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2012-03-15
Filing Date
2013-03-12
Publication Date
2024-12-03
Estimated Expiration
2033-03-12

AI Technical Summary

Technical Problem

Existing methods for forming a white decorative layer on capacitive touch panels using liquid resist coating or screen printing result in bubbles, unevenness, and reduced yield, making it difficult to achieve desired characteristics of brightness, whiteness, network structure, adhesion, and development residue, while also increasing thickness and weight.

Method used

A photosensitive film comprising a temporary support and a photocurable resin layer with specific compositions and thicknesses, allowing for the formation of a white decorative layer with improved properties through a simpler process.

Benefits of technology

The photosensitive film enables the production of a thin, lightweight capacitive input device with a high-yield white decorative layer that meets brightness, whiteness, network structure, adhesion, and development residue requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114089600B_ABST
    Figure CN114089600B_ABST
Patent Text Reader

Abstract

The present invention provides an electrostatic capacitive input device and a manufacturing method thereof, and an image display device. The manufacturing method of the electrostatic capacitive input device uses a photosensitive film, and the photosensitive film has a temporary support and a photocurable resin layer. The photocurable resin layer contains at least (A) a white inorganic pigment, (B) a monomer, (C) an adhesive, and (D) a photopolymerization initiator. The thickness of the photocurable resin layer is 1 μm to 40 μm, and the content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is 20% to 75% by mass. According to the photosensitive film, a white decorative layer with good brightness, whiteness, network structure, adhesion, development residue, and unevenness can be obtained with a high yield.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the application filed by the applicant with application number 201380014203.X, international publication number WO2013 / 137226A1, and invention name “Photosensitive film, method for manufacturing electrostatic capacitive input device, electrostatic capacitive input device, and image display device having the same”. The filing date of the parent case of this application is March 12, 2013, and the earliest priority date is March 15, 2012. Technical Field

[0002] The present invention relates to a decorative photosensitive film for manufacturing a capacitive input device capable of detecting the contact position of a finger by changes in electrostatic capacitance, a method for manufacturing a capacitive input device, a capacitive input device obtained by the manufacturing method, and an image display device having the capacitive input device as a constituent element. Background Art

[0003] In recent years, electronic devices such as mobile phones, car navigation systems, personal computers, ticket machines, and bank terminals have included devices that have a panel-type input device on the surface of a liquid crystal device, etc., which can input information corresponding to the indication image by touching the portion where the indication image is displayed with a finger or a touch pen while referring to the indication image displayed in the image display area of ​​the liquid crystal device.

[0004] Such input devices (touch panels) include resistive film type, electrostatic capacitance type, etc. However, resistive film type input devices have a narrow operating temperature range and are weak to time-dependent changes because they have a two-layer structure of film and glass and a structure in which the film is pressed to short-circuit.

[0005] In contrast, an electrostatic capacitance type input device has the advantage that a light-transmitting conductive film can be formed on only one substrate. Among the electrostatic capacitance type input devices, there are devices of the following type, for example, in which electrode patterns are extended in mutually intersecting directions, and when a finger or the like touches, the change in electrostatic capacitance between the electrodes is detected to detect the input position (for example, refer to the following patent document 1).

[0006] In addition, as an electrostatic capacitance type input device, there is also a device of the following type: when an alternating current of the same phase and the same potential is applied to both ends of a light-transmitting conductive film, a weak current flowing when a capacitor is formed by detecting finger contact or proximity is detected, and the input position is detected. As such an electrostatic capacitance type input device, the following electrostatic capacitance type input device is disclosed, which comprises: a plurality of first transparent electrode patterns, a plurality of pad portions are extended in a first direction via a connecting portion to form; a plurality of second transparent electrode patterns are electrically insulated from the first transparent electrode pattern via an interlayer insulating layer, and are composed of a plurality of pad portions formed by extending in a direction intersecting the first direction (for example, refer to the following patent document 2). However, since the front panel is stacked on the manufactured electrostatic capacitance type input device, the electrostatic capacitance type input device becomes thicker and heavier.

[0007] Furthermore, a capacitive touch panel is disclosed in which a mask layer, a readout circuit, and an interlayer insulating layer are integrally formed on the non-contact side surface of a front panel (for example, see Patent Document 3 below). In Patent Document 3, since the front panel and the capacitive input device are integrated, the capacitive touch panel can be thinned / lightened, and a decorative layer of various tones (black, white, light colors, metallic colors, etc.) can be provided between the mask layer and the front panel as required, and it is particularly required to improve the brightness and whiteness of the white decorative layer.

[0008] Currently, the mainstream method for providing the decorative layer is to use liquid resist coating, screen printing, or the like.

[0009] On the other hand, in smartphones and tablets having a capacitive touch panel on a liquid crystal or organic EL display, a structure using tempered glass such as Corning's Gorilla Glass on the front panel (the surface directly touched by a finger) has been developed and announced.

[0010] If a white decorative layer is to be formed on the substrate using a decorative layer-forming liquid resist or screen printing ink, the liquid resist coating and screen printing must be performed several times in order to form the white decorative layer using a liquid resist or screen printing ink with low hiding power. This may cause bubbles and unevenness, and may reduce the yield due to the large number of steps, making it difficult to reduce costs.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Publication No. 2007-122326

[0014] Patent Document 2: Japanese Patent No. 4506785

[0015] Patent Document 3: Japanese Patent Application Publication No. 2009-193587 Summary of the invention

[0016] Problems to be solved by the invention

[0017] The present inventors have conducted studies and found that when a white decorative layer is formed by the method described in the above document, a white decorative layer having performance satisfying all characteristics of brightness, whiteness, network structure, adhesion, development residue, and unevenness cannot be obtained.

[0018] It is also found that it is difficult to obtain a white decorative layer satisfying the above-mentioned properties with a high yield.

[0019] The problem to be solved by the present invention is to provide a photosensitive film capable of obtaining a white decorative layer having good brightness, whiteness, network structure, adhesion, development residue and unevenness at a high yield.

[0020] Accordingly, the object of the present invention is to provide a method for manufacturing an electrostatic capacitive input device that can manufacture an electrostatic capacitive input device that uses a photosensitive film that satisfies the above-mentioned characteristics and can be thinned / lightened with a simple process and of high quality, as well as an electrostatic capacitive input device obtained by the manufacturing method and an image display device using the electrostatic capacitive input device.

[0021] Solutions to the problem

[0022] [1] A photosensitive film comprising a temporary support and a photocurable resin layer, wherein:

[0023] The photocurable resin layer contains at least (A) a white inorganic pigment, (B) a monomer, (C) a binder, and (D) a photopolymerization initiator. The thickness of the photocurable resin layer is 1 to 40 μm, and the content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is 20 to 75% by mass.

[0024] [2] The photosensitive film according to [1], wherein the white inorganic pigment is preferably rutile titanium oxide.

[0025] [3] The photosensitive film according to [1] or [2], wherein the content ratio B / C of the solid content of the (B) monomer to the solid content of the (C) binder is preferably 0.4 or more.

[0026] [4] The photosensitive film according to any one of [1] to [3], preferably comprising a thermoplastic resin layer between the temporary support and the photocurable resin layer.

[0027] [5] A method for manufacturing a capacitive input device,

[0028] The electrostatic capacitance input device comprises a front panel and at least the following elements (1) and (3) to (5) on the non-contact side of the front panel.

[0029] (1) Decorative layer;

[0030] (3) a plurality of first transparent electrode patterns, which are formed by a plurality of pad portions extending in a first direction via a connecting portion;

[0031] (4) a plurality of second electrode patterns, which are electrically insulated from the first transparent electrode patterns and include a plurality of pad portions extending in a direction intersecting the first direction;

[0032] (5) an insulating layer that electrically insulates the first transparent electrode pattern from the second electrode pattern,

[0033] The manufacturing method comprises:

[0034] A step of transferring the colored layer of the photosensitive film according to any one of [1] to [4] to the non-contact side of the front plate to form at least the following (1) decorative layer.

[0035] [6] The method for manufacturing a capacitive input device according to [5], wherein the capacitive input device preferably further comprises:

[0036] (6) Another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern.

[0037] [7] The method for manufacturing an electrostatic capacitive input device as described in [5] or [6], wherein the second electrode pattern is preferably a transparent electrode pattern.

[0038] [8] The method for manufacturing an electrostatic capacitive input device as described in any one of [5] to [7], wherein preferably, (2) a mask layer is further provided on the surface of the (1) decorative layer opposite to the front panel.

[0039] [9] A method for manufacturing an electrostatic capacitive input device as described in [8], wherein at least one of the first transparent electrode pattern and the second electrode pattern is preferably provided so as to cover two areas, namely, a non-contact surface of the front panel and a surface of the mask layer opposite to the front panel.

[0040]

[10] The method for manufacturing a capacitive input device according to [8] or [9], wherein the capacitive input device preferably further comprises:

[0041] (6) another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern,

[0042] And the (6) other conductive element is at least arranged on the surface side of the mask layer opposite to the front panel.

[0043]

[11] The method for manufacturing an electrostatic capacitive input device as described in any one of [5] to

[10] , wherein a transparent protective layer is preferably further provided in a manner covering all or part of the elements (1) and (3) to (5).

[0044]

[12] The method for manufacturing a capacitive input device according to

[11] , wherein:

[0045] The transparent protective layer is preferably formed using a photosensitive film having a temporary support, a thermoplastic resin layer, and a photocurable resin layer in this order.

[0046]

[13] The method for manufacturing a capacitive input device according to any one of [5] to

[12] , wherein the capacitive input device preferably further comprises:

[0047] (6) another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern,

[0048] The second electrode pattern is a transparent electrode pattern,

[0049] The transparent conductive material is etched using an etching pattern formed by a photosensitive film having a temporary support, a thermoplastic resin layer, and a photocurable resin layer in sequence to form at least one of the first transparent electrode pattern, the second transparent electrode pattern, and the conductive element.

[0050]

[14] The method for manufacturing a capacitive input device according to any one of [5] to

[13] , wherein the capacitive input device preferably further comprises:

[0051] (6) another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern,

[0052] The second electrode pattern is a transparent electrode pattern,

[0053] The conductive curable resin layer of the photosensitive film having a temporary support, a thermoplastic resin layer and a conductive photocurable resin layer in sequence is transferred to form at least one of the first transparent electrode pattern, the second transparent electrode pattern and the conductive element.

[0054]

[15] The method for manufacturing a capacitive input device according to any one of [5] to

[14] , wherein:

[0055] Preferably, the non-contact surface of the front panel is subjected to surface treatment,

[0056] The photosensitive film described in any one of [1] to [4] is provided on the non-contact surface of the front panel subjected to the surface treatment.

[0057]

[16] In the method for manufacturing a capacitive input device according to

[15] , a silane compound is preferably used in the surface treatment of the front panel.

[0058]

[17] In the method for manufacturing a capacitive input device as described in any one of [5] to

[16] , it is preferred that the front panel has an opening in at least a portion.

[0059]

[18] An electrostatic capacitance input device manufactured according to the method for manufacturing an electrostatic capacitance input device described in any one of [5] to

[17] .

[0060]

[19] An image display device comprising the electrostatic capacitance input device described in

[18] as a constituent element.

[0061] Effects of the Invention

[0062] According to the present invention, it is possible to provide a photosensitive film capable of obtaining a white decorative layer with good brightness, whiteness, network structure, adhesion, development residue and unevenness at a high yield.

[0063] According to the present invention, there can also be provided a method for manufacturing an electrostatic capacitive input device that can manufacture a thin / light-weight electrostatic capacitive input device using a photosensitive film that satisfies the above-mentioned characteristics in a simple process with high quality, an electrostatic capacitive input device obtained by the manufacturing method, and an image display device using the electrostatic capacitive input device. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] [ Figure 1 ] is a cross-sectional view showing the structure of the electrostatic capacitance input device of the present invention.

[0065] [ Figure 2 ] is an explanatory diagram showing an example of a front panel of the present invention.

[0066] [ Figure 3] is an explanatory diagram showing an example of the first transparent electrode pattern and the second transparent electrode pattern of the present invention.

[0067] [ Figure 4 ] is a top view showing an example of a tempered glass having an opening formed therein.

[0068] [ Figure 5 ] is a top view showing an example of a front panel formed with a decorative layer and a mask layer.

[0069] [ Figure 6 ] is a top view showing an example of a front panel having a first transparent electrode pattern formed thereon.

[0070] [ Figure 7 ] is a top view showing an example of a front panel having first and second transparent electrode patterns formed thereon.

[0071] [ Figure 8 ] is a top view showing an example of a front panel having other conductive elements different from the first and second transparent electrode patterns.

[0072] [ Fig. 9 ] is an explanatory diagram showing a cross section of a metal nanowire.

[0073] [ Fig.10 ] is an explanatory diagram showing the half-cut method.

[0074] [ Fig.11 ] is an explanatory diagram showing a half-cut method of a transfer film used for forming a decorative layer on the XX' section of a front panel.

[0075] [ Fig.12 ] is an explanatory diagram showing a half-cut method of a transfer film used to form a decorative layer in a YY' section of a front panel.

[0076] [ Fig.13 ] is an illustration showing the die-cutting method.

[0077] [ Fig.14 ] is an explanatory diagram showing a die-cutting method of a transfer film used to form a decorative layer on the XX' section of the front panel.

[0078] [ Fig.15 ] is an explanatory diagram showing a die-cutting method of a transfer film used to form a decorative layer on the YY' section of the front panel.

[0079] Explanation of symbols

[0080] 1: Front panel

[0081] 3: First transparent electrode pattern

[0082] 3a: Pad part

[0083] 3b: Connection part

[0084] 4: Second transparent electrode pattern

[0085] 5: Insulation layer

[0086] 6: Conductive components

[0087] 7: Transparent protective layer

[0088] 8: Opening

[0089] 10: Capacitive input device

[0090] 11: Strengthened glass

[0091] 21: Temporary support

[0092] 22: Thermoplastic resin layer

[0093] 23: Middle layer

[0094] 24: Coloring layer

[0095] 25: Covering film

[0096] 31: Non-image part

[0097] 32: Image Department

[0098] 33: Blade

[0099] C: Direction 1

[0100] D: 2nd direction DETAILED DESCRIPTION

[0101] Next, the photosensitive film, the method for manufacturing the capacitive input device, the capacitive input device, and the image display device of the present invention are described.

[0102] The description of the constituent elements described below is based on representative embodiments of the present invention, but the present invention is not limited to such embodiments. In addition, "to" in the present application specification is used to mean that the numerical values ​​described before and after it are used as lower limits and upper limits.

[0103] [Photosensitive film]

[0104] The photosensitive film of the present invention has a temporary support and a photocurable resin layer, wherein the photocurable resin layer contains at least (A) a white inorganic pigment, (B) a monomer, (C) a binder, and (D) a photopolymerization initiator. The thickness of the photocurable resin layer is 1 μm to 40 μm, and the content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is 20% by mass to 75% by mass.

[0105] With such a structure, the photosensitive film of the present invention can obtain a white decorative layer having excellent brightness, whiteness, network structure, adhesion, development residue, and unevenness at a high yield.

[0106] The photosensitive film of the present invention comprises a temporary support and a photocurable resin layer. In addition, a thermoplastic resin layer may be provided between the temporary support and the photocurable resin layer.

[0107] The photosensitive film used in the present invention may be a negative-type material or a positive-type material.

[0108] <Temporary Support>

[0109] As the temporary support, a material that is flexible and does not significantly deform, shrink or elongate under pressure or under pressure and heating can be used. Examples of the support include polyethylene terephthalate film, cellulose triacetate film, polystyrene film, polycarbonate film, etc. Among them, biaxially stretched polyethylene terephthalate film is particularly preferred.

[0110] The thickness of the temporary support is not particularly limited, but is usually in the range of 5 μm to 200 μm, and is particularly preferably in the range of 10 μm to 150 μm in terms of ease of handling, versatility, and the like.

[0111] In addition, the temporary support may be transparent, and may contain dyed silica, alumina sol, chromium salt, zirconium salt, or the like.

[0112] Furthermore, conductivity can be imparted to the temporary support by the method described in Japanese Patent Application Laid-Open No. 2005-221726 or the like.

[0113] <Photocurable resin layer>

[0114] For the photosensitive film of the present invention, the photocurable resin layer contains at least (A) a white inorganic pigment, (B) a monomer, (C) a binder, and (D) a photopolymerization initiator, the thickness of the photocurable resin layer is 1 μm to 40 μm, and the content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is 20% by mass to 75% by mass.

[0115] (thickness)

[0116] From the viewpoint of improving the hiding power of the photocurable resin layer for use as a decorative layer of a capacitive input device using the photosensitive film of the present invention, the thickness of the photocurable resin layer needs to be 1 μm to 40 μm.

[0117] The thickness of the photocurable resin layer is more preferably 1.5 μm to 38 μm, and particularly preferably 1.8 μm to 35 μm.

