Semiconductor device and method for manufacturing the same, and storage device

By thinning the first film layer and performing patterning on the wafer of the semiconductor device, the problem of through hole shrinkage defects in the dynamic random access memory is solved and the yield rate of the device is improved.

CN114156267BActive Publication Date: 2024-10-29CHANGXIN MEMORY TECH INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202010928257.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-07
Publication Date
2024-10-29
Estimated Expiration
2040-09-07

AI Technical Summary

Technical Problem

During the etching process of dynamic random access memory, due to uneven plasma in the cavity, there are differences in etching between the edge and the middle of the wafer. Shrinkage defects occur in the through holes of the capacitor structure formed, resulting in reduced device yield.

Method used

By forming a stacked film structure on the wafer of the semiconductor device, and thinning the thickness of the first film layer so that the thickness at the edge of the wafer is smaller than the thickness in the middle, a chemical mechanical polishing process is used to increase the pressure at the edge of the grinding head, An annular arc surface is formed to form connected through holes during the patterning process to avoid shrinkage defects.

Benefits of technology

The thickness difference of the through hole at the edge of the wafer is reduced, the connection problem between the capacitor structure and the semiconductor structure is avoided, and the yield rate of the semiconductor device is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114156267B_ABST
    Figure CN114156267B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor technology, and proposes a semiconductor device and a preparation method thereof, and a storage device, wherein the preparation method comprises: providing a wafer, on which a semiconductor structure is formed; forming a stacked film layer structure on a side of the semiconductor structure away from the wafer, wherein the film layer in the stacked film layer structure that is farthest from the semiconductor structure is the first film layer; thinning the thickness of the first film layer so that the thickness of the orthographic projection of the first film layer on the wafer at the edge of the wafer is less than the thickness of the orthographic projection of the first film layer on the wafer at the middle of the wafer; patterning the stacked film layer structure to form a plurality of through holes, wherein the through holes are connected to the semiconductor structure. The advantage of the present invention is that shrinkage defects are avoided in the process of patterning the stacked film layer structure to form a plurality of through holes, thereby ensuring the device yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor device and a method for preparing the semiconductor device, and a storage device comprising the semiconductor device. Background Art

[0002] Dynamic Random Access Memory (DRAM) is a commonly used semiconductor memory device in computers, consisting of many repeated storage cells. Each storage cell usually includes a capacitor and a transistor; the gate of the transistor is connected to the word line, the drain is connected to the bit line, and the source is connected to the capacitor; the voltage signal on the word line can control the opening or closing of the transistor, and then read the data information stored in the capacitor through the bit line, or write the data information into the capacitor through the bit line for storage.

[0003] With the development and progress of technology, the size of dynamic random access memory is showing a trend of miniaturization. The capacitor inside it is constantly decreasing with the geometric size according to Moore's Law, and the depth-to-width ratio of the capacitor is large, even exceeding 50:1. Due to the uneven plasma in the cavity during the etching process, there are differences in etching at the edge of the wafer and the middle of the wafer, which ultimately leads to shrinkage defects in the through hole that accommodates the capacitor structure formed at the edge of the wafer; due to the shrinkage defects in the through hole that accommodates the capacitor structure formed at the edge of the wafer, the capacitor structure subsequently formed in the through hole cannot be connected to the capacitor contact structure, which ultimately leads to a reduction in the device yield.

[0004] The above information disclosed in this Background section is only for enhancement of understanding of the background of the invention and therefore it may contain information that does not constitute the prior art that is already known to a person of ordinary skill in the art. Summary of the invention

[0005] The object of the present invention is to overcome the above-mentioned shortcomings of the prior art that shrinkage defects are prone to occur, and to provide a semiconductor device that is not prone to shrinkage defects, a method for preparing a semiconductor device, and a storage device including the semiconductor device.

[0006] Additional aspects and advantages of the invention will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the invention.

[0007] According to one aspect of the present invention, there is provided a method for preparing a semiconductor device, comprising:

[0008] Providing a wafer, on which a semiconductor structure is formed;

[0009] forming a stacked film layer structure on a side of the semiconductor structure away from the wafer, wherein the film layer in the stacked film layer structure that is farthest from the semiconductor structure is the first film layer;

[0010] Thinning the thickness of the first film layer so that the thickness of the first film layer at the edge of the wafer where the orthographic projection of the first film layer is located on the wafer is smaller than the thickness of the first film layer at the middle of the wafer where the orthographic projection of the first film layer is located on the wafer;

[0011] The stacked film structure is patterned to form a plurality of through holes, wherein the through holes are connected to the semiconductor structure.

