Scandium oxide with hexagonal prism structure and preparation method thereof

By using oxalate and scandium salt to precipitate and roast under the action of cationic dispersant, the problems of high performance stability and cost in scandium oxide preparation are solved, and the preparation of scandium oxide with hexaprismatic structure is realized, and the uniform particle size is improved and purity reduces production costs.

CN114455624BActive Publication Date: 2024-11-19CHINA ENFI ENG CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210210747.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-03
Publication Date
2024-11-19
Estimated Expiration
2042-03-03

AI Technical Summary

Technical Problem

The existing scandium oxide preparation process cannot produce scandium oxide with good performance stability and low cost, and there are particle size unevenness and structural unevenness, which affects product stability and application prospects.

Method used

Under the action of cationic dispersant, soluble scandium salt is precipitated with oxalic acid or oxalate, and the pH value is controlled between 1 and 10, and roasted to obtain scandium oxide with hexaprismatic structure, using the high solubility of oxalate and The surfactivity of the cationic dispersant improves the dispersion of the precipitate and the escape of gas during the calcination process, achieving uniform particle size and high purity.

Benefits of technology

The preparation of scandium oxide with hexaprismatic structure is realized, which improves the performance stability and production cost of the product, reduces energy consumption, simplifies the process flow, and improves the recovery rate of scandium elements and the purity of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114455624B_ABST
    Figure CN114455624B_ABST
Patent Text Reader

Abstract

The present invention provides a scandium oxide having a hexagonal prism structure and a preparation method thereof. Scandium oxide has a hexagonal prism structure, and the preparation method of scandium oxide comprises: under the action of a cationic dispersant, a soluble scandium salt and a precipitant are subjected to a precipitation reaction to obtain a scandium-containing precipitate, wherein the precipitant is oxalic acid and / or oxalate, the pH of the precipitation reaction is 1 to 10, and the mass ratio of scandium ions, precipitants and cationic dispersants in the soluble scandium salt is 1: (1 to 5): (0.0005 to 0.004); and the scandium-containing precipitate is roasted to obtain scandium oxide. Since the scandium-containing precipitate contains only carbon and oxygen elements in addition to the scandium element, these two elements can be converted into gas and escape during the roasting process, so that the obtained scandium oxide has a higher purity. At the same time, the process flow of the method is simple, and the low temperature of the preparation process and the roasting process is achieved, which reduces energy consumption and reduces costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of scandium oxide preparation, and in particular to scandium oxide with a hexagonal prism structure and a preparation method thereof. Background Art

[0002] Scandium oxide (Sc2O3) is one of the more important products of scandium products. Sc2O3 is a white powder, relatively stable in normal temperature air, with a melting point of 920℃ and a density of 3.864g / cm 3 , belonging to the cubic crystal type. Under certain external conditions, Sc2O3 can be made into metal scandium, salts (scandium chloride, scandium fluoride, scandium iodide, scandium oxalate, etc.) and various scandium alloy products. Some of the characteristics of Sc2O3 make it have good applications in aluminum alloys, electric light sources, lasers, catalysts, activators, ceramics and aerospace, and its development prospects are very broad. The microstructure and particle size of the material have an important influence on the performance of the material. Scandium oxide powder materials with different structures can significantly improve the performance of the subsequently prepared metal scandium, scandium salts and scandium-containing alloys, thereby broadening the application prospects of scandium-containing materials.

[0003] The reaction process conditions of scandium salt during precipitation are complex, difficult to operate and control, and the uneven mixing of materials and precipitants causes the pH in local areas to be too small or too large, resulting in different particle sizes and uneven structures of scandium oxide, which seriously affects the stability of scandium oxide powder material products and increases production costs. At the same time, due to the unevenness of the product particle size, the performance of scandium-based materials is seriously affected, thereby limiting the application of scandium oxide powder materials. In addition, the existing scandium oxide preparation processes cannot produce scandium oxide with a hexagonal prism structure that has stable performance and low cost.

[0004] In view of the above problems, it is necessary to provide a method for preparing scandium oxide with a hexagonal structure having good performance stability and low cost. Summary of the invention

[0005] The main purpose of the present invention is to provide a scandium oxide with a hexagonal prism structure and a preparation method thereof, so as to solve the problem that the existing scandium oxide preparation process cannot produce scandium oxide with advantages such as good performance stability and low cost, and cannot produce scandium oxide with a hexagonal prism structure.