[0118] (composition)

[0119] -(A) White Inorganic Pigments-

[0120] As the white inorganic pigment used in the photocurable resin layer, the white pigment described in paragraph

[0015] or paragraph

[0114] of JP-A-2005-7765 can be used.

[0121] Specifically, titanium oxide (rutile type), titanium oxide (anatase type), zinc oxide, lithopone, light calcium carbonate, white carbon, aluminum oxide, aluminum hydroxide, and barium sulfate are preferred. Titanium oxide (rutile type), titanium oxide (anatase type), and zinc oxide are more preferred, titanium oxide (rutile type) and titanium oxide (anatase type) are further preferred, and rutile titanium oxide is still more preferred.

[0122] The surface of titanium oxide can be treated with silicon dioxide, aluminum oxide or organic matter.

[0123] This can suppress the catalytic activity of titanium oxide, and improve heat resistance, delustering properties, and the like.

[0124] The content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is 20% to 75% by mass, thereby forming a decorative layer having good brightness and whiteness and satisfying other required characteristics. In addition, from the viewpoint of being able to sufficiently shorten the development time when the photosensitive film of the present invention is used in the manufacturing method of the electrostatic capacitance input device of the present invention described later, the content of the white inorganic pigment relative to the total solid content of the photocurable resin layer also needs to be 20% to 75% by mass.

[0125] The content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is more preferably 25% by mass to 60% by mass, and further preferably 30% by mass to 50% by mass.

[0126] The total solid content as used herein refers to the total mass of the photocurable resin layer excluding non-volatile components such as solvents.

[0127] The white inorganic pigment (and other colorants used in the mask layer described later) is preferably used as a dispersion. The dispersion can be prepared by adding a composition obtained by premixing the white inorganic pigment and a pigment dispersant to an organic solvent (or vehicle) described later to disperse the mixture. The vehicle is a medium that disperses the pigment when the coating is in a liquid state, and includes a component (binder) that is liquid and combines with the pigment to form a coating film, and a component (organic solvent) that dissolves and dilutes the pigment.

[0128] There is no particular limitation on the dispersing machine used when dispersing the white inorganic pigment, and examples thereof include kneaders, roller mills, grinders, super grinders, dissolvers, homogenizers, sand mills, and other known dispersing machines described in Item 438 of the first edition of "Dictionary of Pigments" by Kunizo Asakura published by Asakura Bookstore in 2000. Furthermore, the fine pulverization can also be performed by mechanical grinding as described on page 310 of the document, utilizing frictional force.

[0129] From the viewpoint of dispersion stability and hiding power, the white inorganic pigment used in the present invention (colorant for forming a decorative layer) preferably has an average primary particle size of 0.16 μm to 0.3 μm, and more preferably has an average primary particle size of 0.18 μm to 0.27 μm. Pigments with an average primary particle size of 0.19 μm to 0.25 μm are particularly preferred. If the average primary particle size is 0.16 μm, the hiding power drops sharply and the base of the mask layer is easily visible, or the viscosity increases. On the other hand, if the average primary particle size exceeds 0.3 μm, the whiteness decreases, the hiding power drops sharply, and the surface condition during coating deteriorates.

[0130] The “average particle size of primary particles” referred to herein refers to the diameter when the electron microscope image of the particles is set to a circle of the same area, and the “number average particle size” is the particle size obtained for a plurality of particles and refers to the average value of 100 particles.

[0131] On the other hand, when the average particle size in a dispersion or a coating liquid is measured, a laser scattering HORIBAH (manufactured by HORIBA Advanced Techno Co., Ltd.) can be used.

[0132] -(B) Monomer-

[0133] The monomer used in the photocurable resin layer is not particularly limited unless it violates the gist of the present invention, and a known polymerizable compound can be used.

[0134] As the polymerizable compound, the polymerizable compounds described in paragraphs

[0023] to

[0024] of Japanese Patent No. 4098550 can be used.

[0135] In the photosensitive film of the present invention, the content ratio B / C of the solid content of the (B) monomer to the solid content of the (C) binder is preferably 0.4 or more, more preferably 0.58 to 0.95, and particularly preferably 0.6 to 0.9.

[0136] -(C) Adhesive-

[0137] The binder used in the photocurable resin layer is not particularly limited unless it violates the gist of the present invention, and a known polymerizable compound can be used.

[0138] When the photosensitive film of the present invention is a negative material, the photocurable resin layer preferably contains an alkali-soluble resin, a polymerizable compound, a polymerization initiator or a polymerization initiation system. Furthermore, a colorant, an additive, etc. may be used, but are not limited thereto.

[0139] As the alkali-soluble resin contained in the photosensitive film used in the present invention, the polymers described in paragraph

[0025] of JP-A-2011-95716 and paragraphs

[0033] to

[0052] of JP-A-2010-237589 can be used.

[0140] When the photosensitive film is a positive material, for example, materials described in Japanese Patent Application Laid-Open No. 2005-221726 can be used as the photocurable resin layer, but the present invention is not limited thereto.

[0141] -(D) Photopolymerization Initiator-

[0142] As the photopolymerization initiator used in the photocurable resin layer, the polymerizable compounds described in

[0031] to

[0042] described in Japanese Patent Application Publication No. 2011-95716 can be used. Examples of such photopolymerization initiators include "Irgacure-651", "Irgacure-184D", "Irgacure-1800", "Irgacure-907", "Irgacure-369", "Irgacure OXE 01", and "Irgacure OXE 02" (all manufactured by Ciba Speciality Chemicals).

[0143] -additive-

[0144] Furthermore, the photocurable resin layer may also contain additives, such as surfactants described in paragraph

[0017] of Japanese Patent No. 4502784, paragraphs

[0060] to

[0071] of Japanese Unexamined Patent Publication No. 2009-237362, thermal polymerization inhibitors described in paragraph

[0018] of Japanese Patent No. 4502784, and other additives described in paragraphs

[0058] to

[0071] of Japanese Unexamined Patent Publication No. 2000-310706.

[0145] -Solvents-

[0146] Moreover, as a solvent when manufacturing the photosensitive film of this invention by coating, the solvent described in paragraphs

[0043] -

[0044] of Unexamined-Japanese-Patent No. 2011-95716 can be used.

[0147] In the above, the description is mainly based on the case where the photosensitive film of the present invention is a negative-type material, but the photosensitive film may be a positive-type material.

[0148] (Viscosity of photocurable resin layer)

[0149] The viscosity of the photocurable resin layer measured at 100° C. is in the range of 2,000 to 50,000 Pa·sec, and more preferably satisfies the following formula (A).

[0150] Formula (A): Viscosity of thermoplastic resin layer < viscosity of photocurable resin layer

[0151] Here, the viscosity of each layer can be measured as follows. The solvent is removed from the coating liquid for the thermoplastic resin layer or the photocurable resin layer by atmospheric pressure and reduced pressure drying, and the sample is used as a measurement sample. For example, Vibron (DD-III type: manufactured by Toyo Baldwin Co., Ltd.) is used as a measuring instrument, and the measurement is performed under the conditions of a measurement start temperature of 50°C, a measurement end temperature of 150°C, a heating rate of 5°C / min, and a frequency of 1 Hz / deg. The measurement value at 100°C can be used.

[0152] <Thermoplastic Resin Layer>

[0153] The photosensitive film of the present invention preferably has a thermoplastic resin layer between a temporary support and a colored photosensitive resin layer. The thermoplastic resin layer is preferably alkali-soluble. The thermoplastic resin layer acts as a buffer material in a manner that can absorb the concavities and convexities of the substrate surface (including the concavities and convexities caused by the formed image, etc.), and preferably has a property that can be deformed according to the concavities and convexities of the target surface.

[0154] The thermoplastic resin layer preferably contains an organic polymer substance described in Japanese Patent Application Laid-Open No. 5-72724 as a component, and particularly preferably contains at least one substance selected from organic polymer substances having a softening point of about 80° C. or less as measured by the Vicat method [specifically, the polymer softening point measurement method using American Material Testing Method ASTM D1235].

[0155] Specifically, organic polymers include polyolefins such as polyethylene and polypropylene, ethylene copolymers of ethylene and vinyl acetate or its saponified product, copolymers of ethylene and acrylic acid ester or its saponified product, polyvinyl chloride or vinyl chloride copolymers of vinyl chloride and vinyl acetate or its saponified product, polyvinylidene chloride, vinylidene chloride copolymers, polystyrene, styrene copolymers of styrene and (meth)acrylic acid ester or its saponified product, vinyltoluene, vinyltoluene and (meth)acrylic acid ester or its saponified product, vinyltoluene copolymers, poly(meth)acrylate, (meth)acrylate copolymers of butyl (meth)acrylate and vinyl acetate, vinyl acetate copolymer nylon, copolymer nylon, N-alkoxymethylated nylon, N-dimethylamino nylon and other polyamide resins.

[0156] The thickness of the thermoplastic resin layer is preferably 3 μm to 30 μm. When the thickness of the thermoplastic resin layer is less than 3 μm, the followability during lamination is insufficient and the unevenness of the substrate surface cannot be completely absorbed. In addition, when the thickness exceeds 30 μm, the following situations exist: drying (removing the solvent) when forming the thermoplastic resin layer will impose a load on the temporary support, or the development of the thermoplastic resin layer takes time, which deteriorates the process adaptability. As the thickness of the thermoplastic resin layer, it is further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm.

[0157] The thermoplastic resin layer can be formed by coating a preparation liquid containing a thermoplastic organic polymer, and the preparation liquid used for coating can be prepared using a solvent. The solvent is not particularly limited as long as it can dissolve the polymer components constituting the layer, and examples thereof include methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether acetate, n-propanol, 2-propanol, and the like.

[0158] It is preferred that the viscosity of the thermoplastic resin layer measured at 100° C. be in the range of 1000 to 10000 Pa·sec.

[0159] <Other layers>

[0160] The photosensitive film used in the present invention can be appropriately configured by providing an intermediate layer between the photocurable resin layer and the thermoplastic resin layer, or by further providing a protective film on the surface of the photocurable resin layer.

[0161] For the purpose of preventing the mixing of components during coating of multiple layers and storage after coating, it is preferred to provide an intermediate layer in the photosensitive film used in the present invention. As the intermediate layer, an oxygen barrier film having an oxygen barrier function described as a "separation layer" in Japanese Unexamined Patent Publication No. 5-72724 is preferred, which improves the sensitivity during exposure, reduces the time load of the exposure machine, and improves productivity.

[0162] As the intermediate layer and the protective film, those described in paragraphs

[0083] to

[0087] and

[0093] of JP-A-2006-259138 can be appropriately used.

[0163] <Method for producing photosensitive film>

[0164] The photosensitive film of the present invention can be produced according to the method for producing a photosensitive transfer material described in paragraphs

[0094] to

[0098] of JP-A-2006-259138.

[0165] Specifically, in the case of forming the photosensitive film of the present invention having an intermediate layer, it can be appropriately produced by the following operation: a dissolving solution (thermoplastic resin layer coating solution) in which an additive and a thermoplastic organic polymer are dissolved together is applied on a temporary support, and after drying to provide a thermoplastic resin layer, a preparation solution (intermediate layer coating solution) prepared by adding a resin or an additive to a solvent in which the thermoplastic resin layer is not dissolved is applied on the thermoplastic resin layer, and the preparation solution is dried to laminate the intermediate layer, and a colored photosensitive resin layer coating solution prepared using a solvent in which the intermediate layer is not dissolved is further applied on the intermediate layer, and the preparation solution is dried to laminate the colored photosensitive resin layer.

[0166] [Method for manufacturing electrostatic capacitance input device]

[0167] The manufacturing method of the electrostatic capacitive input device of the present invention (hereinafter also referred to as the manufacturing method of the present invention) includes a step of transferring the colored layer of the photosensitive film of the present invention to the non-contact side of the front panel to form at least the following (1) decorative layer, wherein the electrostatic capacitive input device has a front panel and at least the following (1) and (3) to (5) elements on the non-contact side of the front panel.

[0168] (1) Decorative layer

[0169] (3) a plurality of first transparent electrode patterns, which are formed by a plurality of pad portions extending in a first direction via a connecting portion

[0170] (4) a plurality of second electrode patterns which are electrically insulated from the first transparent electrode pattern and include a plurality of pad portions extending in a direction intersecting the first direction.

[0171] (5) An insulating layer that electrically insulates the first transparent electrode pattern from the second electrode pattern. The capacitive input device of the present invention further includes the following (6).

[0172] (6) another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern

[0173] In addition, the second electrode pattern of the electrostatic capacitive input device of the present invention may also be a transparent electrode pattern. It should be noted that in this specification, the second transparent electrode pattern is sometimes described instead of the second electrode pattern, but the preferred embodiment of the second electrode pattern is the same as the preferred embodiment of the second transparent electrode pattern.

[0174] Furthermore, in the method for manufacturing a capacitive input device of the present invention, it is preferable that (2) a mask layer is further provided on the surface of the (1) decorative layer on the non-contact side of the front panel, which is opposite to the front panel.

[0175] <Configuration of Capacitive Input Device>

[0176] First, the structure of the electrostatic capacitance input device formed by the manufacturing method of the present invention will be described. Figure 1 It is a cross-sectional view showing a preferred structure of the electrostatic capacitance input device of the present invention. Figure 1 In the embodiment, the capacitive input device 10 is composed of a front panel 1 , a decoration layer, a mask layer, a first transparent electrode pattern 3 , a second transparent electrode pattern 4 , an insulating layer 5 , a conductive element 6 , and a transparent protective layer 7 .

[0177] The front panel 1 is formed of a light-transmitting substrate such as a glass substrate, and tempered glass such as Corning's Gorilla Glass can be used. Figure 1 In the embodiment of the present invention, the side of the front layer 1 where each element is provided is referred to as a non-contact surface. In the electrostatic capacitance input device 10 of the present invention, input is performed by making a finger or the like contact the contact surface (the opposite side of the non-contact surface) of the front panel 1. Hereinafter, the front panel is sometimes referred to as a "substrate".

[0178] Furthermore, a mask layer is provided on the non-contact surface of the front panel 1. The mask layer is a frame-shaped pattern around the display area formed on the non-contact side of the touch panel front panel, and is formed to hide the extended wiring and the like.

[0179] The decorative layer is formed on the mask layer for the purpose of decoration, that is, between the non-contact side of the touch panel front plate and the mask layer.

[0180] like Figure 2 As shown, in the electrostatic capacitance input device 10 of the present invention, it is preferred to cover a part of the area of ​​the front panel 1 ( Figure 2 The decorative layer and the mask layer are arranged in a manner such that the area other than the input surface is formed. Figure 2As shown, an opening 8 can be provided on a part of the front panel 1. A mechanical switch that can be pressed can be provided in the opening 8. The tempered glass used as the substrate has high strength and is difficult to process. Therefore, in order to form the opening 8, the opening 8 is usually formed before the tempering treatment and then the tempering treatment is performed. However, if a white decorative layer transparent electrode pattern is formed using a liquid resist or screen printing ink for forming a decorative layer on the substrate having the opening 8 after the tempering treatment, the following problems may arise: the resist component leaks from the opening, or the resist component seeps out from the glass end of the mask layer that is necessary to form the light-shielding pattern to the boundary of the front panel as much as possible, thereby contaminating the back side of the substrate. However, the above problems can be solved by using the photosensitive film of the present invention to form a decorative layer on a substrate having an opening 8.

[0181] On the non-contact surface of the front panel 1, there are formed: a plurality of first transparent electrode patterns 3, which are formed by extending a plurality of pad portions in a first direction via a connecting portion; a plurality of second transparent electrode patterns 4, which are electrically insulated from the first transparent electrode pattern 3 and are formed by extending a plurality of pad portions in a direction intersecting the first direction; and an insulating layer 5, which electrically insulates the first transparent electrode pattern 3 and the second transparent electrode pattern 4. The first transparent electrode pattern 3, the second transparent electrode pattern 4 and the conductive element 6 described later can be made, for example, using a translucent conductive metal oxide film such as ITO (Indium Tin Oxide) or IZO (Indium Zinc Oxide). As such a metal film, there can be cited: ITO film; metal films such as Al, Zn, Cu, Fe, Ni, Cr, Mo; metal oxide films such as SiO2, etc. At this time, the film thickness of each element can be set to 10nm to 200nm. In addition, the amorphous ITO film is made into a polycrystalline ITO film by firing, so the resistance can also be reduced. In addition, the first transparent electrode pattern 3, the second transparent electrode pattern 4 and the conductive element 6 described later can also be manufactured using a photosensitive film having a photocurable resin layer described later, and the photocurable resin layer uses conductive fibers. In addition, when the first transparent electrode pattern is formed of ITO or the like, paragraphs

[0014] to

[0016] of Japanese Patent Gazette No. 4506785 can be used as a reference.

