Research method of simulation casting based on generator impeller disk
Through the simulation casting research method, the wax pattern and mold shell parameters of the generator impeller disk are optimized, which solves the problem of complex casting process in high-temperature alloy investment technology, improves product quality and efficiency, and reduces costs.
Patent Information
- Application Number
- CN202111384388.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-11-22
AI Technical Summary
In high-temperature alloy investment technology, the process of casting generator impeller discs is complex, resulting in low product quality and processing efficiency, and high costs. It is difficult to effectively simulate and optimize the casting process with existing technology.
Adopting a simulation casting research method based on the generator impeller disk, the wax model evaluation and simulation calculation are carried out through the alloy casting simulation software, and the wax model parameters and mold shell settings are adjusted, including thickening, rotary file grinding, platform filling, setting Insulation cotton and different heat treatment systems simulate the pouring process under different formwork conditions.
It improves the quality and processing efficiency of generator impeller disc products, reduces processing costs, optimizes the mold shell parameters and temperature conditions through simulation analysis, and improves the casting effect.
Smart Images

Figure CN114101584B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-temperature alloy investment casting application, and specifically relates to a simulation casting research method based on a generator impeller disk, in particular to the manufacturing process of the generator impeller disk. Background Art
[0002] Investment casting and directional solidification of high-temperature alloys are one of the key technologies for manufacturing single crystal (or directional crystallization) turbine blades for aircraft engines and gas turbines.
[0003] With the development of high-temperature alloy investment casting technology, people also consider using it to cast generator impellers, which requires simulation calculation of the casting process to improve the product quality and work efficiency of the cast generator impellers and reduce processing costs.
[0004] Based on the above problems, the present invention provides a simulation casting research method based on a generator impeller disk. Summary of the invention
[0005] Purpose of the invention: The purpose of the present invention is to provide a simulation casting research method based on a generator impeller disk, so as to solve the problems existing in casting alloy generator impeller disks using high-temperature alloy investment casting technology.
[0006] Technical solution: The present invention provides a simulation casting research method based on a generator impeller disk, comprising the following steps: step (1) evaluating the generator impeller disk wax mold model through alloy casting simulation software, combining the generator impeller disk wax mold model evaluation parameters and analysis results, inputting the generator impeller disk wax mold model data parameters and simulation environment settings. Step (2) inputting simulation calculation parameters, using alloy casting simulation software to perform simulation calculations, observing and analyzing the calculation results of the alloy casting simulation software.
[0007] In the technical solution, in step 1, the generator impeller disk wax mold model is observed and measures are taken to improve the generator impeller disk wax mold model, including the following situations: (a) the thickness of the blade exhaust edge is less than 0.5mm, and there is a lack of injection. The wax mold needs to be thickened by 0.5mm, and then it is removed by rotary file grinding in post-processing; (b) the thickness of the blade intake edge is less than 0.5mm, and there is a lack of injection. The wax mold needs to be thickened by 0.3mm, and then it is removed by rotary file grinding in post-processing, and the outer step of the inner ring is filled; (c) the overall thickness of the blade exhaust edge is less than 1mm; (d) the thickness of the inner ring flange is 1. 5mm; (e) The wall thickness of the outer ring of the part is 2mm, and the inner wall step of the outer ring is filled and thickened to 3mm as the machining allowance to improve shrinkage compensation; (f) The wall thickness of the outer ring on the exhaust side is 2.5mm; (g) The shape and improvement of the wax mold model of the generator impeller disk are obtained, the flange edge is filled with a circular shape, and the holes and groove features need to be blocked; the simulation environment setting in the step 1 first sets the fillet parameter of the blade and the outer ring wall to 1mm, and then sets the fillet parameter of the connection surface between the inner ring flange and the inner wall ring to 3mm, and then sets the hole fillet parameter of the inner ring flange to 2.5mm, and finally increases the fillet of the inner ring flange.
[0008] In the technical solution, the simulation calculation parameters in step 2 are as follows: alloy grade, inconel 719; pouring temperature, melting point +100°C; mold preheating temperature, 1000°C; pouring speed, 10 kg / s; pouring weight, 6.5kg; mold, mullite sand; mold thickness, 5 layers / 4mm for the blade part and 8 layers / 6mm for the other parts; alloy melting point range, 1210-1344°C; alloy density, 8.2 g / cm3.