[0012] In an exemplary embodiment of the present invention, thinning the thickness of the first film layer includes: thinning the thickness of the first film layer by a chemical mechanical polishing process.

[0013] In an exemplary embodiment of the present invention, the pressure at the edge of the grinding head of the chemical mechanical grinding equipment is increased so that the pressure at the edge of the grinding head is greater than the pressure in the middle of the grinding head. Therefore, after the thickness of the first film layer is thinned, the thickness of the first film layer whose orthographic projection on the wafer is located at the edge of the wafer is smaller than the thickness of the first film layer whose orthographic projection on the wafer is located in the middle of the wafer.

[0014] In an exemplary embodiment of the present invention, the edge of the wafer is a portion whose distance from the center point of the wafer is greater than or equal to a set value, and the middle of the wafer is a portion whose distance from the center point of the wafer is less than a set value.

[0015] In an exemplary embodiment of the present invention, the orthographic projection of the edge of the grinding head on the wafer coincides with the edge of the wafer, and the orthographic projection of the middle of the grinding head on the wafer coincides with the middle of the wafer.

[0016] In an exemplary embodiment of the present invention, after the thickness of the first film layer is thinned, the side of the first film layer that is projected at the edge of the wafer and is away from the semiconductor structure forms an annular arc surface, and the farther from the center point of the wafer, the thinner the thickness of the first film layer.

[0017] In an exemplary embodiment of the present invention, a stacked film layer structure is formed on a side of the semiconductor structure away from the wafer, comprising:

[0018] forming a first insulating layer on a side of the semiconductor structure away from the wafer;

[0019] forming a first supporting layer on a side of the first insulating layer away from the semiconductor structure;

[0020] forming a second insulating layer on a side of the first supporting layer away from the semiconductor structure;

[0021] forming a second supporting layer on a side of the second insulating layer away from the semiconductor structure;

[0022] forming a third insulating layer on a side of the second supporting layer away from the semiconductor structure;

[0023] forming a dielectric layer on a side of the third insulating layer away from the semiconductor structure;

[0024] forming a third supporting layer on a side of the dielectric layer away from the semiconductor structure;

[0025] The third supporting layer is the first film layer.

[0026] In an exemplary embodiment of the present invention, patterning the stacked film structure to form a plurality of through holes comprises:

[0027] forming a mask layer on a side of the stacked film structure away from the semiconductor structure;

[0028] forming a photoresist layer on a side of the mask layer away from the semiconductor structure;

[0029] Using the photoresist layer as a mask, etching the mask layer, the third supporting layer and a portion of the dielectric layer;

[0030] Using the third supporting layer as a mask, etching the remaining portion of the dielectric layer and a portion of the third insulating layer;

[0031] The remaining portion of the third insulating layer, the second supporting layer, the second insulating layer, the first supporting layer, and the first insulating layer are etched using the dielectric layer as a mask to form a plurality of the through holes.

[0032] In an exemplary embodiment of the present invention, the semiconductor structure includes a capacitor contact structure. After the stacked film layer structure is patterned to form a plurality of through holes, the through holes are connected to the capacitor contact structure so that a side of the capacitor contact structure away from the wafer is exposed.

[0033] According to one aspect of the present invention, there is provided a semiconductor device, which is prepared by any one of the preparation methods described above.

[0034] According to one aspect of the present invention, there is provided a storage device, comprising a semiconductor device as described in any one of the above.

[0035] It can be seen from the above technical solution that the present invention has at least one of the following advantages and positive effects:

[0036] The method for preparing a semiconductor device of the present invention thins the thickness of the first film layer so that the thickness of the orthographic projection of the first film layer on the wafer at the edge of the wafer is less than the thickness of the orthographic projection of the first film layer on the wafer at the middle of the wafer; the stacked film layer structure is patterned to form a plurality of through holes, and the through holes are connected to the semiconductor structure. After the thickness of the first film layer at the edge of the wafer is thinned, the total thickness of the stacked film layer structure is reduced. In the subsequent patterning process, the hole formed at the edge of the wafer is deeper than the hole in the middle of the wafer at the beginning, so that the finally formed through hole will not have a shrinkage defect, so that the capacitor structure subsequently formed in the through hole can be connected to the semiconductor structure, thereby improving the yield of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The above and other features and advantages of the present invention will become more apparent by describing in detail exemplary embodiments thereof with reference to the attached drawings.