[0006] In order to achieve the above-mentioned purpose, the present invention provides a method for preparing scandium oxide on the one hand, wherein the scandium oxide has a hexagonal prism structure, and the method for preparing scandium oxide comprises: under the action of a cationic dispersant, a soluble scandium salt and a precipitant are subjected to a precipitation reaction to obtain a scandium-containing precipitate, wherein the precipitant is oxalic acid and / or oxalate, the pH of the precipitation reaction is 1 to 10, and the mass ratio of scandium ions, the precipitant and the cationic dispersant in the soluble scandium salt is 1:(1 to 5):(0.0005 to 0.004); and the scandium-containing precipitate is roasted to obtain scandium oxide.

[0007] Furthermore, the oxalate precipitant is selected from sodium oxalate and / or potassium oxalate.

[0008] Furthermore, the concentration of scandium ions in the soluble scandium salt is 0.1 to 1.0 mol / L, preferably 0.2 to 0.8 mol / L.

[0009] Furthermore, the pH of the precipitation reaction is 1.3 to 8.0.

[0010] Furthermore, the reaction temperature of the precipitation reaction is 50-95° C., and the reaction time is 20-100 min; preferably, the reaction temperature of the precipitation reaction is 60-85° C., and the reaction time is 30-80 min.

[0011] Furthermore, the temperature of the calcination process is 600-1100° C., preferably 700-1000° C.; the calcination time of the calcination process is 100-400 min, preferably 180-360 min.

[0012] Furthermore, before the calcination process, the method for preparing scandium oxide includes: aging the product obtained in the precipitation reaction process.

[0013] Furthermore, the reaction temperature of the aging process is 50 to 95° C., preferably 70 to 80° C.; the aging time of the aging process is 60 to 300 min, preferably 60 to 240 min.

[0014] Further, the cationic dispersant is selected from one or more of the group consisting of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium bromide and octadecyltrimethylammonium chloride.

[0015] Another aspect of the present application further provides scandium oxide with a hexagonal prism structure, and the scandium oxide with a hexagonal prism structure is prepared using the preparation method provided in the present application.

[0016] By applying the technical solution of the present invention, scandium oxide with a hexagonal prism structure can be prepared. In the preparation method of scandium oxide with a hexagonal prism structure, a soluble scandium salt reacts with a specific precipitant and pH, so that scandium ions and oxalate can be specifically combined, and after a roasting process, a scandium oxide with a hexagonal prism structure is obtained. Since the cationic dispersant has good solubility in aqueous solution and can reduce the surface tension of the precipitate-solution interface, the precipitation reaction under the action of the cationic dispersant is conducive to improving the dispersibility of the scandium-containing precipitate in the reaction system, so that the particle size formed during the roasting process is relatively uniform. At the same time, since the scandium-containing precipitate contains only carbon and oxygen elements in addition to the scandium element, these two elements can be converted into gas escape during the roasting process, so that the obtained scandium oxide has a higher purity. In addition, the preparation method of scandium oxide with a hexagonal prism structure is simple in process flow, and the low temperature of the preparation process and the roasting process is achieved, which reduces energy consumption and reduces costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0018] Figure 1 The SEM image of the hexagonal scandium oxide prepared in Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0020] As described in the background technology, the existing scandium oxide preparation process cannot produce a product having the advantages of good performance stability and low cost, and cannot produce scandium oxide with a hexagonal prism structure. In order to solve the above technical problems, the present application provides a method for preparing scandium oxide, which has a hexagonal prism structure, and the method for preparing scandium oxide comprises: under the action of a cationic dispersant, a soluble scandium salt and a precipitant are subjected to a precipitation reaction to obtain a scandium-containing precipitate, wherein the precipitant is oxalic acid and / or oxalate, the pH of the precipitation reaction is 1 to 10, and the mass ratio of scandium ions, precipitants and cationic dispersants in the soluble scandium salt is 1:(1 to 5):(0.0005 to 0.004); and the scandium-containing precipitate is roasted to obtain scandium oxide.

[0021] When the precipitant is oxalic acid, the soluble scandium salt reacts with oxalic acid to form scandium oxalate hexahydrate precipitate;

[0022] The chemical equation for the precipitation reaction is: 2ScCl3+3H2C2O4(excess)+6H2O=Sc2(C2O4)3·6H2O↓+6HCl;

[0023] During the roasting process of scandium oxalate, scandium oxalate hexahydrate is first dehydrated during the drying process and then undergoes a pyrolysis reaction. The reaction equation involved is:

[0024] Sc2(C2O4)3·6H2O→Sc2(C2O4)3+H2O;

[0025] Sc2(C2O4)3→Sc2O3(hexagonal structure)+CO↑+CO2↑;

[0026] CO+O2→CO2.