[0182] In addition, at least one of the first transparent electrode pattern 3 and the second transparent electrode pattern 4 may be provided over both the non-contact surface of the front panel 1 and the surface of the mask layer opposite to the front panel 1 . Figure 1, a diagram showing that the second transparent electrode pattern is arranged over two regions of the non-contact surface of the front panel 1 and the surface of the mask layer opposite to the front panel 1. Thus, even in the case of laminating a photosensitive film over a mask layer that requires a certain thickness and the back of the front panel, by using the photosensitive film having a specific layer structure of the present invention, lamination without generating bubbles at the boundary of the mask portion can be performed in a simple process without using expensive equipment such as a vacuum laminator.

[0183] use Figure 3 The first transparent electrode pattern 3 and the second transparent electrode pattern 4 are described. Figure 3 1 is an explanatory diagram showing an example of the first transparent electrode pattern and the second transparent electrode pattern of the present invention. Figure 3 As shown, the first transparent electrode pattern 3 is formed by extending the pad portion 3a via the connecting portion 3b in the first direction. In addition, the second transparent electrode pattern 4 is electrically insulated from the first transparent electrode pattern 3 by the insulating layer 5, and is formed by extending the pad portion 3a via the connecting portion 3b in the first direction. Figure 3 Here, when forming the first transparent electrode pattern 3, the pad portion 3a and the connecting portion 3b may be integrally formed, or only the connecting portion 3b may be formed, and the pad portion 3a and the second transparent electrode pattern 4 may be integrally formed (patterned). In the case where the pad portion 3a and the second transparent electrode pattern 4 are integrally formed (patterned), Figure 3 As shown, each layer is formed in such a manner that a part of the connection part 3 b and a part of the pad part 3 a are connected, and the first transparent electrode pattern 3 and the second transparent electrode pattern 4 are electrically insulated by the insulating layer 5 .

[0184] Figure 1 In the embodiment, a conductive element 6 is provided on the surface of the mask layer opposite to the front panel 1. The conductive element 6 is another element electrically connected to at least one of the first transparent electrode pattern 3 and the second electrode pattern 4 and different from the first transparent electrode pattern 3 and the second electrode pattern 4. Figure 1 , a diagram showing that the conductive element 6 is connected to the second transparent electrode pattern 4 is shown.

[0185] in addition, Figure 1 In the embodiment of the present invention, a transparent protective layer 7 is provided in a manner covering all the constituent elements. The transparent protective layer 7 may also be configured in a manner covering only a part of the constituent elements. The insulating layer 5 and the transparent protective layer 7 may be made of the same material or different materials. The materials constituting the insulating layer 5 and the transparent protective layer 7 are preferably materials having high surface hardness and heat resistance, and known photosensitive silicone resin materials, acrylic resin materials, etc. may be used.

[0186] Hereinafter, the production method of the present invention will be described in detail with respect to each layer.

[0187] As an example of the method of forming in the process of the production method of the present invention, there can be mentioned: Figures 4 to 8 way. Figure 4 It is a top view showing an example of the tempered glass 11 in which the opening 8 is formed.

[0188] Figure 5 This is a top view showing an example of a front panel on which a decorative layer and a mask layer are formed. Figure 6 It is a top view showing an example of a front panel on which the first transparent electrode pattern 3 is formed. Figure 7 1 is a top view showing an example of a front panel on which the first transparent electrode pattern 3 and the second transparent electrode pattern 4 are formed. Figure 8 1 is a top view showing an example of a front panel formed with another conductive element 6 different from the first transparent electrode pattern and the second transparent electrode pattern. Figure 6 to Figure 8 This is a conceptual diagram for showing the arrangement of the first transparent electrode pattern 3, the second transparent electrode pattern 4, and other conductive elements 6 inside the front panel when viewed from the decorative layer side of the front panel. Due to the use of the decorative layer, these internal components cannot be observed by naked eyes from the decorative layer side. In addition, Figure 6 to Figure 8 These drawings show examples for concretely implementing the above-described description, and the scope of the present invention is not to be interpreted as being limited by these drawings.

[0189] <(1) Decorative layer>

[0190] The production method of the present invention is characterized in that at least the (1) decorative layer is formed using the photosensitive film of the present invention.

[0191] If the photosensitive film is used to form the decorative layer, etc., there will be no leakage of the resist components from the opening portion on the substrate (front panel) having the opening portion, and in particular, there will be no seepage of the resist components from the glass end of the mask layer which is necessary to form the shading pattern as close as possible to the boundary of the front panel. Therefore, the back side of the substrate will not be contaminated, and a touch panel with the advantages of thin layer / lightweight can be manufactured by a simple process.

[0192] The method of forming the decorative layer using the photosensitive film of the present invention is usually formed by a conventional photolithography method when a transfer film is used, if the coloring layer contains a photocurable resin. After lamination on a substrate, it is exposed to a desired pattern. In the case of a negative material, the non-exposed portion is developed and removed, and in the case of a positive material, the exposed portion is developed and removed, thereby obtaining a pattern. At this time, the thermoplastic resin layer and the photocurable layer can be developed and removed using different solutions, or they can be removed using the same solution. Here, regarding the transfer film of the present invention, the decorative layer can be formed using the transfer film of the present invention using the following transfer method by half cutting or transfer method by die cutting.

[0193] In the transfer method by half-cutting, first, Figure 10 to Figure 12 As shown, after pre-cutting the boundary between the image part 32 and the non-image part 31 of the decorative layer with a razor or the like, the protective film, the decorative layer and the intermediate layer of the non-image part 31 are removed with tape, and then the protective film of the image part 32 is also removed, and the decorative layer pattern is transferred to the substrate.

[0194] On the other hand, in the die-cutting transfer method, first, as Figure 13 to Figure 15 As shown, after pre-cutting the boundary between the image portion 32 and the non-image portion 31 of the decorative layer in a manner penetrating the entire layer using a razor or the like, the protective film of the image portion 32 remaining after the colored layer (non-image portion 31) in the said part of the area is removed using tape, and the decorative layer pattern is transferred onto the substrate.

[0195] Next, the thermoplastic resin layer and the intermediate layer are removed by development, thereby forming a decorative layer pattern.

[0196] A known developing device such as a brush or a high-pressure sprayer may be combined as needed. After the development, post-exposure and post-baking may be performed as needed.

[0197] In addition, in order to improve the adhesion of the photosensitive resin layer achieved by lamination in the transfer process described later, the non-contact surface of the substrate (front panel) may be subjected to surface treatment in advance. As the surface treatment, surface treatment using a silane compound (silane coupling treatment) is preferably performed. As a silane coupling agent, a silane coupling agent having a functional group that interacts with the photosensitive resin is preferred. For example, a silane coupling liquid (0.3% by mass aqueous solution of N-β (aminoethyl) γ-aminopropyltrimethoxysilane, trade name: KBM603, manufactured by Shin-Etsu Chemical Co., Ltd.) is blown by spraying for 20 seconds, and then washed by pure water spraying. Then, it is reacted by heating. A heating tank can be used, or the substrate can be preheated by a laminator to promote the reaction.

[0198] In the case of forming a permanent material using the photosensitive film of the present invention, a patterning method using the photosensitive film of the present invention will be described by taking a method of forming a decorative layer as an example.

[0199] The method for forming the decorative layer may include a method having the following steps: a covering film removal step, in which the covering film is removed from the photosensitive film of the present invention; a transfer step, in which the photosensitive resin layer of the photosensitive transfer material with the covering film removed is transferred onto a substrate; an exposure step, in which the photosensitive resin layer transferred onto the substrate is exposed; and a development step, in which the exposed photosensitive resin layer is developed to obtain a pattern image.

[0200] When forming an image by a conventional photolithography method, there may be mentioned a method having the following steps: a cover film removal step of removing the cover film from the photosensitive film; and a transfer step of transferring the photosensitive resin layer of the photosensitive transfer material from which the cover film has been removed onto a substrate.

[0201] The method for forming a decorative layer also preferably includes the following steps: a half-cutting step, in which an incision is formed in a portion of the transfer film, the incision having a depth that penetrates the colored layer but does not penetrate the temporary support body; a step of removing the colored layer from at least a portion of the area surrounded by the incision; and a step of forming the (1) decorative layer using the transfer film from which the colored layer in the portion of the area has been removed.

[0202] In addition, the method for forming a decorative layer also preferably includes the following steps: a die-cutting step of forming an incision from the colored layer through the temporary support body in a portion of the transfer film; and a step of forming the (1) decorative layer using the transfer film after removing the colored layer in the portion of the area.

[0203] The process of forming a cut in a portion of the transfer film that penetrates the coloring layer but does not penetrate the temporary support body, and the process of forming a cut from the coloring layer to the temporary support body are also referred to as the process of pre-cutting the image portion transferred in the coloring layer. It should be noted that the case of forming a cut that penetrates the coloring layer but does not penetrate the temporary support body as described above is also referred to as half-cutting. The case of forming a cut that penetrates the temporary support body from the coloring layer is also referred to as die-cutting.

[0204] The step of removing the colored layer from at least a part of the region surrounded by the cutout is also referred to as a step of removing the colored layer from the non-image portion that has not been transferred.

[0205] Furthermore, when the transfer film of the present invention includes a protective film, an intermediate layer or a thermoplastic resin layer, the process of removing the colored layer in at least a portion of the area surrounded by the incision is preferably a process of removing the protective film and colored layer of the non-image part, and the protective film of the image part.

[0206] The step of forming the decorative layer (1) using the transfer film from which the colored layer in the partial region has been removed is also referred to as a transfer step of transferring the colored layer of the image portion onto a substrate.

[0207] Furthermore, in the case where the transfer film of the present invention contains a protective film, an intermediate layer or a thermoplastic resin layer, the process of forming the (1) decorative layer using the transfer film after removing the colored layer in the partial area is preferably a transfer process in which the colored layer of the image portion of the transfer film from which the protective film has been removed is transferred onto a substrate.

[0208] In this case, the step of forming the (1) decorative layer using the transfer film from which the colored layer in the partial region is removed preferably includes the step of peeling off the temporary support transferred onto the substrate.

[0209] In this case, the step of forming the (1) decorative layer using the transfer film from which the colored layer in the partial region has been removed preferably includes a step of removing the thermoplastic resin layer and the intermediate layer.

[0210] The manufacturing method of the present invention is more preferably a method comprising the following steps: a step of pre-cutting the transferred image portion in the colored layer of the transfer film of the present invention; a step of removing the protective film and the colored layer of the non-image portion, and the protective film of the image portion; a transfer step of transferring the colored layer of the image portion of the transfer film from which the protective film has been removed onto a substrate; a step of peeling off the temporary support transferred onto the substrate; and a step of removing the thermoplastic resin layer and the intermediate layer.

[0211] On the other hand, when the coloring layer has a photocurable resin layer, the method for forming the decorative layer may include a method including the following steps: a protective film removal step of removing the protective film from the transfer film; and a transfer step of transferring the photocurable resin layer of the photosensitive transfer material from which the protective film has been removed onto a substrate. In this case, it is preferred that after the transfer step, there is further a step of post-exposing the transferred photocurable resin layer.

[0212] (Pre-cutting process)

[0213] In the production method of the present invention, when the image is not formed by a conventional photolithography method, it is necessary to form an image portion on the coloring layer before transfer.

[0214] The types of pre-cutting include the following steps: a step of forming a cut in a portion of the transfer film that penetrates the coloring layer but does not penetrate the temporary support (half-cutting step); and a step of forming a cut that penetrates the temporary support from the coloring layer (die-cutting step).

[0215] (i) Half-cutting process

[0216] First, the half-cutting process will be described below.

[0217] There is no particular limitation on the method for forming the incision, and the incision may be formed by any method such as a blade, a laser, etc., but it is preferably formed by a blade. In addition, the structure of the blade is not particularly limited.

[0218] When the transfer film is composed of, for example, a temporary support, a thermoplastic resin layer, an intermediate layer, a colored layer, and a protective film stacked in this order, a cut can be formed by, for example, using a knife or a laser to penetrate the protective film, the colored layer, and the intermediate layer and reach a part of the thermoplastic resin layer, thereby separating the transferred image portion from the untransferred non-image portion.

[0219] -Step of removing the colored layer from the non-image area-

[0220] In order to selectively transfer the image portion of the coloring layer pre-cut by half-cutting to the substrate, it is necessary to study not to transfer the non-image portion. One method is a method of removing the coloring layer of the non-image portion before transfer, and a method of simultaneously peeling off the coloring layer and the intermediate layer of the non-image portion after removing the protective film. Another method is a method of peeling off the protective film on the non-image portion, then peeling off the coloring layer and the intermediate layer at the same time, and then peeling off the protective film on the image portion. From the viewpoint of protecting the image portion of the coloring layer until just before transfer, the latter method is preferred.

[0221] (ii) Die-cutting process

[0222] Next, a step (die cutting step) of forming a cut in a part of the transfer film so as to penetrate from the colored layer through the temporary support will be described below.

[0223] The method of forming the incision is not particularly limited, as in the case of the half-cut method, and the incision may be formed by any method such as a blade, a laser, etc., and is preferably formed by a blade. In addition, the structure of the blade is not particularly limited.

[0224] When the transfer film is composed of, for example, a temporary support, a thermoplastic resin layer, an intermediate layer, a coloring layer, and a protective film stacked in this order, a cut can be formed on the protective film, penetrating the protective film, the coloring layer, the intermediate layer, the thermoplastic resin layer, and the temporary support, for example by using a knife or a laser, so that the transferred image portion and the untransferred non-image portion can be separated.

[0225] (Transfer process)

[0226] The transfer step is a step of transferring the photocurable resin layer of the photosensitive film from which the cover film has been removed onto a substrate.

[0227] In this case, a method in which the photocurable resin layer of the photosensitive film is laminated on a substrate and then the temporary support is removed is preferred.

[0228] The transfer (lamination) of the photocurable resin layer to the substrate surface is carried out by overlapping the photocurable resin layer on the substrate surface, pressurizing and heating. When laminating, a known laminator such as a laminator, a vacuum laminator, and an automatic cutting laminator that can further improve productivity can be used.

[0229] (Step of exposing the photosensitive resin composition on the substrate)

[0230] When an image is formed by a common photolithography method or a decorative layer is applied to a substrate using the photosensitive film, the exposure step is preferably a step of exposing the photocurable resin layer transferred onto the substrate.

[0231] Specifically, there can be mentioned a method in which a predetermined mask is disposed above the photocurable resin layer formed on the substrate, and then exposure is performed from above the mask via the mask, the thermoplastic resin layer, and the intermediate layer.

[0232] Here, as the light source for the exposure, any light source that can irradiate light in a wavelength region that can cure the photocurable resin layer (e.g., 365 nm, 405 nm, etc.) can be appropriately selected for use. Specifically, ultra-high pressure mercury lamps, high pressure mercury lamps, metal halide lamps, etc. can be cited. The exposure dose is usually 5 to 200 mJ / cm 2 About 10 to 100 mJ / cm 2 about.

[0233] (Development Process)

[0234] In the case of forming an image by a conventional photolithography method, the development can be performed using a developer. The developer is not particularly limited, and a known developer such as the developer described in Japanese Patent Laid-Open No. 5-72724 can be used. In addition, the developer is preferably a developer that dissolves the photocurable resin layer, for example, preferably a developer containing a compound with pKa=7 to 13 at a concentration of 0.05 to 5 mol / L, and a small amount of an organic solvent miscible with water can also be added. Examples of organic solvents miscible with water include methanol, ethanol, 2-propanol, 1-propanol, butanol, diacetone alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-butyl ether, benzyl alcohol, acetone, methyl ethyl ketone, cyclohexanone, ε-caprolactone, γ-butyrolactone, dimethylformamide, dimethylacetamide, hexamethylphosphoramide, ethyl lactate, methyl lactate, ε-caprolactam, N-methylpyrrolidone, and the like. The concentration of the organic solvent is preferably 0.1% by mass to 30% by mass.

[0235] Furthermore, a known surfactant may be further added to the developer, and the concentration of the surfactant is preferably 0.01% by mass to 10% by mass.

[0236] The development method may be any of immersion development, shower development, spray and spin development, immersion development, etc. Here, if the shower development is described, the developer may be blown onto the exposed photocurable resin layer by spraying to remove the uncured portion.

[0237] In addition, when a thermoplastic resin layer or an intermediate layer is provided, it is preferred to remove the thermoplastic resin layer, the intermediate layer, etc. by spraying an alkaline solution with low solubility of the photocurable resin layer before development. In addition, it is preferred to remove the development residue by wiping with a brush, etc. while spraying a cleaning agent, etc. after development. The liquid temperature of the developer is preferably 20°C to 40°C, and the pH value of the developer is preferably 8 to 13.

[0238] On the other hand, when the coloring layer pre-cut by half-cutting or die-cutting is transferred to the substrate, when the desired pattern is formed in advance, the exposure step or the development step of the usual photolithography method may not be included. In this case, when a thermoplastic resin layer or an intermediate layer is also provided, the step of removing the thermoplastic resin layer and the intermediate layer after the transfer step may be included, and the step of removing the thermoplastic resin layer and the intermediate layer may be performed using the same developer as the alkaline developer generally used in the photolithography method.