[0038] Figure 1 It is a schematic diagram of the structure of a semiconductor device when etching begins in the related art;

[0039] Figure 2 yes Figure 1 A schematic diagram of the structure of the semiconductor device after etching is completed;

[0040] Figure 3 yes Figure 2 A top view schematic diagram of

[0041] Figure 4 It is a schematic flow chart of an exemplary embodiment of a method for preparing a semiconductor device of the present invention;

[0042] Figure 5 It is a schematic structural diagram of a semi-finished semiconductor device after the deposition of the stacked film layer structure is completed;

[0043] Figure 6 is Figure 5 A schematic structural diagram of a semi-finished semiconductor device after the first film layer is thinned based on the above;

[0044] Figure 7 It is a schematic diagram of the structure of a dual-axis chemical mechanical polishing device;

[0045] Figure 8 yes Figure 7 Schematic diagram of the partition structure of the grinding head;

[0046] Fig. 9 is Figure 6 A schematic structural diagram of a semi-finished product of a semiconductor device after a mask layer and a photoresist layer are formed on the basis of the semiconductor device;

[0047] Fig.10 is Fig. 9A schematic structural diagram of a semi-finished product of a semiconductor device after the first etching is completed on the basis of FIG.

[0048] Fig.11 is Fig.10 A schematic structural diagram of a semi-finished product of a semiconductor device after the second etching is completed on the basis of FIG.

[0049] Fig.12 is Fig.11 A schematic structural diagram of a semi-finished product of a semiconductor device after the third etching is completed on the basis of FIG.

[0050] Fig.13 It is a schematic structural diagram of an exemplary implementation of a semiconductor device of the present invention.

[0051] The main components in the figure are described as follows:

[0052] 1. Polishing pad; 2. Polishing liquid nozzle; 3. Grinding head;

[0053] 4. semiconductor structure; 41. capacitor contact isolation layer; 42. capacitor contact structure;

[0054] 5. Laminated film layer structure; 51. First insulating layer; 52. First supporting layer; 53. Second insulating layer; 54. Second supporting layer; 55. Third insulating layer; 56. Dielectric layer; 57. Third supporting layer;

[0055] 6. Mask layer; 7. Photoresist layer; 8. Through hole; 9. Blind hole; 10. Polymer. DETAILED DESCRIPTION

[0056] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that the present invention will be comprehensive and complete and fully convey the concepts of the example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their detailed description will be omitted.

[0057] Reference Figure 1 The schematic diagram of the structure of the semiconductor device when etching starts in the related art shown in the figure shows that after etching the dielectric layer 56 and part of the third insulating layer 55, the depth of the hole formed at the edge of the wafer is relatively shallow due to the uneven plasma in the chamber during the etching process. Figure 2The schematic diagram of the structure of the semiconductor device after etching in the related art shown in the figure shows that only blind holes 9 can be formed at the edge of the wafer, and polymer 10 is attached to the inner wall of the blind hole 9 formed by etching, resulting in shrinkage defects, which makes the capacitor structure formed subsequently unable to connect with the capacitor contact structure 42, and finally reduces the yield of the semiconductor device. Figure 3 The schematic top view of the semiconductor device after etching in the related art shown in the figure shows that there is a hole in the dotted frame whose diameter is smaller than that of other holes. This hole is the blind hole 9 with shrinkage defect. Figure 1 , Figure 2 and Figure 3 The side pointed by the middle arrow is the edge side of the wafer.

[0058] The present invention first provides a method for preparing a semiconductor device, referring to Figure 4 As shown, the method for preparing the semiconductor device may include the following steps:

[0059] Step S10, providing a wafer, on which a semiconductor structure 4 is formed.

[0060] Step S20 , forming a stacked film layer structure 5 on a side of the semiconductor structure 4 away from the wafer, wherein the film layer in the stacked film layer structure 5 that is farthest from the semiconductor structure 4 is the first film layer.