[0027] In the above preparation method, a soluble scandium salt is reacted with a specific precipitant and pH, so that the scandium ions and oxalate can be specifically combined, and after a roasting process, a scandium oxide with a hexagonal structure is obtained. Since the cationic dispersant has good solubility in aqueous solution and can reduce the surface tension of the precipitate-solution interface, the precipitation reaction under the action of the cationic dispersant is conducive to improving the dispersibility of the scandium-containing precipitate in the reaction system, so that the particle size formed during the roasting process is relatively uniform. At the same time, since the scandium-containing precipitate contains only carbon and oxygen elements in addition to the scandium element, these two elements can be converted into gaseous escape during the roasting process, so that the obtained scandium oxide has a higher purity. In addition, the above-mentioned preparation method of scandium oxide with a hexagonal structure has a simple process flow, and realizes low temperature of the preparation process and the roasting process, reduces energy consumption, and reduces costs.

[0028] In a preferred embodiment, the oxalate precipitant includes but is not limited to sodium oxalate and / or potassium oxalate. Compared with other oxalates, the above two oxalates have better solubility, so the selection of the above two precipitants is conducive to improving the recovery rate of scandium element and reducing process cost.

[0029] In order to obtain a scandium-containing precipitate, a water-soluble system of scandium ions is selected. In a preferred embodiment, the concentration of scandium ions in the soluble scandium salt is 0.1 to 1.0 mol / L. Compared with other ranges, limiting the concentration of scandium ions in the soluble scandium salt to the above range is conducive to increasing the generation rate of the scandium-containing precipitate and the precipitation rate of the scandium element. Further, in order to improve the generation of the scandium-containing precipitate and the yield of scandium oxide, preferably, the concentration of scandium ions in the soluble scandium salt is 0.2 to 0.8 mol / L.

[0030] In a preferred embodiment, the pH of the precipitation reaction is 1.3 to 8.0. Limiting the pH of the precipitation reaction within the above range is conducive to the precipitation of the scandium-containing precipitate from the reaction system, improving the yield of the scandium-containing precipitate and the yield of scandium oxide, and is also conducive to improving the uniformity of the pH at various locations in the reaction system, thereby improving the uniformity of the particle size of the scandium oxide obtained after the scandium-containing precipitate is calcined. The pH of the above precipitation reaction can be selected to be 1.3, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0.

[0031] In order to accelerate the precipitation reaction rate, improve the yield of the scandium-containing precipitate and the precipitation rate of the scandium element, in a preferred embodiment, the reaction temperature of the precipitation reaction is 50-95°C, and the reaction time is 20-100min. In order to further improve the yield of the scandium-containing precipitate and the precipitation rate of the scandium element. The reaction temperature of the precipitation reaction can be selected from 50°C, 60°C, 70°C, 80°C and 90°C, and the reaction time can be selected from 20min, 30min, 40min, 50min, 60min, 70min, 80min, 90min and 100min. Preferably, the reaction temperature of the precipitation reaction is 60-85°C, and the reaction time is 30-80min.

[0032] The scandium-containing precipitate is pyrolyzed during the roasting reaction to generate scandium oxide with a hexagonal structure. In a preferred embodiment, the temperature of the roasting process is 600 to 1100° C. Compared with other temperature ranges, limiting the temperature of the roasting process to the above range is conducive to further improving the yield of scandium oxide. In order to further improve the purity of scandium oxide with a hexagonal structure, preferably, the temperature of the roasting process is 700 to 1000° C.

[0033] In order to make the raw materials react more fully during the calcination process and improve the yield and purity of the hexagonal scandium oxide, in a preferred embodiment, the calcination time of the calcination process is 100 to 400 minutes. In order to save energy and ensure the calcination efficiency, more preferably, the calcination time is 180 to 360 minutes.

[0034] In a preferred embodiment, before the calcination process, the method for preparing scandium oxide includes: aging the product obtained in the precipitation reaction process. During the aging process, as the small crystals dissolve, the impurities adsorbed, retained or contained in the precipitate will re-enter the solution, which is beneficial to improving the purity of the precipitate and increasing the precipitate particles. The aging reaction can cause more scandium-containing precipitates to precipitate in the precipitation system, thereby further improving the yield of the scandium-containing precipitate and further improving the yield of scandium oxide.