[0009] In the simulation calculation parameters of step 2 of the present technical solution, there are two heat treatment systems: 1) taking into account both high-temperature stretching and durability, keeping warm at 954-982°C for 1h + air cooling at -718°C / 8h + air cooling to 621°C for 8h + air cooling to room temperature; 2) taking into account both room temperature and low-temperature stretching, keeping warm at 1066°C for 1-2h + air cooling at -718°C / 8h + air cooling to 621°C for 8h + air cooling to room temperature.
[0010] In the present technical solution, the casting parameter input setting and result analysis of step 2 include the following situations: (a) the blade is not thickened, the blade starts to solidify first, and the blade solidifies earlier than the inner and outer rings; (b) the blade is not thickened, the inner and outer rings are thickened by 1mm, the blade and the inner and outer rings start to solidify almost at the same time, and the blade and the inner and outer rings solidify almost synchronously; (c) the blade is thickened by 1mm, and the filling is basically completed by the gate of the inner ring. The area aligned with the inner ring gate is filled first, and other areas start to fill later. The blade and the inner and outer rings start to solidify almost at the same time, and then solidify almost synchronously. The position of the outer ring riser starts to solidify first, because it is the last to be filled, the time heated by the alloy liquid is the shortest, the position of the inner ring riser solidifies last, the inner and outer rings solidify before the blade, the blade shrinkage compensation is difficult, the transition arc is solidified last, and the looseness and cracks are mostly concentrated in this area.
[0011] In the technical solution, the casting parameter input setting and result analysis of step 2, (a) and (b) when simulating the casting of alloy, the outer layer of the generator impeller wax mold model is provided with insulation cotton; (c) when simulating the casting of alloy, the outer layer of the generator impeller wax mold model is provided with 20 mm thick insulation cotton.
[0012] Compared with the prior art, the beneficial effect of the simulation casting research method based on the generator impeller disc of the present invention is: by simulating the generator impeller disc cast by alloy under different mold shell conditions, and combining the simulation for analysis, the mold shell parameters, temperature parameters, etc. of the generator impeller disc cast using high-temperature alloy investment wax technology are obtained, thereby improving the product quality and work efficiency of the cast generator impeller disc and reducing processing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is a schematic diagram of step 1 situation (a) of the present invention;
[0014] Figure 2 , Figure 3 is a schematic diagram of situation (b) of step 1 of the present invention;
[0015] Figure 4 is a schematic diagram of situation (c) of step 1 of the present invention;
[0016] Figure 5 is a schematic diagram of situation (d) of step 1 of the present invention;
[0017] Figure 6 , Figure 7 is a schematic diagram of situation (e) of step 1 of the present invention;
[0018] Figure 8 is a schematic diagram of situation (f) of step 1 of the present invention;
[0019] Fig. 9 is a schematic diagram of the simulation environment setting in step 1 of the present invention;
[0020] Fig.10 is a schematic diagram of situation (g) of step 1 of the present invention;
[0021] Fig.11 is a schematic diagram of step 2 situation (a) of the present invention;
[0022] Fig.12 is a schematic diagram of situation (b) of step 2 of the present invention;
[0023] Fig.13 , Fig.14 It is a schematic diagram of the situation (c) of step 2 of the present invention. DETAILED DESCRIPTION
[0024] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments.
[0025] like Figures 1 to 14 The simulation casting research method based on the generator impeller disk shown includes the following steps: step (1) evaluating the generator impeller disk wax mold model through alloy casting simulation software, combining the generator impeller disk wax mold model evaluation parameters and analysis results, inputting the generator impeller disk wax mold model data parameters and simulation environment settings. Step (2) inputting simulation calculation parameters, using alloy casting simulation software to perform simulation calculation, observing and analyzing the calculation results of the alloy casting simulation software.
[0026] The present invention is based on the simulation casting research method of the generator impeller disk. In step 1, the generator impeller disk wax mold model is observed and the generator impeller disk wax mold model is improved by measures, including the following situations:
[0027] (a) The thickness of the exhaust edge of the blade is less than 0.5 mm, indicating under-injection. The wax mold needs to be thickened by 0.5 mm, and then removed by rotary file grinding in post-processing.