[0239] (Post-exposure process)

[0240] The development step may include a post-exposure step after the development step.

[0241] The post-exposure step may be performed only from the surface direction of the photosensitive resin composition on the side in contact with the substrate, only from the surface direction of the side not in contact with the transparent substrate, or from directions of both surfaces.

[0242] (Other processes)

[0243] The production method of the present invention may include other steps such as a post-baking step.

[0244] In addition, as examples of the exposure step, the development step, and other steps, the methods described in paragraphs

[0035] to

[0051] of Japanese Patent Application Laid-Open No. 2006-23696 can also be applied to the present invention.

[0245] The patterned exposure may be performed after peeling off the temporary support, or may be performed before peeling off the temporary support and then peeling off the temporary support. The exposure may be performed through a mask or may be digital exposure using a laser or the like.

[0246] <(2) Mask Layer>

[0247] In the manufacturing method of the present invention, in addition to the decorative layer, at least one of the mask layer, the first transparent electrode pattern 3, the second transparent electrode pattern 4, the insulating layer 5, the conductive element 6, and the transparent protective layer 7 as required is preferably formed by using a photosensitive film having the photosensitive resin composition stacked on a temporary support, and more preferably formed by using a photosensitive film having a temporary support, a thermoplastic resin layer and a photocurable resin layer in sequence.

[0248] For example, when forming a black mask layer, it can be formed by using a photosensitive film having a black photocurable resin layer as the photocurable resin layer and transferring the black photocurable resin layer onto the surface of the front panel 1 .

[0249] Furthermore, in the formation of a mask layer that requires light-shielding properties, bubbles can be prevented from being generated when the photosensitive film is laminated by using a photosensitive film with a specific layer structure, wherein the specific layer structure has a thermoplastic resin layer between the photocurable resin layer and the temporary support body, thereby forming a high-quality mask layer without light leakage.

[0250] When the photocurable resin layer of the photosensitive film is used as a mask layer, a colorant can be used in the photocurable resin layer. As the colorant used in the present invention, a known colorant (organic pigment, inorganic pigment, dye, etc.) can be used appropriately. In addition, a mixture of white, black, red, blue, green and other pigments can be used in the present invention.

[0251] In particular, when the photosensitive film's photocurable resin layer is used as a black mask layer, it preferably contains a black colorant from the viewpoint of optical density. Examples of black colorants include carbon black, titanium carbon, iron oxide, titanium oxide, and graphite, and carbon black is preferred.

[0252] In order to use it as a mask layer of other colors, the pigments or dyes described in paragraphs

[0183] to

[0185] of Japanese Patent No. 4546276 can also be mixed and used. Specifically, the pigments and dyes described in paragraphs

[0038] to

[0054] of Japanese Patent Publication No. 2005-17716, the pigments described in paragraphs

[0068] to

[0072] of Japanese Patent Publication No. 2004-361447, and the colorants described in paragraphs

[0080] to

[0088] of Japanese Patent Publication No. 2005-17521 can be suitably used.

[0253] From the viewpoint of dispersion stability, the colorant used in the present invention other than the decorative layer preferably has a number average particle size of 0.001 μm to 0.1 μm, and more preferably has a number average particle size of 0.01 μm to 0.08 μm. In addition, the so-called "particle size" here refers to the diameter when the electron microscope image of the particle is set to a circle of the same area, and the so-called "number average particle size" is the particle size obtained for a plurality of particles, and refers to the average value of 100 particles.

[0254] <(3) A plurality of first transparent electrode patterns formed by extending a plurality of pad portions in a first direction via a connecting portion>

[0255] The manufacturing method of the electrostatic capacitive input device of the present invention preferably forms the first transparent electrode pattern, the second transparent electrode pattern and at least one of the conductive elements by etching a transparent conductive material using an etching pattern formed by a photosensitive film having a temporary support body, a thermoplastic resin layer and a photocurable resin layer in sequence.

[0256] On the other hand, the manufacturing method of the electrostatic capacitance input device of the present invention preferably uses a photosensitive film having a temporary support, a thermoplastic resin layer and a photocurable resin layer in sequence to form at least one of the first transparent electrode pattern, the second transparent electrode pattern and the conductive element. The use of a transfer film having a temporary support and a conductive photocurable resin layer in sequence to form at least one of the first transparent electrode pattern, the second transparent electrode pattern and the conductive element specifically refers to transferring the conductive photocurable resin layer of the transfer film having a temporary support and a conductive photocurable resin layer in sequence to form at least one of the first transparent electrode pattern, the second transparent electrode pattern and the conductive element.

[0257] That is, the first transparent electrode pattern 3 is preferably formed by etching or using a photosensitive film having a conductive photocurable resin layer.

[0258] (Etching treatment)

[0259] When the first transparent electrode pattern 3 is formed by etching, a transparent electrode layer such as ITO is first formed by sputtering on the non-contact surface of the front panel 1 on which a mask layer is formed. Next, an etching pattern is formed on the transparent electrode layer by exposure and development using a photosensitive film having an etching photocurable resin layer as the photocurable resin layer. Then, the transparent electrode layer is etched, the transparent electrode is patterned, and the etching pattern is removed to form the first transparent electrode pattern 3 and the like.

[0260] When the photosensitive film of the present invention is used as a resist (etching pattern), a resist pattern can be obtained in the same manner as the above method. The etching and resist stripping can be performed by known methods described in paragraphs

[0048] to

[0054] of JP-A-2010-152155.

[0261] For example, as an etching method, a wet etching method in which the etching solution is immersed in an etching solution that is usually performed can be cited. The etching solution used in the wet etching can be an acidic or alkaline etching solution that is appropriately selected according to the object to be etched. Examples of acidic etching solutions include: aqueous solutions of acidic components such as hydrochloric acid, sulfuric acid, hydrofluoric acid, phosphoric acid, etc., mixed aqueous solutions of acidic components and salts such as ferric chloride, ammonium fluoride, potassium permanganate, etc. The acidic component can also be a combination of multiple acidic components. In addition, examples of alkaline etching solutions include: aqueous solutions of alkaline components such as sodium hydroxide, potassium hydroxide, ammonia, organic amines, salts of organic amines such as tetramethylammonium hydroxide, mixed aqueous solutions of alkaline components and salts such as potassium permanganate, etc. The alkaline component can also be a combination of multiple alkaline components.

[0262] The temperature of the etching solution is not particularly limited, but is preferably 45° C. or less. The resin pattern used as the etching mask (etching pattern) in the present invention is formed by using the photocurable resin layer, thereby exhibiting particularly excellent resistance to acidic and alkaline etching solutions in the temperature range. Therefore, the resin pattern is prevented from peeling off during the etching process, and the portion where the resin pattern does not exist is selectively etched.

[0263] After the etching, in order to prevent contamination of the production line, a cleaning process and a drying process may be performed as needed. For the cleaning process, for example, the substrate is cleaned with pure water at room temperature for 10 seconds to 300 seconds. For the drying process, a blower is used and the blower pressure is appropriately adjusted (0.1 to 5 kg / cm 2 Just do it.

[0264] Next, there is no particular limitation on the method for stripping the resin pattern, and for example, a method of immersing the substrate in a stirring stripping solution for 5 to 30 minutes at 30°C to 80°C, preferably 50°C to 80°C, can be cited. The resin pattern used as an etching mask in the present invention exhibits excellent resistance to chemical liquids below 45°C as described above, and if the temperature of the chemical liquid is above 50°C, it exhibits the property of swelling due to an alkaline stripping solution. Due to this property, if a stripping solution of 50°C to 80°C is used for the stripping process, there are advantages in that the process time is shortened and the stripping residue of the resin pattern is reduced. That is, by providing a temperature difference of the chemical liquid between the etching process and the stripping process, the resin pattern used as an etching mask in the present invention exhibits good resistance to chemical liquids in the etching process, and on the other hand, exhibits good stripping properties in the stripping process, and can simultaneously satisfy the two opposite characteristics of resistance to chemical liquids and stripping properties.

[0265] Examples of the stripping solution include those obtained by dissolving an inorganic base component such as sodium hydroxide or potassium hydroxide, or an organic base component such as a tertiary amine or a quaternary ammonium salt in water, dimethyl sulfoxide, N-methylpyrrolidone, or a mixed solution thereof. The stripping solution may be used to perform stripping by a spraying method, a showering method, an immersion method, or the like.

[0266] (Method using a photosensitive film having a conductive photocurable resin layer)

[0267] In addition, the photosensitive film of the present invention can also be used as a lift-off material to form a first transparent electrode pattern, a second transparent electrode pattern and other conductive components. In this case, the photosensitive film of the present invention can be used for patterning to form a transparent conductive layer on the entire surface of the substrate, and then the photocurable resin layer of the present invention is dissolved and removed together with the deposited transparent conductive layer, thereby obtaining the desired transparent conductive layer pattern (lift-off method).

[0268] When the first transparent electrode pattern 3 is formed using a photosensitive film having a conductive photocurable resin layer, the first transparent electrode pattern 3 may be formed by transferring the conductive photocurable resin layer onto the surface of the front panel 1 .

[0269] If the photosensitive film having a conductive photocurable resin layer is used to form the first transparent electrode pattern 3, there will be no leakage of the resist component from the opening portion on the substrate (front panel) having an opening portion, and the back side of the substrate will not be contaminated. A touch panel with the advantages of thin layer / lightweight can be manufactured with a simple process.

[0270] Furthermore, in the formation of the first transparent electrode pattern 3, the generation of bubbles during lamination of the photosensitive film can be prevented by using the photosensitive film of the present invention having a specific layer structure, thereby forming the first transparent electrode pattern 3 with excellent conductivity and low resistance, wherein the specific layer structure has a thermoplastic resin layer between the conductive photocurable resin layer and the temporary support.

[0271] In addition, when the photosensitive film has a conductive photocurable resin layer, the photocurable resin layer contains conductive fibers and the like.

[0272] - Conductive photocurable resin layer (conductive fiber) -

[0273] When the photosensitive film on which the conductive photocurable resin layer is laminated is used to form a transparent electrode pattern or other conductive elements, the following conductive fibers and the like can be used for the photocurable resin layer.

[0274] The structure of the conductive fiber is not particularly limited and can be appropriately selected depending on the intended purpose, but is preferably a solid structure or a hollow structure.

[0275] Here, solid fibers are sometimes referred to as “wires”, and hollow fibers are sometimes referred to as “tubes.” Also, conductive fibers having an average minor axis length of 5 nm to 1,000 nm and an average major axis length of 1 μm to 100 μm are sometimes referred to as “nanowires.”

[0276] In addition, conductive fibers having an average minor axis length of 1 nm to 1,000 nm and an average major axis length of 0.1 μm to 1,000 μm and having a hollow structure are sometimes referred to as “nanotubes”.

[0277] The material of the conductive fiber is not particularly limited as long as it has conductivity and can be appropriately selected according to the purpose. It is preferably at least any one of metal and carbon. Among these materials, the conductive fiber is particularly preferably at least any one of metal nanowires, metal nanotubes, and carbon nanotubes.

[0278] -Metal nanowires-

[0279] --Metal--

[0280] There is no particular limitation on the material of the metal nanowires, but it is preferably at least one metal selected from the 4th, 5th, and 6th periods of the periodic table (IUPAC 1991), more preferably at least one metal selected from groups 2 to 14, further preferably at least one metal selected from groups 2, 8, 9, 10, 11, 12, 13, and 14, and it is particularly preferred to contain it as a main component.

[0281] Examples of the metal include copper, silver, gold, platinum, palladium, nickel, tin, cobalt, rhodium, iridium, iron, ruthenium, osmium, manganese, molybdenum, tungsten, niobium, tantalum, titanium, bismuth, antimony, lead, and alloys of these metals. Among these metals, metals mainly containing silver or metals containing an alloy of silver and a metal other than silver are preferred because of their excellent electrical conductivity.

[0282] Mainly containing silver means that the metal nanowires contain 50% by mass or more of silver, preferably 90% by mass or more of silver.

[0283] Examples of the metal used in the form of an alloy with silver include platinum, osmium, palladium, and iridium. These metals may be used alone or in combination of two or more.

[0284] --shape--

[0285] The shape of the metal nanowires is not particularly limited and can be appropriately selected according to the purpose. For example, any shape such as a cylinder, a rectangular parallelepiped, or a column with a polygonal cross section can be adopted. However, in applications requiring high transparency, a cylinder or a polygonal cross section with rounded corners is preferred.

[0286] The cross-sectional shape of the metal nanowires can be investigated by applying a metal nanowire aqueous dispersion on a substrate and observing the cross section using a transmission electron microscope (TEM).

[0287] The so-called corners of the cross section of the metal nanowire refer to the periphery of the point where the perpendicular lines extending the sides of the cross section from the adjacent sides intersect. In addition, the so-called "sides of the cross section" refer to the straight lines connecting these adjacent corners. In this case, the ratio of the "circumference of the cross section" to the total length of the "sides of the cross section" is taken as the sharpness. In, for example Fig. 9In the metal nanowire cross section shown, the sharpness can be expressed by the ratio of the outer perimeter of the cross section represented by the solid line and the outer perimeter of the pentagon represented by the dotted line. The cross-sectional shape with a sharpness of less than 75% is defined as a cross-sectional shape with rounded corners. The sharpness is preferably less than 60%, more preferably less than 50%. If the sharpness exceeds 75%, the following situation exists: electrons are locally present in the corner, and yellowing may remain due to increased plasmon absorption, thereby causing deterioration in transparency. In addition, sometimes the linearity of the edge of the pattern decreases and instability occurs. The lower limit of the sharpness is preferably 30%, more preferably 40%.

[0288] --Average minor axis length and average major axis length--

[0289] The average minor axis length (sometimes referred to as "average minor axis diameter" or "average diameter") of the metal nanowires is preferably 150 nm or less, more preferably 1 nm to 40 nm, further preferably 10 nm to 40 nm, and particularly preferably 15 nm to 35 nm.

[0290] If the average minor axis length is less than 1 nm, the oxidation resistance may be deteriorated and the durability may be poor. If it exceeds 150 nm, scattering due to the metal nanowires may occur and sufficient transparency may not be obtained.

[0291] The average minor axis length of the metal nanowires is obtained by observing 300 metal nanowires using a transmission electron microscope (TEM, manufactured by JEOL Ltd., JEM-2000FX), and calculating the average minor axis length of the metal nanowires based on the average value thereof. It should be noted that the minor axis length of the metal nanowires when the minor axis is not circular is the longest minor axis length.

[0292] The average major axis length (sometimes referred to as “average length”) of the metal nanowires is preferably 1 μm to 40 μm, more preferably 3 μm to 35 μm, and further preferably 5 μm to 30 μm.

[0293] If the average major axis length is less than 1 μm, it may be difficult to form a dense network and sufficient conductivity may not be obtained. If it exceeds 40 μm, the metal nanowires may be too long and entangled during production, resulting in agglomerates during the production process.

[0294] The average major axis length of the metal nanowires is obtained by observing 300 metal nanowires using, for example, a transmission electron microscope (TEM, manufactured by JEOL Ltd., JEM-2000FX), and calculating the average major axis length of the metal nanowires based on the average value thereof. In addition, when the metal nanowires are curved, the arc is considered as a circle, and the value calculated based on the radius and curvature is used as the major axis length.

[0295] From the viewpoint of process adaptability such as stability of the coating liquid, drying during coating or development time during patterning, the thickness of the conductive photocurable resin layer is preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 18 μm, and particularly preferably 1 μm to 15 μm. From the viewpoint of conductivity and stability of the coating liquid, the content of the conductive fiber relative to the total solid content of the conductive photocurable resin layer is preferably 0.01% to 50% by mass, more preferably 0.05% to 30% by mass, and particularly preferably 0.1% to 20% by mass.

[0296] <(4) A plurality of second transparent electrode patterns electrically insulated from the first transparent electrode pattern and composed of a plurality of pad portions extending in a direction intersecting the first direction>

[0297] The second transparent electrode pattern 4 can be formed by etching or using a photosensitive film having a conductive photocurable resin layer. The preferred method in this case is the same as the method for forming the first transparent electrode pattern 3 .

[0298] <(5) Insulating layer electrically insulating the first transparent electrode pattern from the second transparent electrode pattern>

[0299] When forming the insulating layer 5 , it can be formed by using a photocurable resin layer having insulating properties as the photosensitive film of the present invention as the photocurable resin layer and transferring the photocurable resin layer onto the surface of the front panel 1 having the first transparent electrode pattern formed thereon.

[0300] When the insulating layer is formed using the photosensitive film, the thickness of the photocurable resin layer is preferably 0.1 μm to 5 μm, more preferably 0.3 μm to 3 μm, and particularly preferably 0.5 μm to 2 μm from the viewpoint of maintaining insulation properties.

[0301] <(6) Other conductive elements electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern>

[0302] The other conductive element 6 can be formed by an etching process or by using a photosensitive film having a conductive photocurable resin layer.