[0061] Step S30 , reducing the thickness of the first film layer so that the thickness of the first film layer whose orthographic projection is on the wafer at the edge of the wafer is smaller than the thickness of the first film layer whose orthographic projection is on the wafer at the middle of the wafer.

[0062] In step S40 , patterning is performed on the stacked film structure 5 to form a plurality of through holes 8 , wherein the through holes 8 are connected to the semiconductor structure 4 .

[0063] The following is a detailed description of each step of the method for preparing a semiconductor device according to an embodiment of the present invention:

[0064] In all the figures, the side pointed by the arrow is the edge side of the wafer.

[0065] Step S10 , providing a wafer (not shown in the figure), on which a semiconductor structure 4 is formed.

[0066] In this example implementation, refer to Figure 5 As shown, the semiconductor structure 4 includes a capacitor contact isolation layer 41 and a capacitor contact structure 42, and at least one side of the capacitor contact structure 42 is exposed. The semiconductor structure 4 also includes semiconductor devices such as transistors, word lines, and bit lines, which are not shown in the figure because they do not involve the technical features of the present invention.

[0067] Step S20 , forming a stacked film layer structure 5 on a side of the semiconductor structure 4 away from the wafer, wherein the film layer in the stacked film layer structure 5 that is farthest from the semiconductor structure 4 is the first film layer.

[0068] In this example implementation, please continue to refer to Figure 5 As shown, forming a stacked film structure 5 on the side of the semiconductor structure 4 away from the wafer may include: depositing a first insulating layer 51 on the side of the semiconductor structure 4 away from the wafer; the material of the first insulating layer 51 may be silicon nitride, silicon boronitride, etc., and the thickness of the first insulating layer 51 is 10-20nm. Depositing a first supporting layer 52 on the side of the first insulating layer 51 away from the semiconductor structure 4; the material of the first supporting layer 52 may be silicon oxide, silicon oxynitride, etc., and the thickness of the first supporting layer 52 is about 50-100nm. Depositing a second insulating layer 53 on the side of the first supporting layer 52 away from the semiconductor structure 4; the material of the second insulating layer 53 may be silicon nitride, silicon carbonitride, etc., and the thickness of the second insulating layer 53 is 10-20nm. Depositing a second supporting layer 54 on the side of the second insulating layer 53 away from the semiconductor structure 4; the material of the second supporting layer 54 may be silicon oxide, silicon oxynitride, etc., and the thickness of the second supporting layer 54 is about 50-100nm. A third insulating layer 55 is deposited on the side of the second supporting layer 54 away from the semiconductor structure 4; the material of the third insulating layer 55 can be silicon nitride, silicon carbonitride, etc., and the thickness of the third insulating layer 55 is about 10 to 20 nm. A dielectric layer 56 is deposited on the side of the third insulating layer 55 away from the semiconductor structure 4; the material of the dielectric layer 56 can be a carbon film, a silicon film, etc., and the thickness of the dielectric layer 56 is 30 to 50 nm. A third supporting layer 57 can be deposited on the side of the dielectric layer 56 away from the semiconductor structure 4, and the material of the third supporting layer 57 can be silicon oxide, and the thickness of the third supporting layer 57 is 80 to 150 nm. The third supporting layer 57 is the first film layer. Since the material of silicon oxide is relatively soft and easy to grind, the third supporting layer 57 is used as the first film layer for thinning. Of course, in other exemplary embodiments of the present invention, the mask layer 6 formed subsequently can also be thinned. The third insulating layer 55, the second supporting layer 54, etc. can also be thinned.

[0069] Step S30 , reducing the thickness of the first film layer so that the thickness of the first film layer whose orthographic projection is on the wafer at the edge of the wafer is smaller than the thickness of the first film layer whose orthographic projection is on the wafer at the middle of the wafer.

[0070] Reference Figure 6As shown, after the thickness of the first film layer (third supporting layer 57) is thinned, the first film layer (third supporting layer 57) located at the edge of the wafer and away from the semiconductor structure 4 forms a circular arc surface, and the farther from the center of the wafer, the thinner the first film layer is. That is, the arc surface of the first film layer is bent toward the semiconductor structure 4.

