A ruthenium / phosphorus catalyst and its preparation method and application

Preparation of ruthenium/phosphorus catalysts by solvent thermal reaction method solves the problems of high preparation cost and cumbersome reaction steps of platinum-based catalysts, and achieves efficient electrochemical water decomposition reactions, improves hydrogen and oxygen evolution performance, simplifies the preparation process and reduces the production costs.

CN114522704BActive Publication Date: 2024-11-15HUBEI MOPHOS TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011222748.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-05
Publication Date
2024-11-15
Estimated Expiration
2040-11-05

AI Technical Summary

Technical Problem

In the prior art, the preparation cost of platinum-based catalysts is high, the reaction steps are cumbersome, making it difficult to achieve large-scale application, and the energy consumption of electrolyzed hydrogen production is large, which limits its practical application.

Method used

Ruthenium nanoparticles with uniform particle size at room temperature were prepared by solvent-thermal reaction method. The high adsorption energy of phosphorus elements formed ruthenium phosphorus bonds, regulated the electronic structure of the ruthenium surface, and prepared an efficient ruthenium/phosphorus catalyst for electricity use. Chemical decomposition reaction.

Benefits of technology

It realizes a low-cost and high catalytic activity ruthenium/phosphorus catalyst, which can act as a dual-function catalyst, greatly improves hydrogen evolution and oxygen evolution performance, simplifies the preparation process, reduces production costs, and performs excellent in electrocatalytic full decomposition water reaction. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114522704B_ABST
    Figure CN114522704B_ABST
Patent Text Reader

Abstract

The present invention discloses a ruthenium / phosphorus catalyst and a preparation method and application thereof. The ruthenium / phosphorus catalyst is prepared by the following preparation methods: 1) Synthesis of ruthenium carbon catalyst: mixing a ruthenium salt solution and a solvent uniformly by ultrasonication, adding a carbon carrier and mixing and reacting, and the obtained solid product is a ruthenium carbon catalyst; 2) Phosphation of ruthenium carbon catalyst: mixing a ruthenium carbon catalyst, a phosphorus source and an organic solvent and reacting, and the obtained solid product is a ruthenium / phosphorus catalyst. Also disclosed is the application of the ruthenium / phosphorus catalyst as an electrocatalyst in electrochemical water decomposition. Compared with the prior art, the present invention can achieve the effect of regulating the surface electronic structure of metal ruthenium at room temperature and pressure, thereby obtaining a high-efficiency bifunctional electrocatalytic material with simple synthesis, convenient process and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst materials, and in particular to a ruthenium / phosphorus catalyst and a preparation method and application thereof. Background Art

[0002] Energy shortage and environmental pollution have attracted widespread attention to renewable energy. Hydrogen energy is considered to be an ideal green and clean energy. The high efficiency, low cost and large-scale preparation of hydrogen energy can drive the rapid development of hydrogen fuel cells, new energy vehicles and other fields. Among the hydrogen production technologies currently used, fossil fuel hydrogen production has serious environmental pollution problems, solar photolysis of water hydrogen production has low efficiency and is discontinuous, and water electrolysis hydrogen production technology has great potential in large-scale hydrogen generation. However, the high energy consumption of water electrolysis limits its practical application. Therefore, it is particularly important to find an electrocatalyst with low price and excellent performance. The precious metal platinum is a well-known hydrogen evolution electrocatalyst with excellent performance. Ruthenium dioxide and iridium dioxide are typical oxygen evolution catalysts, but their low reserves and high prices limit their large-scale application.