[0035] In a preferred embodiment, the reaction temperature of the aging process is 50-95°C. Compared with other temperature ranges, limiting the reaction temperature of the aging process to the above range can increase the dissolution rate of the precipitate and the diffusion rate of ions in the solution, accelerate the rate of the aging reaction, shorten the aging time, accelerate the formation of the scandium-containing precipitate, and increase the yield of the scandium-containing precipitate and the yield of scandium oxide. In order to further accelerate the aging reaction rate, increase the yield of the scandium-containing precipitate and the yield of scandium oxide, preferably, the reaction temperature of the aging process is 70-80°C.

[0036] In a preferred embodiment, the aging time of the aging process is 60 to 300 minutes. Compared with other time ranges, limiting the aging time within the above range can make the purity of the scandium-containing precipitate higher and improve the yield of the scandium-containing precipitate; further, the preferred aging time is 60 to 240 minutes, which is conducive to making the aging reaction more complete, and is conducive to further improving the yield of the scandium-containing precipitate and the yield of scandium oxide.

[0037] The cationic dispersant may be any of those commonly used in the art. In a preferred embodiment, the cationic dispersant includes, but is not limited to, one or more of the group consisting of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium bromide and octadecyltrimethylammonium chloride. Compared with other types of cationic dispersants, the use of the above cationic dispersants is beneficial to improving the dispersibility of the scandium-containing precipitate in the reaction system, thereby improving the particle size and structural uniformity of the scandium oxide obtained by roasting.

[0038] The present application also provides scandium oxide with a hexagonal prism structure. The scandium oxide with a hexagonal prism structure prepared by the preparation method provided by the present application has a cationic dispersant added during the precipitation process, which improves the dispersibility of the scandium-containing precipitate in the reaction system, so that scandium oxide with a relatively uniform particle size is formed during the roasting process. At the same time, since the scandium-containing precipitate contains only carbon and oxygen elements in addition to the scandium element, these two elements can be converted into gas and escape during the roasting process, so that the obtained scandium oxide has a higher purity.

[0039] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0040] Example 1

[0041] Precipitation reaction: Take 100mL of 1.0mol / L scandium chloride solution, add cationic dispersant (hexadecyltrimethylammonium chloride) at a reaction temperature of 50°C and normal pressure, and then add oxalic acid solution under stirring conditions of 200r / min, and make the mass ratio of scandium ions, oxalic acid and cationic dispersant in the reaction system 1:1:0.0005, and control the pH of the precipitation reaction process to 1.3 by adding an appropriate amount of ammonia water. After adding the oxalic acid precipitant, continue stirring at a temperature of 50°C and a stirring speed of 100r / min for 80min.

[0042] Aging reaction: After the precipitation reaction is completed, the precipitation reaction product is aged at 70°C for 240 minutes.

[0043] Drying treatment: The obtained precipitated product system was filtered and washed with ethanol and pure water for 3 times and 5 times respectively. The obtained precipitate was placed in an oven and dried at 100°C for 300 minutes.

[0044] Calcination reaction: The dried sample is placed in a corundum crucible and calcined at 600°C for 400 min in a muffle furnace. After calcination, the sample is cooled to room temperature with the furnace. The sample is tested and analyzed to find that the scandium oxide powder material prepared under this condition is a hexagonal structure scandium oxide powder material (such as Figure 1 As shown), the D50 of the material is 8μm and the precipitation rate of scandium element is 90%.

[0045] Example 2

[0046] The difference from Example 1 is that the precipitant is sodium oxalate, and the molar ratio of scandium ions, sodium oxalate precipitant and cationic dispersant in the reaction system is 1:1:0.0005.

[0047] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 9 μm; the precipitation rate of the scandium element was 82%.

[0048] Example 3

[0049] The difference from Example 1 is that the precipitant is oxalic acid, and the molar ratio of scandium ions, sodium oxalate precipitant and cationic dispersant in the reaction system is 1:5:0.004.

[0050] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 7.3 μm; the precipitation rate of the scandium element was 87%.

[0051] Example 4

[0052] The difference from Example 1 is that the pH during the precipitation reaction is 8.0.

[0053] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 12 μm; the precipitation rate of the scandium element was 85%.

[0054] Example 5

[0055] The difference from Example 1 is that the pH during the precipitation reaction is 1.0.