[0071] In this example embodiment, the edge of the wafer is the portion whose distance from the center point of the wafer is greater than or equal to six sevenths of the wafer radius, and the middle of the wafer is the portion whose distance from the center point of the wafer is less than six sevenths of the wafer radius. For example, when the radius of the wafer is 150 mm, the edge of the wafer is the annular portion whose distance from the center position of the wafer is greater than or equal to 129 mm, and the middle of the wafer is the circular portion whose distance from the center position of the wafer is less than 129 mm. Of course, in other example embodiments of the present invention, the position and size of the edge of the wafer can be set according to actual conditions, and are not limited to the above description.

[0072] The edge of the grinding head 3 corresponds to the edge of the wafer, and the middle of the grinding head 3 corresponds to the middle of the wafer; that is, the diameter of the grinding head 3 and the diameter of the wafer can be the same, the orthographic projection of the edge of the grinding head 3 on the wafer coincides with the edge of the wafer, and the orthographic projection of the middle of the grinding head 3 on the wafer coincides with the middle of the wafer.

[0073] In this example embodiment, the thickness of the first film layer can be thinned by a chemical mechanical polishing process. Specifically, when the first film layer is polished, the pressure at the edge of the polishing head 3 of the chemical mechanical polishing equipment can be increased so that the pressure at the edge of the polishing head 3 of the chemical mechanical polishing equipment is greater than the pressure in the middle of the polishing head 3. That is, the first film layer can be polished by a dual-axis chemical mechanical polishing equipment to thin the thickness of the edge of the first film layer. Chemical mechanical polishing equipment is different from traditional pure mechanical or pure chemical polishing methods. Chemical mechanical polishing equipment avoids the surface damage caused by pure mechanical polishing and the shortcomings of slow polishing speed, poor surface flatness and polishing consistency caused by pure chemical polishing through the combined action of chemistry and mechanics. It utilizes the "soft grinding hard" principle in wear, that is, using softer materials for polishing to achieve high-quality surface polishing. The polishing liquid of the chemical mechanical polishing equipment is a high-purity, low-metal ion type polishing product produced by a special process using high-purity silicon powder as raw material. It is widely used in nano-level high flatness polishing of various materials. Reference Figure 7As shown, the dual-axis chemical mechanical polishing equipment may include a polishing pad 1, a polishing liquid nozzle 2 and a grinding head 3. The polishing pad 1 can rotate, and the grinding head 3 can also rotate and apply pressure. The grinding head 3 adsorbs the wafer provided with a stacked film layer structure 5, and makes the first film layer fit with the polishing pad 1. The polishing liquid nozzle 2 sprays the polishing liquid, the polishing pad 1 rotates, and the grinding head 3 also rotates and applies pressure to the wafer provided with the stacked film layer structure 5 to achieve thinning of the thickness of the first film layer, and make the thickness of the first film layer whose orthographic projection on the wafer is located at the edge of the wafer smaller than the thickness of the first film layer whose orthographic projection on the wafer is located in the middle of the wafer.

[0074] In this example implementation, refer to Figure 8 As shown, the grinding head 3 can be divided into a central area Z connected in sequence. 中 The six annular areas are concentrically arranged. The six annular areas are respectively a first annular area Z1, a second annular area Z2, a third annular area Z3, a fourth annular area Z4, a fifth annular area Z5 and a sixth annular area Z6. The central area Z 中 The radius of the first annular area Z1 is about 40 mm. The inner ring of the first annular area Z1 is connected to the central area Z 中 , the outer ring radius of the first annular area Z1 is about 70mm. The inner ring of the second annular area Z2 is connected to the outer ring of the first annular area Z1, and the outer ring radius of the second annular area Z2 is about 95mm. The inner ring of the third annular area Z3 is connected to the outer ring of the second annular area Z2, and the outer ring radius of the third annular area Z3 is about 125mm. The inner ring of the fourth annular area Z4 is connected to the outer ring of the third annular area Z3, and the outer ring radius of the fourth annular area Z4 is about 139mm. The inner ring of the fifth annular area Z5 is connected to the outer ring of the fourth annular area Z4, and the outer ring radius of the fifth annular area Z5 is about 145mm. The inner ring of the sixth annular area Z6 is connected to the outer ring of the fifth annular area Z5, and the outer ring radius of the sixth annular area Z6 is about 150mm. Of course, in other exemplary embodiments of the present invention, the areas of the grinding head 3 can be set to four, five, eight or more, and the size of each area can also be set larger or smaller as needed.