[0028] (b) The thickness of the blade inlet edge is less than 0.5mm, indicating under-injection. The wax mold needs to be thickened by 0.3mm. The wax mold is removed by rotary file grinding in post-processing, and the outer step of the inner ring is filled.
[0029] (c) The overall thickness of the exhaust edge of the blade is less than 1 mm;
[0030] (d) The thickness of the inner ring flange is 1.5 mm;
[0031] (e) The wall thickness of the outer ring of the part is 2 mm, and the inner wall step of the outer ring is filled and thickened to 3 mm as the machining allowance to improve shrinkage compensation;
[0032] (f) The wall thickness of the outer ring on the exhaust side is 2.5 mm;
[0033] (g) The shape and improvement of the generator impeller wax model are obtained, the flange edge is filled with a circular shape, and the holes and groove features need to be blocked;
[0034] The simulation environment setting in step 1 first sets the fillet parameters of the blade and the outer ring wall to 1mm, then sets the fillet parameters of the connection surface between the inner ring flange and the inner wall ring to 3mm, then sets the fillet parameters of the hole of the inner ring flange to 2.5mm, and finally increases the fillet of the inner ring flange.
[0035] The present invention is based on the simulation casting research method of the generator impeller disk. The simulation calculation parameters in step 2 are as follows: alloy grade, inconel 719; melting point range of the alloy, 1210-1344°C; density of the alloy, 8.2 g / cm3; pouring temperature, melting point + 100°C (100°C higher than the melting point); mold preheating temperature, 1000°C; pouring speed, 10 kg / s; pouring weight, 6.5 kg; mold material, mullite sand; mold thickness, 5 layers / 4 mm for the blade part (5 layers have a thickness of 4 mm), and 8 layers / 6 mm for other parts (8 layers have a thickness of 4 mm).
[0036] The present invention is based on the simulation casting research method of the generator impeller disk. In the simulation calculation parameters of step 2, there are two heat treatment systems: 1) Taking into account both high-temperature stretching and durability, keep warm at 954-982℃ for 1h + air cool to -718℃ / 8h + air cool to 621℃ for 8h + air cool to room temperature; 2) Taking into account both room temperature and low-temperature stretching, keep warm at 1066℃ for 1-2h + air cool to -718℃ / 8h + air cool to 621℃ for 8h + air cool to room temperature.
[0037] The present invention is based on the simulation casting research method of the generator impeller disk. The casting parameter input setting and result analysis of step 2 include the following situations:
[0038] (a) The blade is not thickened, the blade starts to solidify first, and the blade solidifies earlier than the inner and outer rings;
[0039] (b) The blade is not thickened, and the inner and outer rings are thickened by 1 mm. The blade and the inner and outer rings begin to solidify almost at the same time. The blade and the inner and outer rings solidify almost synchronously.
[0040] (c) The blade is thickened by 1mm, and the filling is basically completed by the gate of the inner ring. The area aligned with the inner ring gate is filled first, and other areas start to fill later. The blade and the inner and outer rings start to solidify almost at the same time, and then solidify almost synchronously. The position of the outer ring riser starts to solidify first, because it is the last to be filled and the time heated by the alloy liquid is the shortest. The position of the inner ring riser solidifies last. The inner and outer rings solidify before the blade, making it difficult to compensate for the shrinkage of the blade. The transition arc solidifies last, and the looseness and cracks are mostly concentrated in this area.
[0041] The present invention is based on the simulation casting research method of the generator impeller disk, the casting parameter input setting and result analysis of step 2, (a) and (b) when simulating the casting of alloy, the outer layer of the generator impeller disk wax mold model is provided with insulation cotton; (c) when simulating the casting of alloy, the outer layer of the generator impeller disk wax mold model is provided with 20 mm thick insulation cotton.
[0042] The present invention is based on a simulation casting research method of a generator impeller disk, and the alloy casting simulation software is ProCAST.
[0043] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention. These improvements should also be regarded as within the scope of protection of the present invention.