[0303] The second transparent electrode pattern 4 can be formed by etching or using a photosensitive film having a conductive photocurable resin layer. The preferred method in this case is the same as the method for forming the first transparent electrode pattern 3 .

[0304] <(7) Transparent protective layer>

[0305] When forming the transparent protective layer 7 , it can be formed by using a photosensitive film having a transparent photocurable resin layer as the photocurable resin layer and transferring the photocurable resin layer onto the surface of the front panel 1 on which each element is formed.

[0306] When forming a transparent protective layer using the photosensitive film, the thickness of the photocurable resin layer is preferably 0.5 μm to 10 μm, more preferably 0.8 μm to 5 μm, and particularly preferably 1 μm to 3 μm from the viewpoint of exhibiting sufficient surface protection ability.

[0307] "Capacitive input device, and image display device having a capacitive input device as a component"

[0308] The electrostatic capacitive input device obtained by the manufacturing method of the present invention, and the image display device having the electrostatic capacitive input device as a constituent element can apply the structures disclosed in: "The Latest Touch Panel Technology" (published on July 6, 2009, TechnoTimes Co., Ltd.), "Technology and Development of Touch Panels" edited by Yuji Mitani and published by CMC (December 2004), 2009 Flat Panel Display International Forum (FPD International 2009 Forum) T-11 lecture text, Cypress Semiconductor Corporation's application note AN2292, etc.

[0309] Example

[0310] Hereinafter, the present invention will be further described in detail using examples.

[0311] The materials, dosage, ratio, processing content, processing sequence etc. shown in the following examples can be appropriately changed as long as they do not depart from the purpose of the present invention. Therefore, the scope of the present invention is not interpreted restrictively by the specific examples shown below. It should be noted that, as long as there is no special explanation, "%" and "part" are mass references.

[0312] [Example 1]

[0313] - Preparation of the photosensitive film of the present invention -

[0314] <Preparation of the Photosensitive Film L1 for Forming Decorative Layer, ie, the Photosensitive Film of Example 1>

[0315] Use a slit nozzle to apply a coating liquid for a thermoplastic resin layer composed of the following formula H1 on a temporary support of a polyethylene terephthalate film with a thickness of 75 μm, and let it dry. Next, apply a coating liquid for an intermediate layer composed of the following formula P1 and let it dry. Furthermore, apply a coating liquid for a white photocurable resin layer composed of the following formula L1 and let it dry. According to the above method, a thermoplastic resin layer with a dry film thickness of 15.1 μm, an intermediate layer with a dry film thickness of 1.6 μm, and a white photocurable resin layer with a dry film thickness of 35 μm are arranged on the temporary support, and finally a protective film (polypropylene film with a thickness of 12 μm) is crimped. In this way, a transfer material in which a temporary support, a thermoplastic resin layer, an intermediate layer (oxygen barrier film) and a white photocurable resin layer are integrated is prepared, and the sample is named as a photosensitive film L1 for forming a decorative layer (the photosensitive film of Example 1).

[0316] (Coating liquid for thermoplastic resin layer: Formulation H1)

[0317]

[0318] The fluorocarbon polymer is 40 parts of C6F 13 A copolymer of CH2CH2OCOCH=CH2, 55 parts of H(OCH(CH3)CH2)7OCOCH=CH2 and 5 parts of H(OCHCH2)7OCOCH=CH2, weight average molecular weight 30,000, 30% by mass solution of methyl ethyl ketone (trade name: Megafac F780F, manufactured by Dainippon Ink & Chemicals Co., Ltd.)

[0319] The viscosity of the thermoplastic resin layer coating liquid H1 after the solvent was removed at 120° C. was 1500 Pa·sec.

[0320] (Intermediate layer coating liquid: Formulation P1)

[0321]

[0322] (Coating liquid for white photocurable resin layer: Formulation L1)

[0323]

[0324] - Composition of white pigment dispersion 1 -

[0325] Titanium oxide (alumina treated rutile type, primary particle size 0.2μm

[0326] : 70.0% by mass

[0327] Random copolymer of benzyl methacrylate / methacrylic acid = 72 / 28 molar ratio, weight average molecular weight 37,000): 3.5% by mass

[0328] Methyl ethyl ketone (manufactured by Tonen Chemical Co., Ltd.): 26.5% by mass

[0329] <Evaluation of the Decorative Layer Forming Photosensitive Film L1, ie, the Photosensitive Film of Example 1>

[0330] (Evaluation of transferability)

[0331] The cover film of the photosensitive film L1 (photosensitive film of Example 1) for forming a decorative layer prepared in the above manner was peeled off, and after lamination using a laminator, the temporary support made of polyethylene terephthalate film was peeled off, and the film surface after peeling was observed and evaluated according to the following criteria. C or above is a practical level.

[0332] <Evaluation Criteria>

[0333] A: The transfer is complete over the entire surface, and the transferability is extremely good.

[0334] B: There is only a small amount of transfer residue at the edge of the film, and the transferability is good.

[0335] C: There is a little transfer residue on the entire film, and the transferability is average.

[0336] D: Film-like transfer residues of the photosensitive resin exist in various places on the film, and the transferability is poor.

[0337] The evaluation results are shown in Table 1 below.

[0338] -Manufacturing of the electrostatic capacitance input device of the present invention-

[0339] The photosensitive film of Example 1 obtained as described above was used as a photosensitive film for forming a decorative layer, and the electrostatic capacitance input device of Example 1 was manufactured.

[0340] Formation of the decorative layer

[0341] A tempered glass (300 mm×400 mm×0.7 mm) having an opening (15 mm Φ) was sprayed with a glass cleaning agent adjusted to 25° C. for 20 seconds, and then cleaned with a rotating brush having nylon bristles. After pure water spray cleaning, a silane coupling liquid (0.3% by mass aqueous solution of N-β-aminoethyl)γ-aminopropyltrimethoxysilane, trade name: KBM603, manufactured by Shin-Etsu Chemical Co., Ltd.) was sprayed with a silane coupling liquid for 20 seconds, and then pure water spray cleaning was performed. The substrate was heated at 140° C. for 2 minutes using a substrate preheating device. The cover film was removed from the obtained photosensitive film L1 for forming a decorative layer (photosensitive film of Example 1), and the surface of the white photocurable resin layer exposed after the removal was contacted with the surface of the silane coupling treated glass substrate, and laminated on the substrate heated at 120° C. using a laminator (Lamic II model, manufactured by Hitachi Industries, Ltd.) at a rubber roller temperature of 120° C., a linear pressure of 100 N / cm, and a conveying speed of 2.5 m / min. Next, the temporary support of polyethylene terephthalate was peeled off at the interface with the thermoplastic resin layer, and the temporary support was removed. After peeling off the temporary support, a proximity exposure machine with an ultra-high pressure mercury lamp (manufactured by Hitachi High-Tech Electronics Engineering Co., Ltd.) was used to vertically stand the substrate and the exposure mask (quartz exposure mask with a frame pattern), and the distance between the exposure mask surface and the white photocurable resin layer was set to 500 μm. The exposure amount was 1000 mJ / cm 2 (i-ray) for pattern exposure.

[0342] Next, a triethanolamine-based developer (containing 30% by mass of triethanolamine, a solution prepared by diluting the trade name: T-PD2 (manufactured by Fujifilm Corporation) to 10 times with pure water) was spray developed at 30° C. with a flat nozzle pressure of 0.1 MPa for 60 seconds to remove the thermoplastic resin layer and the intermediate layer. Next, air was blown onto the upper surface of the glass substrate to control the liquid, and then pure water was sprayed for 10 seconds to perform pure water spray cleaning, and air was blown to reduce the liquid accumulation on the substrate.

[0343] Then, a sodium carbonate / sodium bicarbonate-based developer (a solution prepared by diluting trade name: T-CD1 (manufactured by Fujifilm Corporation) to 5 times with pure water) was used, and the spray pressure was set to 0.1 MPa at 35° C., and the time (hereinafter referred to as the breakpoint) at which the unexposed portion can be completely developed was determined, and development was performed for 1.5 times the development time, and then washed with pure water. The breakpoint of the photosensitive film LI for forming a decorative layer (the photosensitive film of Example 1) was 110 seconds.

[0344] Next, a cleaning solution containing a surfactant (a solution obtained by diluting the trade name: T-SD3 (manufactured by Fujifilm Corporation) to 10 times with pure water) was sprayed at 33°C with a cone nozzle pressure of 0.1 MPa for 44 seconds, and then the formed pattern image was wiped with a rotating brush having soft nylon hair to remove the residue. Furthermore, ultrapure water was sprayed at a pressure of 8 MPa using an ultra-high pressure cleaning nozzle to remove the residue, and the water was removed by air knife control, and the oven was dried at 80°C for 10 minutes.

[0345] Next, the substrate was exposed to light at an exposure dose of 1300 mJ / cm from the front and back of the substrate. 2 After post-exposure, a post-baking treatment was performed at 240°C for 30 minutes in a vacuum oven under the condition of 15 mmHg or less, to obtain a front panel with a decorative layer having a thickness of 35 μm. The lightness was measured from the surface of the front panel without the decorative layer, and the L value was 83.4. In addition, the whiteness was judged by naked eye observation, and the result was no problem and was at a good level.

[0346] (Film thickness measurement)

[0347] In the front panel having the decorative layer formed on the tempered glass, the film thickness of the decorative layer was measured using a surface roughness meter P-10 (manufactured by TENCOR). The results are shown in Table 1 below.

[0348] 《Evaluation of front panels with decorative layers》

[0349] (Network structure evaluation)

[0350] After the front panel with the decorative layer formed on the tempered glass was placed in an environment of 23°C and 50% relative humidity for 24 hours, the surface of the decorative layer of the front panel and the surface opposite to the surface with the decorative layer formed were observed under a microscope using reflected light and transmitted light, and evaluated according to the following criteria. C and above are practical level.

[0351] <Evaluation Criteria>

[0352] A: No fine "wrinkles" were observed on the decorative layer pattern surface, which was extremely good.

[0353] B: Very weak "wrinkles" were observed only in the center of the decorative layer pattern surface, but they were not recognized from the surface opposite to the surface on which the decorative layer was formed, which was good.

[0354] C: A small amount of fine "wrinkles" etc. were observed on the surface of the decorative layer pattern, but they were not recognizable from the side opposite to the side on which the decorative layer was formed. This is a level that poses no practical problem and is considered average.

[0355] D: A considerable amount of fine "wrinkles" and the like were observed, and slight unevenness was also observed on the opposite side of the surface on which the decorative layer was formed, which was a poor level.

[0356] E: Generation of fine "wrinkles" and the like was confirmed over the entire surface, and unevenness was also observed on the surface opposite to the surface on which the decorative layer was formed, which was a very poor level.

[0357] The evaluation results are shown in Table 1 below.

[0358] (Evaluation of Yield)

[0359] 500 front panels having a decorative layer formed on tempered glass were produced, and the yield of usable front panels was examined.

[0360] <Evaluation Criteria>

[0361] A: The yield exceeded 94%, which is a very good level.

[0362] B: The yield was 91% or more and less than 94%, which was a good level.

[0363] C: The yield is 88% or more and less than 91%, which is fair.

[0364] D: The yield was 83% or more and less than 88%, which was poor.

[0365] E: The yield was less than 83%, which was very poor.

[0366] The evaluation results are shown in Table 1 below.

[0367] (Evaluation of Adhesion of Decorative Layer)

[0368] According to JIS K 5600-5-6: ISO2409 (cross-hatch method), a 1 mm wide cut is made on the decorative layer of the front panel having a decorative layer formed on tempered glass, and the decorative layer is peeled off with a cellophane tape to observe whether there is peeling or pinholes on the surface of the decorative layer. C and above are practical level.

[0369] <Evaluation Criteria>

[0370] A: The decorative layer component was not peeled off at all and adhered at a very good level.

[0371] B: There is only a slight peeling of the decorative layer component at the cut edge, but there is no checkered part at all, which is a good level.

[0372] C: The peeling of the decorative layer component is 0% or more and less than 2%, which is a practical level and is average.

[0373] D: The lattice peeling of the decorative layer component is 2% or more and less than 5%. The lattice peeling of the decorative layer component is confirmed and repair is necessary for practical use. Poor.

[0374] E: Peeling of 5% or more of the grid decorative layer components was observed, and repair was necessary for practical use. This was very poor.

[0375] The evaluation results are shown in Table 1 below.

[0376] (Development residue evaluation)

[0377] After the decorative layer was developed, the contour and peripheral portion of the formed decorative pattern were observed by SEM, and the following criteria were used to evaluate whether residues remained in the contour and peripheral portion. The practical level was C or higher.

[0378] <Evaluation Criteria>

[0379] A: No residue was observed at all, and the residue was extremely good.

[0380] B: Slight residue was observed only in the outline of the decorative pattern, and the residue was good.

[0381] C: Although a small amount of residue was observed in the outline of the decorative pattern, no residue was observed in other parts, and the level was practically no problem. The residue was normal.

[0382] D: A large amount of residue is observed in the outline of the decorative pattern, or residue is observed not only around the decorative pattern but also on the substrate outside the decorative pattern, poor.

[0383] E: Residues were observed over the entire surface of the substrate, and the residue was very poor.

[0384] The evaluation results are shown in Table 1 below.

[0385] (Uneven evaluation)

[0386] 60 people observed the decorative layer formed on the tempered glass from the front and back of the substrate, and evaluated the unevenness according to the following evaluation criteria. The practical level was C or higher.

[0387] <Evaluation Criteria>

[0388] A: The number of people who recognized the unevenness was 0 to 1

[0389] B: 2 to 3 people were identified as having uneven numbers

[0390] C: 4 to 5 people were identified as having uneven numbers

[0391] D: 6 to 10 people identified the unevenness

[0392] E: More than 11 people were identified as having uneven numbers

[0393] The evaluation results are shown in Table 1 below.

[0394] (Evaluation of Opening Contamination)

[0395] The opening of the front panel having the decorative layer formed on the tempered glass was observed under a microscope to check whether components of the decorative layer were present as contamination.

[0396] <Evaluation Criteria>

[0397] A: There is no contamination of the decorative layer component at the opening, which is extremely good.

[0398] B: Slight contamination of the decorative layer component was observed only at the edge of the opening, but the sample was usable and good.

[0399] C: Contamination of the decorative layer component of about several μm was observed from the edge of the opening to the inside of the opening, but it is practically usable and is fair.

[0400] D: Contamination of the decorative layer component is confirmed from the edge of the opening to the inside of the opening up to half the thickness of the glass. Repair is necessary for practical purposes. Poor.

[0401] E: Contamination of the decorative layer component was observed from the edge of the opening through the inside of the opening to the back side of the glass, which was very poor.

[0402] The evaluation results are shown in Table 1 below.

[0403] (Evaluation of opening defects)

[0404] The periphery of the opening of the front panel having the decorative layer formed on the tempered glass was observed under a microscope to check whether there was peeling of the decorative layer component or pinholes.

[0405] <Evaluation Criteria>

[0406] A: There is no peeling of the decorative layer component of the substrate near the opening, which is a very good level.

[0407] B: There is only a slight peeling at the edge of the opening, and there is no peeling at all in other parts, which is a good level.

[0408] C: Peeling of the decorative layer component of several μm around the edge of the opening was observed, but it was practically usable and was considered average.

[0409] D: Peeling of the decorative layer component was observed in a width of several mm around the opening, and repair was necessary for practical purposes. Poor.

[0410] E: Peeling of the decorative layer component was observed in a width of several centimeters around the opening, and repair was necessary for practical purposes. This was very poor.

[0411] 《Formation of mask layer》

[0412] <Preparation of Photosensitive Film K1 for Mask Layer Formation>

[0413] In the preparation of the photosensitive film L1 for forming a decorative layer (the photosensitive film of Example 1), except that the coating liquid for the white photocurable resin layer is replaced by the coating liquid for forming a mask layer composed of the following formula K1, a photosensitive film K1 for forming a mask layer (the film thickness of the mask layer photocurable resin layer is 2.2 μm) is obtained in the same manner as the preparation of the photosensitive film L1 for forming a decorative layer (the photosensitive film of Example 1).

[0414] (Coating liquid for black photocurable resin layer)

[0415]

[0416]

[0417] - Composition of K pigment dispersion 1 -

[0418]

[0419] [Chemical formula 1]

[0420]

[0421] - Composition of R pigment dispersion 1 -

[0422] Pigment (CI Pigment Red 177): 18% by mass

[0423] Binder 1 (random copolymer of benzyl methacrylate / methacrylic acid = 72 / 28 molar ratio, weight average molecular weight 37,000): 12 mass%

[0424] Propylene glycol monomethyl ether acetate: 70% by mass

[0425] <Formation of Mask Layer>

[0426] The front panel with the decorative layer formed thereon was cleaned in the same manner as the formation of the decorative layer, and the etching photosensitive film K1 with the cover film removed was laminated (substrate temperature: 140°C, rubber roller temperature 130°C, line pressure 100N / cm, conveying speed 2.2m / min). After peeling off the temporary support, the distance between the exposure mask (quartz exposure mask with a transparent electrode pattern) and the etching photocurable resin layer was set to 200μm, and the exposure amount was 70mJ / cm 2(i-ray) for pattern exposure.