[0075] The pressure of each area of ​​the grinding head 3 may be different. Refer to Table 1 for the pressure values ​​that need to be applied to each area of ​​the grinding head 3 under different thinning thickness requirements. The unit of the value in the table is PSI (Pounds per square inch). In this example embodiment, the sixth annular area Z6 may be the edge of the grinding head 3. The rest may be the middle of the grinding head 3.

[0076] Table 1

[0077]

[0078] From Table 1 we can get:

[0079] When the thickness of the first film layer at the edge of the wafer is thinned by an average of 10 nm, the pressure of the sixth annular region Z6 can be 5.1, the pressure of the fifth annular region Z5 can be 2.44, the pressure of the fourth annular region Z4 can be 2.08, the pressure of the third annular region Z3 can be 2.08, the pressure of the second annular region Z2 can be 2.18, the pressure of the first annular region Z1 can be 2.15, and the pressure of the central region Z 中 The pressure can be 2.15.

[0080] When the thickness of the first film layer at the edge of the wafer is thinned by an average of 20 nm, the pressure of the sixth annular area Z6 can be 5.95, the pressure of the fifth annular area Z5 can be 2.84, the pressure of the fourth annular area Z4 can be 2.08, the pressure of the third annular area Z3 can be 2.08, the pressure of the second annular area Z2 can be 2.18, the pressure of the first annular area Z1 can be 2.15, and the pressure of the central area Z 中 The pressure can be 2.15.

[0081] When the thickness of the first film layer at the edge of the wafer is thinned by an average of 30 nm, the pressure of the sixth annular region Z6 can be 6.8, the pressure of the fifth annular region Z5 can be 3.25, the pressure of the fourth annular region Z4 can be 2.08, the pressure of the third annular region Z3 can be 2.08, the pressure of the second annular region Z2 can be 2.18, the pressure of the first annular region Z1 can be 2.15, and the pressure of the central region Z 中 The pressure can be 2.15.

[0082] The above three example implementations of the thinning thickness at the edge of the first film layer are listed, which are average thinning of 10nm, 20nm and 30nm respectively; in other example implementations of the present invention, the thinning thickness of the first film layer is not limited to the above description. Through countless experiments, it is found that the average thinning thickness of the first film layer can be greater than or equal to 10nm and less than or equal to 40nm, which will not be explained one by one here. Due to the subsequent etching of the stacked film layer structure 5, due to the uneven plasma in the cavity and other reasons, the part of the stacked film layer structure 5 projected at the edge of the wafer will be etched shallower, and the farther from the center of the wafer, the shallower it will be etched. Therefore, after thinning the first film layer, it is necessary to make the thickness of the first film layer projected on the wafer at the edge of the wafer less than the thickness of the first film layer projected on the wafer in the middle of the wafer. And the farther from the center point of the wafer, the thinner the thickness of the first film layer.

[0083] Of course, in other example embodiments of the present invention, the thickness of the edge of the first film layer can be thinned by an etching method. After thinning, the side of the edge of the first film layer away from the semiconductor structure 4 can be an annular slope or an annular step surface, so that the farther the first film layer is from its center point, the thinner its thickness.

[0084] In step S40 , patterning is performed on the stacked film structure 5 to form a plurality of through holes 8 , wherein the through holes 8 are connected to the semiconductor structure 4 .

[0085] In this example implementation, refer to Fig. 9 As shown, first, a mask layer 6 can be deposited on the side of the stacked film structure 5 away from the semiconductor structure 4. The material of the mask layer 6 can be silicon oxynitride, and the thickness of the mask layer 6 is about 30 to 50 nm. A photoresist layer 7 can be deposited on the side of the mask layer 6 away from the semiconductor structure 4, and the thickness of the photoresist layer 7 is about 40 to 70 nm.

[0086] Then, the mask layer 6, the third support layer 57 and part of the dielectric layer 56 are etched using the photoresist layer 7 as a mask. Specifically, a mask is placed on the photoresist layer 7, the photoresist layer 7 is exposed to light, the photoresist layer not covered by the mask is removed, and then the mask is removed, the mask layer 6, the third support layer 57 and part of the dielectric layer 56 not covered by the photoresist layer 7 are etched, and the remaining photoresist layer 7 is removed to form Fig.10 As can be clearly seen from the semi-finished product shown in the figure, the depth of the holes formed by etching near the edge is deeper.