[0003] Chinese patent CN110860301A premixes ruthenium salt with a phosphorus source and then calcines it at high temperature (850-900°C) to obtain a ruthenium phosphide-supported carbon nanosheet bifunctional electrocatalyst for hydrazine hydrate oxidation-assisted hydrogen production. Chinese patent CN109112563A mixes ruthenium salt with carbon nanotubes by ultrasound and then reduces them with sodium borohydride to obtain a ruthenium / carbon nanotube material, then introduces a phosphorus source into a small sleeve, places it in a quartz tube for high-temperature annealing (650-850°C), and obtains a ruthenium phosphide / carbon nanotube composite material. The catalyst can only be used for hydrogen evolution reaction, and the catalytic performance obtained is still lower than that of commercial platinum carbon. Based on the comparative documents, the present invention obtains ruthenium particles with a uniform particle size of about 3nm in one step by a solvent thermal reaction (80-180°C), and quickly obtains an efficient water electrolysis catalyst by a method of ruthenium phosphide carbon catalyst at room temperature and pressure. Compared with the comparative documents, this method has milder reaction conditions, shorter time, simpler process, and can regulate the electronic structure of the ruthenium surface through phosphating to obtain a dual-function catalyst for hydrogen and oxygen evolution with excellent performance. Summary of the invention

[0004] The existing technical solutions have the disadvantages of high cost, harsh conditions, strong equipment dependence, and difficulty in large-scale application. In order to overcome the defects of the prior art, the present invention aims to solve the technical problems of high preparation cost and complicated reaction steps of conventional platinum and platinum-based alloy catalysts in the prior art, and proposes a solution to replace high-priced platinum-based catalysts, thereby providing a ruthenium / phosphorus catalyst with low cost and high catalytic activity in the electrochemical water decomposition reaction, and its preparation method and application.

[0005] The present invention is based on the principle of regulating the surface electronic structure of ruthenium to achieve the regulation of its catalytic activity, and designs a ruthenium / phosphorus electrocatalyst. Through the high adsorption energy of phosphorus and ruthenium, ruthenium nanoparticles and phosphorus are alloyed on the surface to form ruthenium-phosphorus bonds, thereby achieving the purpose of regulating the surface electronic structure state of ruthenium nanoparticles.

[0006] The technical solution adopted by the present invention is:

[0007] A method for preparing a ruthenium / phosphorus catalyst comprises the following steps:

[0008] 1) Synthesis of ruthenium-carbon catalyst: a ruthenium salt solution and a solvent are mixed by ultrasonication to be uniform, a carbon support is added and mixed to react, and a solid product is obtained as a ruthenium-carbon catalyst;

[0009] 2) Phosphation of ruthenium-carbon catalyst: The ruthenium-carbon catalyst, a phosphorus source and an organic solvent are mixed and reacted to obtain a solid product which is a platinum / phosphorus catalyst.

[0010] Preferably, in step 1) of the preparation method of the ruthenium / phosphorus catalyst, the loading amount of metal ruthenium is 1-50 wt%.

[0011] Preferably, in step 1) of the preparation method of the ruthenium / phosphorus catalyst, the ruthenium salt is at least one of ruthenium chloride, ruthenium acetylacetonate, dichlorotetrakis(triphenylphosphine)ruthenium, tris(triphenylphosphine)dichloride, and dichloro(p-methylisopropylphenyl)triphenylphosphinedichloride.

[0012] Preferably, in step 1) of the preparation method of the ruthenium / phosphorus catalyst, the solvent is N,N-dimethylformamide, N-methylpyrrolidone, toluene, or ethanol.

[0013] Preferably, in step 1) of the preparation method of the ruthenium / phosphorus catalyst, the carbon carrier is at least one of graphite, graphene, carbon black, activated carbon, and carbon nanotubes.

[0014] Preferably, in step 1) of the preparation method of the ruthenium / phosphorus catalyst, the mass ratio of the carbon support, the solvent, and the ruthenium salt is 1:(100-500):(0.01-0.5).

[0015] Preferably, in step 1) of the preparation method of the ruthenium / phosphorus catalyst, after uniform ultrasonic mixing at room temperature, repeated exhaust and deoxygenation operations are performed in a high-pressure reactor, 2-6 MPa hydrogen is filled, and then heated to a reaction temperature of 80-180°C and reacted for 2-10 hours.

[0016] Preferably, in step 1) of the preparation method of the ruthenium / phosphorus catalyst, the mixed reaction is followed by centrifugal separation to obtain a solid product, which is then repeatedly washed with a solvent to obtain a ruthenium-carbon catalyst.