[0427] Next, a triethanolamine-based developer (containing 30% triethanolamine, a solution obtained by diluting trade name: T-PD2 (manufactured by Fujifilm Corporation) to 10 times with pure water) was used for development at 33°C for 600 seconds, and then a sodium carbonate / sodium bicarbonate-based developer (a solution obtained by diluting trade name: T-CD1 (manufactured by Fujifilm Corporation) to 5 times with pure water) was used for development at 32°C with the spray pressure set to 0.1 MPa, and the film was washed with pure water for 45 seconds.

[0428] Next, a cleaning solution containing a surfactant (a solution prepared by diluting the trade name: T-SD3 (manufactured by Fujifilm Corporation) to 10 times with pure water) was sprayed at 33°C with a cone-shaped nozzle pressure of 0.1 MPa for 20 seconds, and then the formed pattern image was wiped with a rotating brush having soft nylon hair to remove the residue. Furthermore, ultrapure water was sprayed at a pressure of 9.8 MPa using an ultra-high pressure cleaning nozzle to remove the residue.

[0429] Next, the substrate was exposed to light at an exposure dose of 1300 mJ / cm from the front and back of the substrate in the atmosphere. 2 Post-exposure was performed, and then post-baking treatment was performed at 240° C. for 80 minutes to obtain a front panel having a mask layer with an optical density of 4.0 and a film thickness of 2.0 μm and a decorative layer formed in this order.

[0430] 《Evaluation of front panels with decorative layers and mask layers》

[0431] (Evaluation of brightness)

[0432] In the front panel having a decorative layer and a mask layer formed on tempered glass, black paper was placed on the surface opposite to the surface having the decorative layer formed, and the lightness was evaluated based on the L value using a 938 Spectrodensitometer manufactured by X-Rite. The practical level is D or higher, preferably C or higher.

[0433] A: L value is 83 or above

[0434] B: L value is 82 or more and less than 83

[0435] C: L value is 80 or more and less than 82

[0436] D: L value is 77 or more and less than 80

[0437] E: L value is less than 77

[0438] The evaluation results are shown in Table 1 below.

[0439] (Evaluation of whiteness)

[0440] 60 people were asked to observe the front panel having the decorative layer and the mask layer formed on the tempered glass from the front and back of the substrate, and the whiteness was evaluated according to the following evaluation criteria. The practical level was C or higher.

[0441] <Evaluation Criteria>

[0442] A: The number of people who can identify yellowing is 0 to 1

[0443] B: 2 to 3 people with yellow spots were identified

[0444] C: 4 to 5 people with yellow spots

[0445] D: 6 to 10 people with yellow spots

[0446] E: More than 11 people were identified with yellow

[0447] The evaluation results are shown in Table 1 below.

[0448] 《Formation of the first transparent electrode pattern》

[0449] <Formation of Transparent Electrode Layer>

[0450] The front panel with the mask layer formed was introduced into a vacuum chamber, and an ITO target (indium: tin = 95:5 (molar ratio)) with a SnO2 content of 10% by mass was used to form an ITO film with a thickness of 40nm by DC magnetron sputtering (conditions: substrate temperature 250°C, argon pressure 0.13Pa, oxygen pressure 0.01Pa), thereby obtaining a front panel with a transparent electrode layer formed thereon. The surface resistance of the ITO film was 80Ω / □.

[0451] <Preparation of Photosensitive Film E1 for Etching>

[0452] In the preparation of the photosensitive film L1 for forming the decorative layer, except that the coating liquid for the white photocurable resin layer is replaced by the coating liquid for the etching photocurable resin layer composed of the following formula E1, the photosensitive film E1 for etching (the film thickness of the etching photocurable resin layer is 2.0 μm) is obtained in the same manner as the preparation of the photosensitive film L1 for forming the decorative layer.

[0453] (Coating liquid for photocurable resin layer for etching: Formulation E1)

[0454]

[0455]

[0456] <Formation of First Transparent Electrode Pattern>

[0457] In the same manner as the formation of the decorative layer, the front panel with the transparent electrode layer formed thereon was cleaned and the etching photosensitive film E1 was laminated after the cover film was removed (substrate temperature: 130°C, rubber roller temperature 120°C, line pressure 100N / cm, conveying speed 2.2m / min). After peeling off the temporary support, the distance between the exposure mask (quartz exposure mask with a transparent electrode pattern) surface and the etching photocurable resin layer was set to 200μm, and the exposure amount was 50mJ / cm 2 (i-ray) for pattern exposure.

[0458] Next, a triethanolamine-based developer (containing 30% triethanolamine by mass, a solution obtained by diluting trade name: T-PD2 (manufactured by Fujifilm Corporation) to 10 times with pure water) was used for treatment at 25°C for 100 seconds, and then a surfactant-containing cleaning solution (a solution obtained by diluting trade name: T-SD3 (manufactured by Fujifilm Corporation) to 10 times with pure water) was used for treatment at 33°C for 20 seconds. Residues were removed using a rotating brush and an ultra-high pressure cleaning nozzle, and then a post-baking treatment was performed at 130°C for 30 minutes to obtain a front panel having a transparent electrode layer and an etching photocurable resin layer pattern formed thereon.

[0459] The front panel formed with the transparent electrode layer and the etching photocurable resin layer pattern is immersed in an etching tank added with ITO etchant (hydrochloric acid, potassium chloride aqueous solution; liquid temperature 30°C) for 100 seconds to dissolve and remove the transparent electrode layer in the exposed area not covered by the etching photocurable resin layer, thereby obtaining a front panel with a transparent electrode layer pattern attached with the etching photocurable resin layer pattern.

[0460] Next, the front panel with a transparent electrode layer pattern to which an etching photocurable resin layer pattern is attached is immersed in a resist stripping tank to which a resist stripping solution (N-methyl-2-pyrrolidone, monoethanolamine, and a surfactant (trade name: Surfynol 465, manufactured by Air Products), liquid temperature 45° C.) is added, and the treatment is performed for 200 seconds to remove the etching photocurable resin layer, thereby obtaining a front panel having a decorative layer, a mask layer, and a first transparent electrode pattern formed thereon, wherein the first transparent electrode pattern is arranged over the non-contact surface of the front panel and two areas of the surface of the mask layer opposite to the front panel.

[0461] 《Formation of the insulating layer》

[0462] <Preparation of Photosensitive Film W1 for Insulating Layer Formation>

[0463] In the preparation of the photosensitive film L1 for forming a decorative layer, except that the coating liquid for the white photocurable resin layer is replaced by the coating liquid for the insulating layer photocurable resin layer composed of the following formula W1, the photosensitive film W1 for forming an insulating layer is obtained in the same manner as the preparation of the photosensitive film L1 for forming a decorative layer (the film thickness of the photocurable resin layer for the insulating layer is 1.4 μm).

[0464] (Coating liquid for forming insulating layer: Formulation W1)

[0465]

[0466] The viscosity of the insulating layer forming coating liquid W1 at 100° C. after the solvent was removed was 4000 Pa·sec.

[0467] In the same manner as the formation of the decorative layer, the front panel with the first transparent electrode pattern was cleaned and silane-coupled, and the photosensitive film W1 for insulating layer formation after removing the cover film was laminated (substrate temperature: 100°C, rubber roller temperature 120°C, line pressure 100N / cm, conveying speed 2.3m / min). After peeling off the temporary support, the distance between the exposure mask (quartz exposure mask with an insulating layer pattern) and the etching photocurable resin layer was set to 100μm, and the exposure amount was 30mJ / cm 2 (i-ray) for pattern exposure.

[0468] Next, a triethanolamine-based developer (containing 30% triethanolamine by mass, a solution obtained by diluting trade name: T-PD2 (manufactured by Fujifilm Corporation) to 10 times with pure water) was used for treatment at 33°C for 60 seconds, a sodium carbonate / sodium bicarbonate-based developer (a solution obtained by diluting trade name: T-CD1 (manufactured by Fujifilm Corporation) to 5 times with pure water) was used for treatment at 25°C for 50 seconds, and then a surfactant-containing cleaning solution (a solution obtained by diluting trade name: T-SD3 (manufactured by Fujifilm Corporation) to 10 times with pure water) was used for treatment at 33°C for 20 seconds, and residues were removed using a rotating brush and an ultra-high pressure cleaning nozzle, followed by a post-baking treatment at 230°C for 60 minutes to obtain a front panel having a decorative layer, a mask layer, a first transparent electrode pattern, and an insulating layer pattern formed thereon.

[0469] 《Formation of the second transparent electrode pattern》

[0470] <Formation of Transparent Electrode Layer>

[0471] In the same manner as the formation of the first transparent electrode pattern, the front panel formed with the first transparent electrode pattern and the insulating layer pattern was subjected to DC magnetron sputtering treatment (conditions: substrate temperature 50°C, argon pressure 0.13Pa, oxygen pressure 0.01Pa), to form an ITO film with a thickness of 80nm, and obtain a front panel formed with a transparent electrode layer. The surface resistance of the ITO film is 110Ω / □.

[0472] In the same manner as the formation of the first transparent electrode pattern, the etching photosensitive film E1 was used to obtain a front panel having a first transparent electrode pattern, an insulating layer pattern, a transparent electrode layer, and an etching photocurable resin layer pattern (post-baking treatment, 130° C., 30 minutes).

[0473] Furthermore, etching is performed in the same manner as the formation of the first transparent electrode pattern (30° C., 50 seconds), and the etching photocurable resin layer is removed (45° C., 200 seconds), thereby obtaining a front panel formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, and a second transparent electrode pattern, wherein the second transparent electrode pattern is arranged over two areas of the non-contact surface of the front panel and the surface of the mask layer on the opposite side of the front panel.

[0474] 《Formation of other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern》

[0475] In the same manner as the formation of the first transparent electrode pattern and the second transparent electrode pattern, the front panel having the first transparent electrode pattern, the insulating layer pattern and the second transparent electrode pattern is subjected to DC magnetron sputtering treatment to obtain a front panel having an aluminum (Al) thin film with a thickness of 200 nm.

[0476] In the same manner as the formation of the first transparent electrode pattern and the second transparent electrode pattern, using the etching photosensitive film E1, a front panel having a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, and an etching photocurable resin layer pattern is obtained (post-baking treatment, 130°C, 30 minutes).

[0477] Furthermore, etching is performed in the same manner as the formation of the first transparent electrode pattern (30°C, 50 seconds), and the etching photocurable resin layer is removed (45°C, 200 seconds), thereby obtaining a front panel having a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, and other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern.

[0478] 《Formation of a transparent protective layer》

[0479] In the same manner as the formation of the insulating layer, a photosensitive film W1 for forming an insulating layer was laminated on the front panel having other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, from which the cover film was removed, and after peeling off the temporary support, an exposure amount of 50 mJ / cm was applied without using an exposure mask. 2 (i-ray) for front exposure, development, and post exposure (1000mJ / cm 2 ), and post-baking treatment to obtain a front panel 1 on which an insulating layer (transparent protective layer) is stacked in a manner covering all of the mask layer, the first transparent electrode pattern, the insulating layer pattern, the second transparent electrode pattern, and other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern. The obtained front panel 1 is used as the electrostatic capacitance input device of Example 1.

[0480] 《Production of Image Display Device (Touch Panel)》

[0481] The previously manufactured front panel 1 (capacitive input device of Example 1) is bonded to a liquid crystal display element manufactured by the method described in Japanese Patent Application Laid-Open No. 2009-47936, and the image display device 1 of Example 1 having the capacitive input device as a constituent element is manufactured by a known method.

[0482] 《Overall evaluation of front panel 1 and image display device 1》

[0483] In each of the above steps, the front panel 1 (the electrostatic capacitance input device of Example 1) on which a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, and other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern are formed has no contamination at the opening and the back side, is easy to clean, and does not cause contamination of other components.

[0484] In addition, there are no pinholes on the decorative layer, and there are no problems with whiteness or unevenness. There are also no pinholes on the mask layer, and the light shielding property is excellent.

[0485] Furthermore, the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different from these have no problem in their respective conductivity, while on the other hand, the first transparent electrode pattern and the second transparent electrode pattern have insulation properties.

[0486] Furthermore, there are no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics is obtained.

[0487] [Example 2]

[0488] 《Production of photosensitive film C1 laminated with conductive photocurable resin layer》

[0489] In the preparation of the photosensitive film L1 for forming a decorative layer, except that the coating liquid for the white photocurable resin layer is replaced by the coating liquid for forming a conductive photocurable resin layer composed of the following formula C1, a photosensitive film C1 laminated with a conductive photocurable resin layer is obtained in the same manner as the preparation of the photosensitive film L1 for forming a decorative layer (the film thickness of the conductive photocurable resin layer is 2.0 μm).

[0490] <Preparation of coating liquid for forming conductive photocurable resin layer>

[0491] (Preparation of Silver Nanowire Dispersion (1))

[0492] A silver nitrate solution was prepared by dissolving 0.51 g of silver nitrate powder in 50 mL of pure water. Then, 1N ammonia water was added to the silver nitrate solution until it became transparent, and pure water was added to make the total amount 100 mL, thereby preparing an additive solution A.

[0493] Separately, 0.5 g of glucose powder was dissolved in 140 mL of pure water to prepare additive solution G.

[0494] Furthermore, 0.5 g of HTAB (hexadecyl-trimethylammonium bromide) powder was dissolved in 27.5 mL of pure water to prepare an additive solution H.

[0495] Next, 20.6 mL of the additive solution A was added to a three-necked flask and stirred at room temperature. 41 mL of pure water, 20.6 mL of the additive solution H, and 16.5 mL of the additive solution G were added to the solution in sequence using a funnel, and the mixture was heated while being stirred at 200 rpm at 90° C. for 5 hours to obtain a silver nanowire aqueous dispersion (1).

[0496] After cooling the obtained silver nanowire water dispersion (1), polyvinyl pyrrolidone (trade name: K-30, manufactured by Wako Pure Chemical Industries, Ltd.) was added while stirring in an amount of 0.05 relative to the mass 1 of silver, and then centrifuged to purify until the conductivity becomes 50 μS / cm or less. Propylene glycol monomethyl ether was further centrifuged to remove water, and finally propylene glycol monomethyl ether was added to prepare a silver nanowire solvent dispersion (1).

[0497] (Preparation of Coating Liquid C1 for Forming Conductive Photocurable Resin Layer)

[0498] The following composition was stirred and mixed with the silver nanowire dispersion (1) so that the final silver concentration became 1.0 mass %, thereby preparing a coating liquid C1 for forming a conductive photocurable resin layer.

[0499] - Composition of the coating liquid C1 for forming a conductive photocurable resin layer-

[0500]

[0501] 《Formation of transparent electrode patterns and insulating layers, etc.》

[0502] After obtaining a front panel having a decorative layer and a mask layer formed thereon in the same manner as in Example 1, a first transparent electrode pattern was formed using a photosensitive film C1 having a conductive photocurable resin layer laminated thereon.

[0503] First, the front panel with the mask layer formed was cleaned, and the photosensitive film C1 after removing the cover film was laminated (substrate temperature: 120°C, rubber roller temperature 120°C, linear pressure 100N / cm, conveying speed 1.7m / min). After peeling off the temporary support, the distance between the exposure mask (quartz exposure mask with a transparent electrode pattern) and the conductive photocurable resin layer was set to 100μm, and the exposure amount was 100mJ / cm 2 (i-ray) for pattern exposure.

[0504] Next, a triethanolamine-based developer (containing 30% by mass of triethanolamine, a solution obtained by diluting trade name: T-PD2 (manufactured by Fujifilm Corporation) to 10 times with pure water) was used for treatment at 30°C for 60 seconds, a sodium carbonate / sodium bicarbonate-based developer (a solution obtained by diluting trade name: T-CD1 (manufactured by Fujifilm Corporation) to 5 times with pure water) was used for treatment at 25°C for 60 seconds, and then a surfactant-containing cleaning solution (a solution obtained by diluting trade name: T-SD3 (manufactured by Fujifilm Corporation) to 10 times with pure water) was used for treatment at 33°C for 20 seconds, and residues were removed using a rotating brush and an ultra-high pressure cleaning nozzle, followed by a post-baking treatment at 230°C for 60 minutes to obtain a front panel having a mask layer and a first transparent electrode pattern formed thereon.

[0505] Next, an insulating layer was formed in the same manner as in Example 1. Next, a second transparent electrode pattern was formed using a photosensitive film C1 laminated with a conductive photocurable resin layer. Furthermore, another conductive element different from the first transparent electrode pattern and the second transparent electrode pattern and a transparent protective layer were formed in the same manner as in Example 1 to obtain a front panel 2. This front panel 2 was used as the electrostatic capacitance input device of Example 2.

[0506] In addition, in the same manner as in Example 1, an image display device 2 of Example 2 was produced.