[0087] Next, the remaining portion of the dielectric layer 56 and a portion of the third insulating layer 55 are etched using the third supporting layer 57 as a mask to form Fig.11 As can be seen from the comparison of the dotted lines in the figure, the depth of the holes formed by etching near the edge is deeper.

[0088] Again, the remaining portion of the third insulating layer 55, the second supporting layer 54, the second insulating layer 53, the first supporting layer 52 and the first insulating layer 51 are etched using the dielectric layer 56 as a mask to form a plurality of through holes 8. The through holes 8 are connected to the capacitor contact structure 42, forming Fig.12 Finally, the dielectric layer 56 is removed to form Fig.13 The structure shown.

[0089] The method for preparing a semiconductor device may further include forming a capacitor structure in the through hole 8, the capacitor structure being connected to the capacitor contact structure 42. Specifically, a first electrode is formed in the through hole 8; an interlayer dielectric layer is formed on a side of the first electrode away from the stacked film layer structure 5; and a second electrode is formed on a side of the interlayer dielectric layer away from the first electrode.

[0090] Through multiple experiments, it was found that when there was no thinning at the edge of the first film layer, the average number of shrinkage defects was 57; when the first film layer was thinned by an average of 10 nm at the edge, the average number of shrinkage defects was 7; when the first film layer was thinned by an average of 20 nm at the edge, the average number of shrinkage defects was 4.

[0091] Furthermore, the present invention also provides a semiconductor device, referring to Fig.13 The schematic diagram of the structure of an exemplary embodiment of a semiconductor device of the present invention is shown, and the semiconductor device is prepared by any of the preparation methods described above. The through hole 8 finally formed by the semiconductor device prepared by the above preparation method will not have shrinkage defects, so that the capacitor structure subsequently formed in the through hole 8 can be connected to the capacitor contact structure 42, thereby improving the yield of the semiconductor device. The specific structure of the semiconductor device has been described in detail above, so it will not be repeated here.

[0092] Furthermore, the present invention also provides a storage device, which may include the semiconductor device described above.

[0093] Compared with the prior art, the beneficial effects of the storage device provided by the exemplary embodiment of the present invention are the same as the beneficial effects of the semiconductor device provided by the above exemplary embodiment, which will not be described in detail here.

[0094] The features, structures or characteristics described above may be combined in one or more embodiments in any suitable manner, and if possible, the features discussed in each embodiment are interchangeable. In the above description, many specific details are provided to provide a full understanding of the embodiments of the present invention. However, those skilled in the art will appreciate that the technical solution of the present invention may be practiced without one or more of the specific details, or other methods, components, materials, etc. may be adopted. In other cases, known structures, materials or operations are not shown or described in detail to avoid blurring various aspects of the present invention.

[0095] The terms "about" and "approximately" used in this specification generally mean within 20%, preferably within 10%, and more preferably within 5% of a given value or range. The numbers given here are approximate numbers, which means that in the absence of specific instructions, the meanings of "about", "approximately", "roughly" and "approximately" can still be implied.

[0096] Although relative terms such as "upper" and "lower" are used in this specification to describe the relative relationship of one component of the illustration to another component, these terms are used in this specification only for convenience, such as the orientation of the examples described in the drawings. It is understood that if the device of the illustration is turned over so that it is upside down, the component described as being "upper" will become the component "lower". Other relative terms, such as "high", "low", "top", "bottom", etc., are also used to have similar meanings. When a structure is "on" other structures, it may mean that the structure is formed integrally on the other structure, or that the structure is "directly" disposed on the other structure, or that the structure is "indirectly" disposed on the other structure through another structure.

[0097] In this specification, the terms "a", "an", "the" and "said" are used to indicate the presence of one or more elements / components / etc.; the terms "comprising", "including" and "having" are used to express an open-ended inclusion and mean that there may be additional elements / components / etc. in addition to the listed elements / components / etc.; the terms "first", "second" and "third" etc. are used only as labels and are not intended to limit the quantity of their objects.