[0017] Preferably, in step 2) of the preparation method of the ruthenium / phosphorus catalyst, the phosphorus source is at least one of elemental phosphorus, inorganic phosphate, trioctyl phosphine, triphenyl phosphine, phosphorus pentoxide, and phosphorus trioxide; further preferably, in step 2), the phosphorus source is at least one of black phosphorus, red phosphorus, monoclinic phosphorus, orange phosphorus, trioctyl phosphine, and triphenyl phosphine.

[0018] Preferably, in step 2) of the preparation method of the ruthenium / phosphorus catalyst, the organic solvent is one or more of ketone reagents, alcohol reagents, ether solvents, ester solvents, ketone solvents, and amide solvents. Further preferably, in step 2), the organic solvent is at least one of methanol, ethanol, propanol, isopropanol, and acetone.

[0019] Preferably, in step 2) of the preparation method of the ruthenium / phosphorus catalyst, the mass ratio of ruthenium in the ruthenium-carbon catalyst, phosphorus in the phosphorus source and the organic solvent is 1:(0.01-1.0):(300-3000).

[0020] Preferably, in step 2) of the preparation method of the ruthenium / phosphorus catalyst, the mixing reaction is specifically an ultrasonic treatment at room temperature for 0.5 min to 20 min.

[0021] An electrocatalyst is a ruthenium / phosphorus catalyst prepared by the above preparation method.

[0022] Application of this electrocatalyst in electrochemical water splitting.

[0023] Preferably, in this application, the electrocatalyst is prepared into a catalyst solution, added into a working substrate electrode to prepare a working electrode, and then a three-electrode system is formed to perform electrochemical hydrogen evolution treatment.

[0024] Preferably, in this application, the concentration of ruthenium in the catalyst solution is 0.1 mg / mL to 1 mg / mL.

[0025] Preferably, in this application, the working substrate electrode is a glassy carbon electrode.

[0026] Preferably, in this application, the counter electrode of the three-electrode system is graphite, and the reference electrode is a mercury / mercury oxide electrode.

[0027] The beneficial effects of the present invention are:

[0028] 1. The present invention uses fewer types of starting raw materials, has a simple preparation process, and greatly reduces production costs.

[0029] 2. The high-pressure solvent thermal method used in the present invention is to prepare the ruthenium-carbon catalyst material, and the ruthenium particles are uniform in size and evenly distributed on the carbon carrier.

[0030] 3. The method of phosphating ruthenium-carbon catalyst at room temperature and pressure adopted by the present invention has a fast reaction and saves time. The content of ruthenium-phosphorus bonds can be regulated by controlling the phosphorus source and the amount added, and the hydrogen evolution and oxygen evolution performance of the ruthenium / phosphorus catalyst can be precisely regulated.

[0031] 4. The ruthenium / phosphorus catalyst prepared by the present invention solves the problem of single catalytic activity of platinum-based catalysts and can be used as a bifunctional catalyst to greatly improve the performance of hydrogen and oxygen evolution and realize the electrocatalytic complete water decomposition reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a projection electron microscope image of the ruthenium-carbon catalyst;

[0033] Figure 2 This is the XRD comparison diagram of ruthenium-carbon catalyst and ruthenium-phosphorus catalyst;

[0034] Figure 3 Comparison of electrochemical hydrogen evolution performance between ruthenium-carbon catalyst and ruthenium-phosphorus catalyst;

[0035] Figure 4 Comparison of electrochemical oxygen evolution performance between ruthenium-carbon catalyst and ruthenium-phosphorus catalyst;

[0036] Figure 5 Photo of complete water splitting over ruthenium-phosphorus catalyst; DETAILED DESCRIPTION

[0037] The present invention is further described in detail below by means of specific examples. Unless otherwise specified, the raw materials used in the examples can be obtained from conventional commercial sources.

[0038] Example 1

[0039] a) Dissolve 38 mg of hydrated ruthenium chloride in 10 mL of N,N-dimethylformamide at room temperature, mix evenly by ultrasonication, add 100 mg of graphene, stir with a magnetic bar, react in a high-pressure reactor, repeatedly fill with hydrogen and evacuate, remove oxygen from the system as much as possible, fill with 4.5 MPa of hydrogen, keep the system pressure constant, start heating to 120°C, and end the reaction after 4 hours of reaction. Collect the solid product by centrifugation, wash once with acetone, and then wash three times with ethanol and water to obtain a ruthenium carbon catalyst.