Claims
1. A simulation casting research method based on a generator impeller disk, characterized in that: The following steps are included: Step (1) evaluating the generator impeller disk wax mold model through alloy casting simulation software, inputting the generator impeller disk wax mold model data parameters and simulation environment settings in combination with the generator impeller disk wax mold model evaluation parameters and analysis results; Step (2) inputting simulation calculation parameters, performing simulation calculation using alloy casting simulation software, observing and analyzing the calculation results of the alloy casting simulation software; In the step 1, the generator impeller disk wax mold model is observed and measures are taken to improve the generator impeller disk wax mold model, including the following situations: (a) The thickness of the exhaust edge of the blade is less than 0.5 mm, indicating under-injection. The wax mold needs to be thickened by 0.5 mm, and then removed by rotary file grinding in post-processing. (b) The thickness of the blade inlet edge is less than 0.5mm, indicating under-injection. The wax mold needs to be thickened by 0.3mm. The wax mold is removed by rotary file grinding in post-processing, and the outer step of the inner ring is filled. (c) The overall thickness of the exhaust edge of the blade is less than 1 mm; (d) The thickness of the inner ring flange is 1.5 mm; (e) The wall thickness of the outer ring of the part is 2 mm, and the inner wall step of the outer ring is filled and thickened to 3 mm as the machining allowance to improve shrinkage compensation; (f) The wall thickness of the outer ring on the exhaust side is 2.5 mm; (h) The shape and improvement of the generator impeller wax model are obtained, the flange edge is filled with a circular shape, and the holes and groove features need to be blocked; The simulation environment setting in step 1 is to first set the fillet parameter of the blade and the outer ring wall to 1mm, then set the fillet parameter of the connection surface between the inner ring flange and the inner wall ring to 3mm, then set the fillet parameter of the hole of the inner ring flange to 2.5mm, and finally increase the fillet of the inner ring flange; The simulation calculation parameters in step 2 are as follows: alloy grade, inconel 719; pouring temperature, melting point + 100°C; mold shell preheating temperature, 1000°C; pouring speed, 10 kg / s; Casting weight, 6.5kg; mold shell, mullite sand; mold shell thickness, blade part 5 layers / 4mm, other parts 8 layers / 6mm; alloy melting point range, 1210-1344℃; alloy density, 8.2 g / cm3; In the simulation calculation parameters of step 2, there are two heat treatment systems: 1) taking into account both high-temperature stretching and durability, keeping warm at 954-982°C for 1h + air cooling to -718°C / 8h + air cooling to 621°C for 8h + air cooling to room temperature; 2) taking into account both room temperature and low-temperature stretching, keeping warm at 1066°C for 1-2h + air cooling to -718°C / 8h + air cooling to 621°C for 8h + air cooling to room temperature.
2. The simulation casting research method based on the generator impeller disk according to claim 1 is characterized in that: The pouring parameter input setting and result analysis of step 2 include the following situations: (a) The blade is not thickened, the blade starts to solidify first, and the blade solidifies earlier than the inner and outer rings; (b) The blade is not thickened, and the inner and outer rings are thickened by 1 mm. The blade and the inner and outer rings begin to solidify almost at the same time. The blade and the inner and outer rings solidify almost synchronously. (c) The blade is thickened by 1mm, and the filling is basically completed by the gate of the inner ring. The area aligned with the inner ring gate is filled first, and other areas start to fill later. The blade and the inner and outer rings start to solidify almost at the same time, and then solidify almost synchronously. The position of the outer ring riser starts to solidify first, because it is the last to be filled and the time heated by the alloy liquid is the shortest. The position of the inner ring riser solidifies last. The inner and outer rings solidify before the blade, making it difficult to compensate for the shrinkage of the blade. The transition arc solidifies last, and the looseness and cracks are mostly concentrated in this area.
3. The simulation casting research method based on the generator impeller disk according to claim 2 is characterized in that: The pouring parameter input setting and result analysis of step 2, (a) and (b) When simulating the casting of alloy, the outer layer of the generator impeller wax model is provided with thermal insulation cotton; (c) When simulating the casting of alloy, a 20 mm thick insulation cotton is set on the outer layer of the generator impeller wax mold model.
Citation Information
Patent Citations
Method for preventing blades of whole turbine impeller of high temperature alloy from under-casting
CN102441642A
Alloy micro-cast forming process simulation method based on fluent software
CN105302985A
Simulation method for casting forming of double-performance blisk
CN112001037A