[0056] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 7.5 μm; the precipitation rate of the scandium element was 83%.

[0057] Example 6

[0058] The difference from Example 1 is that the cationic dispersant is added at a reaction temperature of 95° C. and normal pressure. After the oxalic acid precipitant is added, stirring is continued at a temperature of 95° C. and a stirring speed of 100 r / min for 20 min.

[0059] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 9.1 μm; the precipitation rate of the scandium element was 87%.

[0060] Example 7

[0061] The difference from Example 1 is that the cationic dispersant is added at a reaction temperature of 70° C. and normal pressure. After the oxalic acid precipitant is added, stirring is continued at a temperature of 70° C. and a stirring speed of 100 r / min for 60 min.

[0062] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 6 μm; the precipitation rate of the scandium element was 92%.

[0063] Example 8

[0064] The difference from Example 1 is that the cationic dispersant is added at a reaction temperature of 100° C. and normal pressure. After the oxalic acid precipitant is added, stirring is continued at a temperature of 100° C. and a stirring speed of 100 r / min for 120 min.

[0065] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 12 μm; the precipitation rate of the scandium element was 79%.

[0066] Example 9

[0067] The difference from Example 1 is that after the precipitation reaction is completed, the aging reaction is carried out at 95° C. for 60 minutes.

[0068] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 9.2 μm; the precipitation rate of the scandium element was 87.4%.

[0069] Example 10

[0070] The difference from Example 1 is that after the precipitation reaction is completed, the aging reaction is carried out at 80° C. for 180 min.

[0071] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 7.6 μm; the precipitation rate of the scandium element was 92.5%.

[0072] Embodiment 11

[0073] The difference from Example 1 is that after the precipitation reaction is completed, the aging reaction is carried out at 110° C. for 30 minutes.

[0074] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 10.7 μm; the precipitation rate of the scandium element was 83.6%.

[0075] Example 12

[0076] The difference from Example 1 is that the temperature of the calcination process is 1050° C. and the calcination time is 180 min.

[0077] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 7.8 μm; the precipitation rate of the scandium element was 88.6%.

[0078] Embodiment 13

[0079] The difference from Example 1 is that the temperature of the calcination process is 700° C. and the calcination time is 360 min.

[0080] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the particle size distribution of the material was D50 of 7.4 μm; the precipitation rate of the scandium element was 91.3%.

[0081] Embodiment 14

[0082] The difference from Example 1 is that the temperature of the calcination process is 900° C. and the calcination time is 180 min.

[0083] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 7.5 μm; the precipitation rate of the scandium element was 91.7%.

[0084] Embodiment 15

[0085] The difference from Example 1 is that the temperature of the calcination process is 500° C. and the calcination time is 60 min.

[0086] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 8.7 μm; the precipitation rate of the scandium element was 83.9%.

[0087] Example 16

[0088] The difference from Example 1 is that the concentration of the scandium chloride solution is 0.1 mol / L.

[0089] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 7.5 μm; the precipitation rate of the scandium element was 91.5%.

[0090] Embodiment 17

[0091] The difference from Example 1 is that the concentration of the scandium chloride solution is 1.4 mol / L.

[0092] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a ... structure, and the D50 of the material was 15μm; the precipitation rate of the scandium element was 84%.

[0093] Comparative Example 1

[0094] The difference from Example 1 is that the precipitating agent is sodium hydroxide.

[0095] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a block-structured scandium oxide powder material with a D50 of 20 μm; and the precipitation rate of the scandium element was 80%.

[0096] Comparative Example 2

[0097] The difference from Example 1 is that the precipitant is oxalic acid, and the molar ratio of scandium ions, sodium oxalate precipitant and cationic dispersant in the reaction system is 1:0.5:0.0045.

[0098] After testing and analyzing the samples, it was found that the scandium oxide powder material prepared under this condition was a scandium oxide powder material with a hexagonal prism structure, and the D50 of the material was 14 μm; the precipitation rate of the scandium element was 60%.

[0099] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0100] By comparing Examples 1 and 2 and Comparative Example 1, it can be seen that scandium oxide with a hexagonal prism structure can be prepared by using the precipitant provided by the present application, while it cannot be prepared by using a strong alkaline precipitant.

[0101] Comparing Examples 1 and 3 with Comparative Example 2, it can be seen that limiting the mass ratio of scandium ions, precipitants and cationic dispersants within the above range can allow the scandium ions and precipitants to undergo precipitation reaction to generate a scandium-containing precipitate, which is beneficial for the final scandium oxide to form a hexagonal prism structure. At the same time, adding the above cationic dispersant can improve the dispersion uniformity of the scandium ions, which is beneficial for the precipitation reaction to proceed more completely.