[0040] b) The obtained ruthenium carbon catalyst is dispersed in ethanol, and the ruthenium content is 1 mg / mL as determined by ICP. 1 mL of the ruthenium carbon catalyst solution is added with 0.2 mL of black phosphorus nanosheet ethanol dispersion (0.1 mg / mL), and then ultrasonically treated at room temperature and pressure for 2-5 minutes to obtain a solid product as a ruthenium / phosphorus catalyst.

[0041] c) Electrocatalytic application: Shanghai Chenhua electrochemical workstation CHI 760E was used for measurement, and the measurement system was a standard three-electrode system. Glassy carbon electrode (0.07 cm 2 ), graphite rod and mercury / mercury oxide electrode are working electrode, counter electrode and reference electrode respectively. In all measurements, the mercury / mercury oxide electrode is calibrated against the reversible hydrogen electrode (RHE). In 1.0 mol / L KOH, E(RHE)=E(SCE)+0.0592*14+0.095V. Take 0.2mL of ruthenium / phosphorus catalyst ethanol dispersion (1mg / mL), mix with 20μL of 5wt% naphthol solution, ultrasonically treat for 2-10 minutes to prepare catalyst slurry, drop 2μL of catalyst slurry onto the surface of glassy carbon electrode, dry naturally at room temperature for electrocatalytic performance test. The hydrogen and oxygen evolution performance of ruthenium / phosphorus catalyst was measured by linear sweep voltammetry, with 5mV s -1 The performance test was carried out at a scanning speed of 100 ℃ and iR drop compensation was performed on all polarization curves.

[0042] Characterization analysis

[0043] The structure of the prepared ruthenium / carbon catalyst was characterized by transmission electron microscopy. Figure 1 This is a transmission electron microscope image of the ruthenium / carbon catalyst. Figure 1 It can be seen that the ruthenium particles are evenly distributed on the substrate surface, and the particle size is about 3-4 nm.

[0044] Figure 2 This is the XRD comparison diagram of ruthenium-carbon catalyst and ruthenium-phosphorus catalyst. The peak of black phosphorus is near 34°. The diffraction peak is severely broadened, which may be due to the small particle size of Ru particles.

[0045] from Figure 3 It can be seen that after phosphating, the electrocatalytic hydrogen evolution performance of the ruthenium-phosphorus catalyst is improved by 3.86 times compared with the ruthenium-carbon catalyst. -2 The overpotentials at current densities of -0.033 V and -0.079 V were respectively, indicating that the electronic structure of Ru full water splitting was effectively regulated after phosphating, and its electrochemical hydrogen evolution performance was greatly improved.

[0046] from Figure 4 It can be seen that after phosphating, the current density of the ruthenium-phosphorus catalyst can reach 10 mA cm at an overpotential of 1.58 V. -2 The electrocatalytic oxygen evolution performance of the ruthenium-carbon catalyst is improved by 4.5 times compared with that of the ruthenium-carbon catalyst, indicating that the phosphating treatment can adjust the adsorption energy between the ruthenium-phosphorus catalyst and oxygen molecules, achieve a significant improvement in performance, and can surpass the oxygen evolution performance of commercial RuO2 under the same conditions.

[0047] from Figure 5It can be seen that when the ruthenium-phosphorus catalyst is used as the cathode and anode respectively, and a double-electrode system is used to carry out a full water splitting experiment, a large number of bubbles can be clearly observed to emerge, indicating that the ruthenium-phosphorus catalyst has dual functionality and can effectively split water to produce hydrogen.

[0048] Example 2

[0049] The difference between this embodiment and embodiment 1 is that in step a), the mass of hydrated ruthenium chloride is 25 mg, the carbon black is 200 mg, and the N,N-dimethylformamide is 15 mL. According to the washing and separation method in embodiment 1, ruthenium particles with uniform size distribution can be obtained.