[0507] 《Evaluation of front panel 2 and image display device 2》

[0508] In each of the above steps, the front panel 2 formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, and other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern has no contamination at the opening and the back side, is easy to clean, and has no problem of contamination of other components.

[0509] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0510] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0511] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0512] [Example 3 and Example 4]

[0513] In Example 1, the photosensitive films for forming the decorative layer of Example 3 and Example 4 were prepared in the same manner as in Example 1, except that the coating liquid formulation L3 and the coating liquid formulation L4 for the white photocurable resin layer were used instead of the coating liquid formulation L1 for the white photocurable resin layer, and the monomer / binder ratio was changed to that shown in Table 1. The front panel having the decorative layer formed thereon was evaluated in the same manner as in Example 1, except that the prepared photosensitive films for forming the decorative layer of Example 3 and Example 4 were used, and the evaluation results are described in the following Table 1. Then, the electrostatic capacitive input devices of Example 3 and Example 4, i.e., the front panel 3 and the front panel 4, and the image display device 3 and the image display device 4 having the electrostatic capacitive input device as a constituent element, were prepared in the same manner as in Example 1.

[0514] Compared with the front panel 1, the brightness, whiteness, unevenness, opening contamination, mesh structure, yield, etc. of the front panel 3 are slightly lower, but are at a practical level. The adhesion of the decorative layer, development residue, and opening defects are improved.

[0515] On the other hand, compared with the front panel 1, the front panel 4 has slightly lower decoration layer adhesion, development residue, opening defects, etc., but is at a practical level, and the brightness, whiteness, unevenness, opening contamination, network structure, and yield are improved.

[0516] The front panels 3 and 4 have no problem with contamination of the openings and the backs, are easy to clean, and do not have the problem of contamination of other components.

[0517] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0518] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0519] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0520] [Example 5 to Example 10]

[0521] In Example 1, photosensitive films for forming decorative layers of Examples 5 to 10 were prepared in the same manner as in Example 1, except that the white photocurable resin layer coating liquid formulations L5 to L10 were used instead of the white photocurable resin layer coating liquid formulation L1, and the titanium oxide content / solid content ratio was changed to that shown in Table 1. The front panels on which the decorative layers were formed were evaluated in the same manner as in Example 1, except that the prepared photosensitive films for forming decorative layers of Examples 5 to 10 were used, and the evaluation results are described in the following Table 1. Then, in the same manner as in Example 1, electrostatic capacitive input devices of Examples 5 to 10, i.e., front panels 5 to 10, on which the decorative layer, mask layer, first transparent electrode pattern, insulating layer pattern, second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and transparent protective layer were formed, and image display devices 5 to 10 having the electrostatic capacitive input device as a constituent element were prepared.

[0522] As the ratio of titanium oxide to the total solid content increases, the adhesion of the decorative layer, the developer residue, the opening defects, etc. of the front panels 5 to 10 are slightly reduced, but at a practical level, the whiteness, unevenness, the opening pollution, the mesh structure, and the yield are improved. In addition, the evaluation results of the brightness are also at a practical level. There is no problem with the pollution of the opening and the back of these front panels, and they are easy to clean, and there is no problem of pollution of other parts.

[0523] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0524] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0525] Furthermore, there are no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics is obtained.

[0526] [Example 11 and Example 12]

[0527] In Example 1, the photosensitive films for forming the decorative layer of Examples 11 and 12 were prepared in the same manner as in Example 1, except that the coating liquid formulations L11 (Example 11, initiator, IRGACURE 127 manufactured by BASF Japan Co., Ltd.) and L12 (Example 12, initiator, Lunar 6 manufactured by DKSH Japan Co., Ltd.) for the white photocurable resin layer were used instead of the coating liquid formulation L1, and the initiator type, initiator / monomer ratio, and exposure amount were changed to those shown in Table 1. The front panel having the decorative layer formed thereon was evaluated in the same manner as in Example 1, except that the prepared photosensitive films for forming the decorative layer of Examples 11 and 12 were used, respectively. The evaluation results are recorded in Table 1 below. Then, in the same manner as in Example 1, capacitive input devices of Example 11 and Example 12, namely, front panels 11 and 12, and image display devices 11 and 12 having capacitive input devices as constituent elements, are manufactured, wherein the devices have a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer.

[0528] The front panels 11 and 12 have no problem with contamination at the openings and the backs thereof, are easy to clean, and do not cause contamination of other components.

[0529] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0530] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0531] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0532] [Example 13 and Example 14]

[0533] In Example 1, the photosensitive films for forming the decorative layer of Examples 13 and 14 were prepared in the same manner as in Example 1, except that the primary particle size of the titanium oxide used in the white photocurable resin layer coating liquid formulation L1 was changed from 0.2 μm (white pigment dispersion 1) to 0.19 μm (Example 13, white pigment dispersion 2) and 0.25 μm (Example 14, white pigment dispersion 3), respectively. The front panel having the decorative layer formed thereon was evaluated in the same manner as in Example 1, except that the prepared photosensitive films for forming the decorative layer of Examples 13 and 14 were used, and the evaluation results are described in Table 1 below. Then, in the same manner as in Example 1, electrostatic capacitive input devices of Example 13 and Example 14, namely, front panels 13 and 14, and image display devices 13 and 14 having electrostatic capacitive input devices as constituent elements, are produced, each of which is provided with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer.

[0534] Compared with the front panel 1, the brightness and yield of the front panel 13 are slightly lower, but at a practical level, and the opening defects and opening contamination are improved. In addition, the evaluation results of the mesh structure, whiteness, unevenness, decorative layer adhesion, and development residue are also at a practical level.

[0535] The lightness, whiteness, yield, and decorative layer adhesion of the front panel 14 were slightly lower than those of the front panel 1, but were still at a practical level. The other evaluation results were also at a practical level.

[0536] These front panels have no problem with contamination of the opening and the back, are easy to clean, and do not have the problem of contamination of other parts.

[0537] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0538] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0539] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0540] [Example 15]

[0541] In Example 1, the photosensitive film for forming the decorative layer of Example 15 was prepared by using the coating liquid formulation L1 for the white photocurable resin layer and changing the thickness of the formed photocurable resin layer from 35 μm to 17.5 μm.

[0542] In the same manner as in Example 1, on a silane coupling treated glass substrate, the covering film is removed from the obtained photosensitive film for forming a decorative layer (photosensitive film of Example 15), and laminated using a laminator. Next, the temporary support of polyethylene terephthalate is peeled off at the interface with the thermoplastic resin layer, and the temporary support is removed. Hereinafter, a decorative layer is formed in the same manner as in Example 1, and the front panel formed with the decorative layer is evaluated, and the evaluation results are recorded in the following Table 1. Then, in the same manner as in Example 1, an electrostatic capacitance type input device of Example 15, i.e., a front panel 15, and an image display device 15 having an electrostatic capacitance type input device as a constituent element, formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer, are manufactured.

[0543] Compared with the front panel 1, the brightness and yield of the front panel 15 are lower, but at a practical level, and the mesh structure, unevenness, decorative layer adhesion, development residue, opening defects, and opening contamination are improved. In addition, the evaluation results of whiteness are also at a practical level.

[0544] The front panel 15 has no problem with contamination of the opening and the back surface, is easy to clean, and does not cause contamination of other components.

[0545] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0546] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0547] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0548] [Example 16]

[0549] In Example 1, the coating liquid formulation L1 for a white photocurable resin layer was used, and the thickness of the photocurable resin layer to be formed was changed from 35 μm to 17.5 μm, thereby producing a photosensitive film 16 ′ for forming a decorative layer.

[0550] The cover film was removed from the obtained photosensitive film 16' for forming a decorative layer on the silane coupling treated glass substrate and laminated using a laminator in the same manner as in Example 1. Next, the temporary support of polyethylene terephthalate was peeled off at the interface with the thermoplastic resin layer and removed.

[0551] Next, a triethanolamine-based developer (containing 30% by mass of triethanolamine, a solution prepared by diluting T-PD2 (manufactured by Fujifilm Corporation) to 10 times with pure water) was sprayed for 60 seconds at 30° C. with a flat nozzle pressure of 0.1 MPa to remove the thermoplastic resin layer and the intermediate layer. Next, air was blown onto the upper surface of the glass substrate to control the liquid, and then pure water was sprayed for 10 seconds to perform pure water spray cleaning, and air was blown to reduce the liquid accumulation on the substrate. A silane coupling liquid (0.3% by mass aqueous solution of N-β-aminoethyl)γ-aminopropyltrimethoxysilane, trade name: KBM603, manufactured by Shin-Etsu Chemical Co., Ltd.) was sprayed for 20 seconds, and pure water was sprayed for cleaning. After drying at 100° C. for 5 minutes, the thickness of the decorative layer was set to 17.5 μm, and the cover film was removed from the photosensitive film 16 ′ for decorative layer formation, and laminated again by a laminator. Next, the temporary support of polyethylene terephthalate was removed. The thickness of the photocurable resin layer formed was set to 17.5 μm×2 layers, and a photosensitive film for forming a decorative layer of Example 16 was prepared. Hereinafter, a decorative layer was formed in the same manner as in Example 1, and the front panel formed with the decorative layer was evaluated, and the evaluation results are recorded in the following Table 1. Then, in the same manner as in Example 1, an electrostatic capacitance input device of Example 16, i.e., a front panel 16, and an image display device 16 having an electrostatic capacitance input device as a constituent element, formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer were prepared.

[0552] Compared with front panel 1, the yield, decoration layer adhesion, and opening defects of front panel 16 are slightly lower, but are at a practical level. In addition, the evaluation results of network structure, whiteness, unevenness, and development residue are also at a practical level.

[0553] The front panel 16 has no problem with contamination of the opening and the back surface, is easy to clean, and does not cause contamination of other components.

[0554] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0555] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0556] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0557] [Example 17]

[0558] In Example 1, a photosensitive film for forming a decorative layer of Example 17 was prepared by using a coating liquid formula L1 for a white photocurable resin layer, and the thickness of the formed layer was changed from 35 μm to 6 μm. A front panel 17' having a decorative layer was prepared in the same manner as in Example 1, except that the photosensitive film for forming a decorative layer of Example 17 prepared was used. Next, on the front panel 17', a white screen printing ink S1 was used to screen print the printing ink using a screen printer (manufactured by Mishima Co., Ltd.; UDF-5L, mesh size 250 μm), and it was dried at 100°C for 10 minutes to prevent it from sticking. The thickness of the ink was 6 μm. Screen printing was then performed in the same manner as above, and drying was performed at 100°C for 10 minutes. The printing to drying process was repeated a total of 4 times. Drying was performed at 150°C for 30 minutes, and the results of the evaluation of the front panel having a decorative layer are recorded in the following Table 1. Then, in the same manner as in Example 1, an electrostatic capacitive input device of Example 17, i.e., a front panel 17, and an image display device 17 having an electrostatic capacitive input device as a constituent element were produced, which were formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer.

[0559] (White screen printing ink: Formulation S1)

[0560] Benzyl methacrylate / methacrylic acid=78 / 22 random copolymer, weight average molecular weight 30,000, propylene glycol monomethyl ether acetate solution (solid content 40.5% by mass)

[0561] : 331 parts by mass

[0562] White pigment dispersion 1: 157 parts by mass

[0563] Surfactant (trade name: Megafac F-780F, manufactured by Dainippon Ink Co., Ltd.)

[0564] : 1.0 parts by mass

[0565] Compared with front panel 1, the brightness, decorative layer adhesion, yield, unevenness, and opening contamination of front panel 17 are slightly lower, but at a practical level, and the development residue is improved. In addition, the evaluation results of network structure, whiteness, opening defects, etc. are also at a practical level.

[0566] The front panel 17 has no problem with contamination of the opening and the back surface, is easy to clean, and does not cause contamination of other components.

[0567] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0568] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0569] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0570] [Example 18]

[0571] In Example 17, a coating liquid formula L1 for a white photocurable resin layer was used to change the thickness of the formed layer from 6 μm to 2 μm, and a photosensitive film for forming a decorative layer of Example 18 was prepared. A front panel 18' having a decorative layer was prepared in the same manner as in Example 1, except that the photosensitive film for forming a decorative layer of Example 18 prepared was used. Next, on the front panel 18', screen printing ink S1 was used to screen print the printing ink with a screen printer (made by Mishima Co., Ltd., UDF-5L, mesh size 250 μm), and it was dried at 100°C for 10 minutes to make it non-adhesive. The thickness of the ink was 6 μm. Screen printing was then performed in the same manner as above, and drying was performed at 100°C for 10 minutes. The printing to drying process was repeated a total of 5 times. The front panel having a decorative layer was evaluated by drying at 150°C for 30 minutes, and the evaluation results are recorded in Table 1 below. Then, in the same manner as in Example 1, an electrostatic capacitive input device of Example 18, i.e., a front panel 18, and an image display device 18 having an electrostatic capacitive input device as a constituent element, were produced, which were formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer.

[0572] Compared with the front panel 1, the brightness, mesh structure, unevenness, yield, decorative layer adhesion, opening defects, and opening contamination yield of the front panel 18 are lower, but at a practical level, and the development residue is improved. In addition, the evaluation results of whiteness are also at a practical level.

[0573] The front panel 18 has no problem with contamination of the opening and the back surface, is easy to clean, and does not cause contamination of other components.

[0574] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0575] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0576] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0577] [Example 19 and Example 20]

[0578] In Example 1, the photosensitive films for forming the decorative layer of Examples 19 and 20 were prepared in the same manner as in Example 1, except that the coating liquid formulation L19 (Example 19, initiator, IRGACURE OXE-01 manufactured by BASF Japan Co., Ltd.) and the coating liquid formulation L20 (Example 12, initiator, Lunar 6 manufactured by DKSH Japan Co., Ltd.) were used instead of the coating liquid formulation L1 for the white photocurable resin layer, and the initiator type, initiator / monomer ratio, and exposure amount were changed to those shown in Table 1. The front panel having the decorative layer formed thereon was evaluated in the same manner as in Example 1, except that the prepared photosensitive films for forming the decorative layer of Examples 19 and 20 were used, respectively, and the evaluation results are recorded in the following Table 1. Then, in the same manner as in Example 1, electrostatic capacitive input devices of Example 19 and Example 20, namely, front panels 19 and 20, which are formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer, and image display devices 19 and 20 having electrostatic capacitive input devices as constituent elements, were manufactured.

[0579] The front panels 19 and 20 have no problem with contamination of the openings and the back surfaces, are easy to clean, and do not cause contamination of other components.

[0580] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0581] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0582] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0583] [Comparative Example 1]

[0584] After the tempered glass (300mm×400mm×0.7mm) with an opening (15mmΦ) was cleaned with a UV cleaning device, it was brushed with a cleaning agent and then ultrasonically cleaned with ultrapure water. The substrate was heat treated at 120°C for 3 minutes to stabilize the surface state. After the substrate was cooled and the temperature was adjusted to 23°C, the coating liquid L1 for the white photocurable resin layer obtained in Example 1 was applied using a glass substrate coater with a slit nozzle (manufactured by FAS Japan Co., Ltd., trade name: MH-1600). The coating liquid L1 for the white photocurable resin layer flowed into the opening of the tempered glass, causing contamination of the opening and the back of the substrate. Next, a portion of the solvent was dried using a VCD (vacuum drying device, manufactured by Tokyo Ohka Industry Co., Ltd.) for 30 seconds to eliminate the fluidity of the coating layer, and then unnecessary coating liquid around the substrate was removed using an EBR (Edge Bead Remover). The coating was pre-baked at 120°C for 3 minutes to obtain a white photocurable resin layer L21 with a film thickness of 5.0 μm on the tempered glass (liquid resist method).

[0585] Using a proximity exposure machine with an ultra-high pressure mercury lamp (manufactured by Hitachi High-Tech Electronics Engineering Co., Ltd.), the substrate and the exposure mask (quartz exposure mask with a frame pattern) were vertically raised, and the distance between the exposure mask surface and the black photocurable resin layer L21 was set to 200 μm. In a nitrogen atmosphere, the white photocurable resin layer L21 was exposed to light at an exposure dose of 1000 mJ / cm 2 Perform pattern exposure.

[0586] Next, pure water was sprayed using a spray nozzle to evenly wet the surface of the white photocurable resin layer L21, and then a sodium carbonate / sodium bicarbonate-based developer (a solution prepared by diluting trade name: T-CD1 (manufactured by FUJIFILM Corporation) to 5 times with pure water) was used. The spray pressure was set to 0.1 MPa at 35°C, and the time for complete development of the unexposed part (hereinafter referred to as the breakpoint) was calculated. The unexposed part was developed at 1.5 times the development time and washed with pure water.