[0102] By comparing Examples 1, 4 and 5, it can be seen that limiting the pH of the precipitation reaction within the preferred range of the present application is beneficial to the precipitation of the scandium-containing precipitate from the reaction system, improving the yield of the scandium-containing precipitate and the yield of scandium oxide, and is also beneficial to improving the uniformity of the pH at various locations in the reaction system, thereby improving the uniformity of the particle size of the scandium oxide obtained after the scandium-containing precipitate is calcined.

[0103] Comparing Examples 1, 6 to 8, it can be seen that limiting the precipitation reaction temperature and precipitation time to the preferred range of the present application is beneficial to accelerating the precipitation reaction rate and improving the precipitation rate of the scandium element.

[0104] By comparing Examples 1, 9 to 11, it can be seen that, compared with other temperature ranges, limiting the reaction temperature and time of the aging process within the preferred range of the present application is beneficial to increasing the dissolution rate of the precipitate and the diffusion rate of ions in the solution, which can accelerate the rate of the aging reaction, shorten the aging time, accelerate the formation of scandium-containing precipitates, and increase the precipitation rate of the scandium element.

[0105] Comparing Examples 1, 12 to 15, it can be seen that, compared with other temperature ranges, limiting the temperature of the roasting process within the preferred range of the present application is conducive to further improving the yield and purity of scandium oxide. Limiting the time of the roasting process within the above range can make the reaction raw materials react more fully during the roasting process, improve the yield and purity of hexagonal prism structure scandium oxide, and help save energy and improve roasting efficiency.

[0106] Comparing Examples 1, 16 and 17, it can be seen that, compared with other ranges, limiting the concentration of scandium ions in the soluble scandium salt to the preferred range of the present application is beneficial to improving the precipitation rate of the scandium-containing element.

[0107] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0108] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing scandium oxide, characterized in that: The scandium oxide has a hexagonal prism structure, and the preparation method of the scandium oxide includes: Under the action of a cationic dispersant, a soluble scandium salt and a precipitant are subjected to a precipitation reaction to obtain a scandium-containing precipitate, wherein the precipitant is oxalic acid and / or oxalate, the pH of the precipitation reaction is 1 to 10, the reaction temperature of the precipitation reaction is 50 to 95° C., the reaction time is 20 to 100 min, the mass ratio of the scandium ions in the soluble scandium salt, the precipitant and the cationic dispersant is 1:(1 to 5):(0.0005 to 0.004), and the concentration of the scandium ions in the soluble scandium salt is 0.1 to 1.0 mol / L; and calcining the scandium-containing precipitate to obtain the scandium oxide; Before the calcination process, the method for preparing scandium oxide includes: aging the product obtained in the precipitation reaction process, the reaction temperature of the aging process is 70 to 80° C., and the aging time of the aging process is 60 to 240 minutes.

2. The method for preparing scandium oxide according to claim 1, characterized in that: The oxalate precipitant is selected from sodium oxalate and / or potassium oxalate.

3. The method for preparing scandium oxide according to claim 1 or 2, characterized in that: The concentration of scandium ions in the soluble scandium salt is 0.2-0.8 mol / L.

4. The method for preparing scandium oxide according to claim 3, characterized in that: The pH of the precipitation reaction is 1.3-8.

0.

5. The method for preparing scandium oxide according to claim 4, characterized in that: The reaction temperature of the precipitation reaction is 60-85° C., and the reaction time is 30-80 min.

6. The method for preparing scandium oxide according to claim 1 or 2, characterized in that: The temperature of the calcination process is 600-1100°C; The calcination time of the calcination process is 100 to 400 minutes.

7. The method for preparing scandium oxide according to claim 6, characterized in that: The temperature of the calcination process is 700-1000°C.

8. The method for preparing scandium oxide according to claim 6, characterized in that: The roasting time of the roasting process is 180 to 360 minutes.

9. The method for preparing scandium oxide according to claim 1, characterized in that: The cationic dispersant is one or more selected from the group consisting of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium bromide and octadecyltrimethylammonium chloride.

10. Scandium oxide having a hexagonal prism structure, characterized in that: The scandium oxide having a hexagonal prism structure is prepared by the preparation method described in any one of claims 1 to 9.