[0050] Example 3

[0051] The difference between this embodiment and embodiment 1 is that: in step a), the mass of hydrated ruthenium chloride is 50 mg, the activated carbon is 100 mg, the solvent N-methylpyrrolidone is 10 mL, the reaction temperature is 180° C., the reaction time is 2 h, and according to the washing and separation method in embodiment 1, ruthenium particles with uniform size distribution can be obtained.

[0052] Example 4

[0053] The difference between this embodiment and embodiment 1 is that: in step a), the mass of hydrated ruthenium chloride is 50 mg, the graphite is 50 mg, the solvent toluene is 10 mL, the reaction temperature is 100° C., the reaction time is 6 h, and according to the washing and separation method in embodiment 1, ruthenium particles with uniform size distribution can be obtained.

[0054] Example 5

[0055] The difference between this embodiment and embodiment 1 is that: in step a), the mass of hydrated ruthenium chloride is 20 mg, the carbon nanotubes are 90 mg, the solvent ethanol is 10 mL, the reaction temperature is 80° C., the reaction time is 10 h, and according to the washing and separation method in embodiment 1, ruthenium particles with uniform size distribution can be obtained.

[0056] Example 6

[0057] The difference between this embodiment and embodiment 1 is that in step b), the phosphorus source is an ethanol dispersion of red phosphorus (0.1 mg / mL), and the hydrogen and oxygen production effects are lower than those of black phosphorus nanosheets.

[0058] Example 7

[0059] The difference between this embodiment and embodiment 1 is that in step b), the phosphorus source is an ethanol dispersion of monoclinic phosphorus (0.2 mg / mL), the hydrogen production effect is lower than that of black phosphorus nanosheets, and the oxygen production effect is very low.

[0060] Example 8

[0061] The difference between this embodiment and embodiment 1 is that in step b), the phosphorus source is an ethanol dispersion of orange phosphorus (0.05 mg / mL), the hydrogen production effect is lower than that of black phosphorus nanosheets, and the oxygen production effect is very low.

Claims

1. A method for preparing a ruthenium / phosphorus catalyst, characterized in that: The following steps are involved: 1) Synthesis of ruthenium carbon catalyst: ruthenium salt and solvent are mixed by ultrasonic treatment, and then a carbon carrier is added and mixed for reaction. After ultrasonic mixing at room temperature, exhaust and deoxygenate operations are repeatedly performed in a high-pressure reactor, and 2-6 MPa of hydrogen is charged, and then heated to a reaction temperature of 80-180° C. and reacted for 2-10 hours. The solid product obtained is a ruthenium carbon catalyst. The solvent is one of N, N-dimethylformamide, N-methylpyrrolidone, toluene, and ethanol; the carbon carrier is at least one of graphite, graphene, carbon black, activated carbon, and carbon nanotubes; the ruthenium salt is at least one of ruthenium chloride, ruthenium acetylacetonate, dichlorotetrakis(triphenylphosphine)ruthenium, tris(triphenylphosphine)dichloride, and dichloro(p-methylisopropylphenyl)triphenylphosphinedichloride; 2) Phosphation of ruthenium-carbon catalyst: The ruthenium-carbon catalyst obtained in step 1) is mixed with a phosphorus source and an organic solvent to react, and the solid product obtained is a ruthenium / phosphorus catalyst; the phosphorus source is black phosphorus; and the organic solvent is ethanol.

2. The method for preparing a ruthenium / phosphorus catalyst according to claim 1, characterized in that: In step 1), the loading amount of metal ruthenium is 1-50wt%.

3. The method for preparing a ruthenium / phosphorus catalyst according to claim 2, characterized in that: In step 1), the mass ratio of the carbon support, the solvent and the ruthenium salt is 1:(100-500):(0.01-0.5).

4. The method for preparing a ruthenium / phosphorus catalyst according to claim 1, characterized in that: In step 2), the mass ratio of ruthenium in the ruthenium-carbon catalyst, phosphorus in the phosphorus source and the organic solvent is 1:(0.01-1.0):(300-3000).

5. The method for preparing a ruthenium / phosphorus catalyst according to claim 4, characterized in that: In step 2), the mixing reaction is specifically carried out by ultrasonic treatment at room temperature for 0.5 min to 20 min.