[0098] It should be understood that the present invention is not limited in its application to the detailed structure and arrangement of the components proposed in this specification. The present invention can have other embodiments and can be implemented and executed in a variety of ways. The aforementioned variations and modifications fall within the scope of the present invention. It should be understood that the present invention disclosed and defined in this specification extends to all alternative combinations of two or more individual features mentioned or evident in the text and / or the drawings. All these different combinations constitute multiple alternative aspects of the present invention. The embodiments described in this specification illustrate the best mode known for implementing the present invention and will enable those skilled in the art to utilize the present invention.

Claims

1. A method for preparing a semiconductor device, characterized in that: include: Providing a wafer, on which a semiconductor structure is formed; forming a stacked film layer structure on a side of the semiconductor structure away from the wafer, wherein the film layer in the stacked film layer structure that is farthest from the semiconductor structure is the first film layer; Thinning the thickness of the first film layer by a chemical mechanical polishing process so that the thickness of the first film layer at the edge of the wafer where the orthographic projection of the first film layer is on the wafer is smaller than the thickness of the first film layer at the middle of the wafer where the orthographic projection of the first film layer is on the wafer; The stacked film structure is patterned to form a plurality of through holes, wherein the through holes are connected to the semiconductor structure.

2. The method for preparing a semiconductor device according to claim 1, wherein: By increasing the pressure at the edge of the grinding head of the chemical mechanical grinding equipment, the pressure at the edge of the grinding head is made greater than the pressure in the middle of the grinding head, so that after the thickness of the first film layer is thinned, the thickness of the first film layer whose orthographic projection on the wafer is located at the edge of the wafer is smaller than the thickness of the first film layer whose orthographic projection on the wafer is located in the middle of the wafer.

3. The method for preparing a semiconductor device according to claim 2, characterized in that: The edge of the wafer is a portion whose distance from the center point of the wafer is greater than or equal to a set value, and the middle portion of the wafer is a portion whose distance from the center point of the wafer is less than a set value.

4. The method for preparing a semiconductor device according to claim 3, characterized in that: The orthographic projection of the edge of the grinding head on the wafer coincides with the edge of the wafer, and the orthographic projection of the middle of the grinding head on the wafer coincides with the middle of the wafer.

5. The method for preparing a semiconductor device according to claim 1, characterized in that: After the thickness of the first film layer is reduced, the first film layer at the edge of the wafer whose orthographic projection is away from the semiconductor structure forms an annular arc surface, and the farther from the center point of the wafer, the thinner the first film layer is.

6. The method for preparing a semiconductor device according to claim 1, wherein: A stacked film layer structure is formed on a side of the semiconductor structure away from the wafer, comprising: forming a first insulating layer on a side of the semiconductor structure away from the wafer; forming a first supporting layer on a side of the first insulating layer away from the semiconductor structure; forming a second insulating layer on a side of the first supporting layer away from the semiconductor structure; forming a second supporting layer on a side of the second insulating layer away from the semiconductor structure; forming a third insulating layer on a side of the second supporting layer away from the semiconductor structure; forming a dielectric layer on a side of the third insulating layer away from the semiconductor structure; forming a third supporting layer on a side of the dielectric layer away from the semiconductor structure; The third supporting layer is the first film layer.

7. The method for preparing a semiconductor device according to claim 6, characterized in that: The stacked film structure is patterned to form a plurality of through holes, comprising: forming a mask layer on a side of the stacked film structure away from the semiconductor structure; forming a photoresist layer on a side of the mask layer away from the semiconductor structure; Using the photoresist layer as a mask, etching the mask layer, the third supporting layer and a portion of the dielectric layer; Using the third supporting layer as a mask, etching the remaining portion of the dielectric layer and a portion of the third insulating layer; The remaining portion of the third insulating layer, the second supporting layer, the second insulating layer, the first supporting layer, and the first insulating layer are etched using the dielectric layer as a mask to form a plurality of the through holes.

8. The method for preparing a semiconductor device according to claim 1, characterized in that: The semiconductor structure includes a capacitor contact structure. After the stacked film layer structure is patterned to form a plurality of through holes, the through holes are connected to the capacitor contact structure so that a side of the capacitor contact structure away from the wafer is exposed.

9. A semiconductor device, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

10. A storage device, characterized in that: Comprising the semiconductor device as claimed in claim 9.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method thereof

    CN110223958A

  • Wiring structure, method for manufacturing the same, electro-optical device, and electronic device

    US20040119899A1