[0587] Furthermore, ultrapure water was sprayed at a pressure of 8 MPa using an ultrahigh pressure cleaning nozzle to remove residues, and then the substrate was exposed to light at an exposure dose of 1300 mJ / cm 2After post-exposure, a post-baking treatment was performed at 240°C for 30 minutes in a vacuum oven under the condition of 15 mmHg or less, thereby obtaining a front panel having a decorative layer formed thereon. The front panel having a decorative layer formed thereon was evaluated in the same manner as in Example 1, and the evaluation results are recorded in Table 1 below. Hereinafter, in the same manner as in Example 1, a capacitive input device, i.e., a front panel 21, of Comparative Example 1 having a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer, and an image display device 21 having a capacitive input device as a constituent element were prepared.

[0588] Compared with the front panel 1, the front panel 21 has contamination at the opening and the back surface, and must be cleaned, resulting in a significant decrease in yield and insufficient brightness.

[0589] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0590] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0591] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0592] [Comparative Example 2]

[0593] In Comparative Example 1, the coating liquid L1 for the white photocurable resin layer obtained in Example 1 was repeatedly coated 7 times to form 7 layers with a film thickness of 5.0 μm on the tempered glass, thereby obtaining a white photocurable resin layer L22 (liquid resist method). The front panel formed with the decorative layer was evaluated in the same manner as in Example 1, and the evaluation results are recorded in the following Table 1. Hereinafter, the electrostatic capacitance input device of Comparative Example 2, i.e., the front panel 22, and the image display device 22 having the electrostatic capacitance input device as a constituent element, formed with the decorative layer, the mask layer, the first transparent electrode pattern, the insulating layer pattern, the second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and the transparent protective layer, were prepared in the same manner as in Comparative Example 1.

[0594] Compared with the front panel 1, the front panel 22 has contamination in the opening and the back, which requires cleaning, greatly reduces the yield, and the brightness is insufficient. Compared with the front panel 21, the unevenness is further deteriorated, resulting in a low yield. It is a practical level. In addition, there are no pinholes on the mask layer, and the light-shielding property is excellent.

[0595] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0596] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0597] [Comparative Example 3]

[0598] A tempered glass (300 mm×400 mm×0.7 mm) formed with an opening (15 mm Φ) was cleaned with a rotating brush having nylon bristles while spraying and blowing a glass cleaning agent adjusted to 25° C. for 20 seconds, and then sprayed and washed with pure water. A silane coupling liquid (0.3 mass % aqueous solution of N-β (aminoethyl) γ-aminopropyltrimethoxysilane, trade name: KBM603, manufactured by Shin-Etsu Chemical Co., Ltd.) was sprayed and blown for 20 seconds, and then sprayed and washed with pure water. The substrate was heated at 110° C. for 10 minutes by a substrate preheating device, and then cooled to room temperature. The above-mentioned white screen printing ink S1 was used on the obtained silane coupling treated glass substrate, and the printing ink was screen printed by a screen printer (manufactured by Mishima Co., Ltd.; UDF-5L, mesh size 250 μm), and pre-baked and dried at 100° C. for 10 minutes to prevent adhesion. The ink had a thickness of 6 μm. The ink was then dried at 150° C. for 30 minutes as a final bake to obtain a white photocurable resin layer L23. It should be noted that the primary particle size of the titanium oxide particles used was 0.20 μm. The front panel formed with the decorative layer was evaluated, and the evaluation results are recorded in Table 1 below.

[0599] Then, the front panel formed with the decorative layer was evaluated in the same manner as in Example 1, and the evaluation results are recorded in the following Table 1. Next, the electrostatic capacitance input device of Comparative Example 3, i.e., the front panel 23, and the image display device 23 having the electrostatic capacitance input device as a constituent element, formed with the decorative layer, the mask layer, the first transparent electrode pattern, the insulating layer pattern, the second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and the transparent protective layer, were manufactured in the same manner as in Comparative Example 1.

[0600] Compared with front panel 1 , front panel 23 has lower brightness and opening defects, and its yield is lowered.

[0601] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0602] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0603] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0604] [Comparative Example 4]

[0605] In Comparative Example 3, screen printing and pre-baking were repeated 6 times, and final baking was performed to obtain a white photocurable resin layer L24 having 6 layers with a film thickness of 6.0 μm formed on the tempered glass. The front panel having the decorative layer formed thereon was evaluated in the same manner as in Example 1, and the evaluation results are recorded in the following Table 1. Then, in the same manner as in Comparative Example 1, a front panel 24 of a capacitive input device of Comparative Example 4 having a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer, and an image display device 24 having a capacitive input device as a constituent element were prepared.

[0606] Compared with the front panel 1, the brightness, mesh structure, unevenness, adhesion of the decorative layer, opening defects, and opening contamination of the front panel 24 are reduced, and the yield is reduced.

[0607] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0608] The opening and the back are free of contamination, easy to clean, and free of contamination from other parts.

[0609] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0610] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0611] [Example 21 and Example 22]

[0612] In Example 1, the photosensitive films for forming the decorative layer of Examples 21 and 22 were prepared in the same manner as in Example 1, except that the primary particle diameter of the titanium oxide used in the white photocurable resin layer coating liquid formulation L15 and L16 was changed to 0.17 μm (Example 21, white pigment dispersion 4) and 0.35 μm (Example 22, white pigment dispersion 5) respectively. The decorative layer was formed in the same manner as in Example 1, except that the prepared photosensitive films for forming the decorative layer of Examples 21 and 22 were used. The evaluation results of the front panel formed with the decorative layer are described in the following Table 1. Then, in the same manner as in Example 1, electrostatic capacitive input devices of Example 21 and Example 22, namely, front panels 25 and 26, and image display devices 25 and 26 having electrostatic capacitive input devices as constituent elements, were produced, each of which was formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer.

[0613] Compared with the front panel 1, the brightness and yield of the front panel 25 are reduced, but they are at a practical level, and the opening defects and the opening pollution are improved. In addition, the evaluation results of whiteness, mesh structure, unevenness, and developer residue are also at a practical level. There is no pollution in the opening and the back, it is easy to clean, and there is no problem of pollution of other parts.

[0614] Relative to front panel 1, the brightness, yield, and developer residue of front panel 26 decreased, but were at a practical level. In addition, the evaluation results of whiteness, mesh structure, unevenness, opening defect, and opening pollution were also at a practical level. Front panel 25 and front panel 26 had no problem with the pollution of the opening and the back, were easy to clean, and had no problem with the pollution of other components.

[0615] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0616] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0617] Furthermore, there are no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics is obtained.

[0618] [Comparative Example 5]

[0619] In Example 1, the coating liquid formulation L1 for a white photocurable resin layer was used, and the thickness of the formed layer was changed from 35 μm to 42 μm, so that a photosensitive film for forming a decorative layer of Comparative Example 5 was produced.

[0620] In the same manner as in Example 1, on a silane coupling treated glass substrate, the cover film is removed from the photosensitive film 16' for forming a decorative layer, and laminated using a laminator. Next, the temporary support of polyethylene terephthalate is peeled off at the interface with the thermoplastic resin layer, and the temporary support is removed. Hereinafter, a decorative layer is formed in the same manner as in Example 1, and the results of evaluating the front panel formed with the decorative layer are recorded in the following Table 1. Then, in the same manner as in Example 1, a capacitive input device of Comparative Example 5, i.e., a front panel 27, and an image display device 27 having a capacitive input device as a constituent element, formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer are prepared.

[0621] Compared with the front panel 1, the front panel 27 has significantly less development residue and is at an NG level. There is no problem with contamination of the opening and the back surface, and it is easy to clean, and there is no problem of contamination of other components.

[0622] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0623] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0624] Furthermore, there are no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics is obtained.

[0625] [Comparative Example 6]

[0626] In Example 1, a photosensitive film for forming a decorative layer of Comparative Example 6 was prepared in the same manner as in Example 1, except that the coating liquid formula L17 for a white photocurable resin layer was used instead of the coating liquid formula L1 for a white photocurable resin layer and the monomer / binder ratio was changed to that shown in Table 1.

[0627] In the same manner as in Example 1, on a silane coupling treated glass substrate, the cover film was removed from the photosensitive film for forming the decorative layer of the comparative example 6 obtained, and the cover film was laminated with a laminator. Then, the temporary support of polyethylene terephthalate was peeled off at the interface with the thermoplastic resin layer, and the temporary support was removed. Below, a decorative layer was formed in the same manner as in Example 1, and the front panel formed with the decorative layer was evaluated, and the evaluation results were recorded in the following table 1. Then, in the same manner as in Example 1, the electrostatic capacitance type input device of the comparative example 6 formed with the decorative layer, the mask layer, the first transparent electrode pattern, the insulating layer pattern, the second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and the transparent protective layer, i.e., the front panel 28, and the image display device 28 having the electrostatic capacitance type input device as a constituent element were made.

[0628] Compared with the front panel 1, the front panel 28 has significantly reduced the adhesion of the decorative layer, the developer residue, and the opening defects, becoming the NG level. There is no problem with the pollution of the opening and the back, the opening and the back do not have pollution, are easy to clean, and there is no problem of pollution of other parts.

[0629] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0630] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0631] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0632] [Comparative Examples 7 and 8]

[0633] In Example 1, except that the coating liquid formulations L18 and L19 for white photocurable resin layer were used instead of the coating liquid formulation L1 for white photocurable resin layer, and the titanium oxide content / solid content ratio was changed to that shown in Table 1, the photosensitive films for forming the decorative layers of Comparison Examples 7 and 8 were prepared in the same manner as in Example 1.

[0634] In the same manner as in Example 1, on a silane coupling treated glass substrate, the cover film was removed from the photosensitive film for forming the decorative layer of Comparative Examples 7 and 8 obtained, and laminated using a laminator. Next, the temporary support of polyethylene terephthalate was peeled off at the interface with the thermoplastic resin layer, and the temporary support was removed. Hereinafter, a decorative layer was formed in the same manner as in Example 1, and the front panel formed with the decorative layer was evaluated, and the evaluation results are recorded in the following Table 1. Then, in the same manner as in Example 1, electrostatic capacitance type input devices, i.e., front panels 29 and 30, and image display devices 29 and 30 having electrostatic capacitance type input devices as constituent elements of Comparative Examples 7 and 8, which were formed with a decorative layer, a mask layer, a first transparent electrode pattern, an insulating layer pattern, a second transparent electrode pattern, other conductive elements different from the first transparent electrode pattern and the second transparent electrode pattern, and a transparent protective layer, were prepared.

[0635] Compared with the front panel 1, the front panel 29 has significantly reduced the adhesion of the decorative layer, the developer residue, and the opening defects, reaching the NG level. There is no problem with the pollution of the opening and the back, it is easy to clean, and there is no problem of pollution of other parts. Compared with the front panel 1, the whiteness, the mesh structure, and the pollution of the opening of the front panel 30 are significantly reduced, reaching the NG level. There is no problem with the pollution of the back, but it must be cleaned due to the pollution of the opening.

[0636] In addition, the mask layer has no pinholes and has excellent light shielding properties.

[0637] Furthermore, there is no problem with the conductivity of the first transparent electrode pattern, the second transparent electrode pattern, and other conductive elements different therefrom, and on the other hand, there is insulation between the first transparent electrode pattern and the second transparent electrode pattern.

[0638] Furthermore, there were no defects such as bubbles on the transparent protective layer, and an image display device with excellent display characteristics was obtained.

[0639]

[0640] As shown in Table 1, by using the photosensitive film of the present invention, a white decorative layer having excellent brightness, whiteness, network structure, adhesion, development residue, and unevenness can be obtained at a high yield.

[0641] In addition, as described above, according to the manufacturing method of the electrostatic capacitance input device of the present invention using the photosensitive film of the present invention, a high-quality electrostatic capacitance input device having the advantages of thin layer / lightweight can be manufactured with a simple process. Therefore, it can be known that the electrostatic capacitance input device manufactured by the manufacturing method of the present invention and the image display device using the electrostatic capacitance input device are of high quality.

[0642] Furthermore, it is found that according to a preferred embodiment of the method for manufacturing a capacitive input device of the present invention, even when a substrate having an opening is used, the oozing out of the resist or the contamination of the back side of the substrate is less.

Claims

1. A method for manufacturing an electrostatic capacitance input device, The electrostatic capacitance input device comprises a front panel and at least the following elements (1) and (3) to (5) on the non-contact side of the front panel. (1) Decorative layer; (3) a plurality of first transparent electrode patterns, which are formed by a plurality of pad portions extending in a first direction via a connecting portion; (4) a plurality of second electrode patterns, which are electrically insulated from the first transparent electrode patterns and include a plurality of pad portions extending in a direction intersecting the first direction; (5) an insulating layer that electrically insulates the first transparent electrode pattern from the second electrode pattern, (2) a mask layer is further provided on the surface of the (1) decorative layer opposite to the front panel, The manufacturing method comprises: a step of transferring the photocurable resin layer of the photosensitive film to the non-contact side of the front panel to form at least the (1) decorative layer; The photosensitive film has a temporary support and a photocurable resin layer. The photocurable resin layer contains at least (A) a white inorganic pigment, (B) a monomer, (C) a binder, and (D) a photopolymerization initiator. The thickness of the photocurable resin layer is 1 μm to 40 μm. The content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is 30% by mass to 50% by mass. The content ratio B / C of the solid content of the (B) monomer to the solid content of the (C) binder is 0.58 to 0.

95.

2. The method for manufacturing a capacitive input device according to claim 1, wherein: The white inorganic pigment is rutile titanium oxide.

3. The method for manufacturing a capacitive input device according to claim 1, wherein: A thermoplastic resin layer is provided between the temporary support and the photocurable resin layer.

4. The method for manufacturing a capacitive input device according to claim 1, wherein: The electrostatic capacitance input device further comprises: (6) Another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern.

5. The method for manufacturing a capacitive input device according to claim 1, wherein: The second electrode pattern is a transparent electrode pattern.

6. The method for manufacturing a capacitive input device according to claim 1, wherein: At least one of the first transparent electrode pattern and the second electrode pattern is provided to cover both a non-contact surface of the front panel and a surface of the mask layer opposite to the front panel.

7. The method for manufacturing a capacitive input device according to claim 1, wherein: The electrostatic capacitance input device further comprises: (6) another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern, And the (6) other conductive element is at least arranged on the surface side of the mask layer opposite to the front panel.

8. The method for manufacturing a capacitive input device according to claim 1, wherein: A transparent protective layer is further provided so as to cover all or part of the elements of (1) and (3) to (5).

9. The method for manufacturing a capacitive input device according to claim 8, wherein: The transparent protective layer is formed using a photosensitive film having a temporary support, a thermoplastic resin layer, and a photocurable resin layer in this order.

10. The method for manufacturing a capacitive input device according to any one of claims 1 to 9, wherein: The electrostatic capacitance input device further comprises: (6) another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern, The second electrode pattern is a transparent electrode pattern, The transparent conductive material is etched using an etching pattern formed by a photosensitive film having a temporary support, a thermoplastic resin layer, and a photocurable resin layer in sequence to form at least one of the first transparent electrode pattern, the second transparent electrode pattern, and the conductive element.

11. The method for manufacturing a capacitive input device according to any one of claims 1 to 9, wherein: The electrostatic capacitance input device further comprises: (6) another conductive element electrically connected to at least one of the first transparent electrode pattern and the second electrode pattern and different from the first transparent electrode pattern and the second electrode pattern, The second electrode pattern is a transparent electrode pattern, The conductive curable resin layer of the photosensitive film having a temporary support, a thermoplastic resin layer and a conductive photocurable resin layer in sequence is transferred to form at least one of the first transparent electrode pattern, the second transparent electrode pattern and the conductive element.

12. The method for manufacturing a capacitive input device according to any one of claims 1 to 9, wherein: The non-contact surface of the front panel is subjected to surface treatment, The photosensitive film is provided on the non-contact surface of the front panel subjected to the surface treatment.

13. The method for manufacturing a capacitive input device according to claim 12, wherein: A silane compound is used in the surface treatment of the front panel.

14. The method for manufacturing a capacitive input device according to any one of claims 1 to 9, wherein: The front panel has an opening in at least a portion.

15. An electrostatic capacitance type input device, comprising a front panel and at least the following elements (1) and (3) to (5) on a non-contact side of the front panel, (1) Decorative layer; (3) a plurality of first transparent electrode patterns, which are formed by a plurality of pad portions extending in a first direction via a connecting portion; (4) a plurality of second electrode patterns, which are electrically insulated from the first transparent electrode patterns and include a plurality of pad portions extending in a direction intersecting the first direction; (5) an insulating layer that electrically insulates the first transparent electrode pattern from the second electrode pattern, (2) a mask layer is further provided on the surface of the (1) decorative layer opposite to the front panel, At least the (1) decorative layer is a photocurable resin layer, The photocurable resin layer contains at least (A) a white inorganic pigment, (B) a monomer, (C) a binder, and (D) a photopolymerization initiator. The thickness of the photocurable resin layer is 6 μm to 40 μm, The content of the white inorganic pigment relative to the total solid content of the photocurable resin layer is 32% by mass to 50% by mass. The content ratio B / C of the solid content of the (B) monomer to the solid content of the (C) binder is 0.58 to 0.

90. 16 . An image display device comprising the capacitive input device according to claim 15 as a constituent element.