Super junction device and manufacturing method
By etching the bottom of the inverted trapezoidal trench of the superjunction device to form a rectangular structure, the voltage withstand problem caused by large charge gap is solved, the voltage withstandability and process stability of the device is improved, and process cost is saved.
Patent Information
- Application Number
- CN202011443290.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-12-08
AI Technical Summary
In the prior art, the etched groove is an inverted trapezoidal structure, resulting in a large charge gap between the superjunction P-type column and the N-type column, affecting the charge balance and voltage resistance of the device.
By etching at the bottom of the inverted trapezoidal groove of the second substrate, the morphology becomes rectangular, thereby narrowing the charge gap between the P-type column and the N-type column, and using the same hard mask as the etching of the inverted trapezoidal groove. Directly etch the bottom of the trench to avoid lithography steps and improve process stability and cost-effectiveness.
The charge balance of the superjunction device is achieved, the voltage withstand performance is improved and the on-resistance is reduced, and the process is stable and cost-saving.
Smart Images

Figure CN114613833B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of semiconductor device design and manufacturing, and in particular relates to a super junction device and a manufacturing method thereof. Background Art
[0002] In the field of power semiconductors, a vertical metal oxide semiconductor field effect transistor (MOSFET) formed by a vertical double diffusion process is called a VDMOSFET, or VDMOS for short. For traditional VDMOS, the breakdown voltage is generally increased by increasing the thickness of the epitaxial layer and reducing the doping concentration of the epitaxial layer. However, this method will significantly increase the resistance of the epitaxial layer. The super junction metal oxide semiconductor field effect transistor (SJ-MOSFET) is an improved structure of the VDMOS device. It forms a P-type column and an N-type column by adding an alternating PN structure in the epitaxial layer. When the device is in a blocking state, the longitudinal electric field in the epitaxial layer is almost constant, which greatly reduces the dependence of the device's on-resistance on the breakdown voltage, thereby reducing the device's on-state loss. Therefore, this structure is widely used in devices with high breakdown voltage. Summary of the invention
[0003] In view of the shortcomings of the prior art described above, the object of the present invention is to provide a super junction device and a manufacturing method, which is used to solve the problem in the prior art that the grooves etched are inverted trapezoidal structures, resulting in a large difference in charge between the super junction P-type columns and N-type columns, which is not conducive to charge balance and causes a decrease in the device's withstand voltage.
[0004] To achieve the above-mentioned purpose and other related purposes, the present invention provides a method for manufacturing a super junction device, the manufacturing method comprising: 1) providing a first substrate, the first substrate comprising a first main surface and a second main surface relative to each other, and forming an oxide layer on the first main surface; 2) providing a second substrate, the second substrate comprising a first main surface and a second main surface relative to each other, bonding the first main surface of the first substrate to the second main surface of the second substrate, and thinning the second substrate from the first main surface of the second substrate; 3) based on a photomask, etching a groove penetrating to the oxide layer on the first main surface of the second substrate by a photolithography-etching process, the groove being in an inverted trapezoidal shape; 4) providing a third substrate, bonding the first main surface of the second substrate to the third substrate; 5) removing the first substrate and removing the oxide layer by etching to expose the bottom of the inverted trapezoidal groove; 6) based on a hard mask plate having the same photomask pattern as that of step 3), directly etching the bottom of the groove after aligning the hard mask plate with the groove to increase the bottom width of the groove so that the morphology of the groove is roughly rectangular.
[0005] Optionally, the bottom width of the groove described in step 3) is between one quarter and three quarters of the top width.
[0006] Optionally, the thickness of the second substrate after thinning is between 1 and 50 microns, the depth of the groove is between 1 and 50 microns, the top width of the groove is between 1 and 6 microns, and the interval between the grooves is between 1 and 10 microns.
[0007] Optionally, the thickness of the second substrate after thinning is between 30 and 45 microns, the depth of the groove is between 30 and 45 microns, the top width of the groove is between 4 and 5 microns, and the interval between the grooves is between 5 and 6 microns.
[0008] Optionally, the etching method of step 3) and step 6) includes one of reactive ion etching (RIE) and deep silicon etching (ICP).
[0009] Optionally, the oxide layer has a thickness between 100 nanometers and 1000 nanometers.
[0010] Optionally, the manufacturing method further includes the step: 7) the second substrate is doped with the first conductivity type, and a semiconductor material layer doped with the second conductivity type is filled in the groove to form a super junction structure together with the second substrate.
[0011] Optionally, the manufacturing method also includes the steps of: 8) forming a second conductive type body region on the super junction structure; 9) forming a first conductive type source region in the second conductive type body region; 10) manufacturing a gate structure on the first conductive type source region and the second conductive type body region; 11) forming an insulating layer and an electrode lead-out structure; wherein the second substrate includes a first conductive type drain region.
[0012] Optionally, step 9) further includes the step of forming a second conductivity type contact region in the first conductivity type source region.
[0013] Optionally, the first conductivity type is N-type, and the second conductivity type is P-type, or the first conductivity type is P-type, and the second conductivity type is N-type.
[0014] The present invention also provides a super junction device, which includes: a first conductive type drain region; a super junction structure located on the first conductive type drain region, including a first conductive type column and a second conductive type column arranged in sequence, and the morphology of the second conductive type column includes a roughly rectangular upper part and an inverted trapezoidal lower part; a second conductive type body region formed on the super junction structure; a first conductive type source region formed in the second conductive type body region; a gate structure formed on the first conductive type source region and the second conductive type body region; an insulating layer and an electrode lead-out structure located on the first conductive type source region and the gate structure.
[0015] Optionally, it also includes a second conductivity type contact region formed in the first conductivity type source region.
[0016] Optionally, the depth of the super junction structure is between 30 and 45 microns.
[0017] Optionally, the first conductivity type is N-type, and the second conductivity type is P-type, or the first conductivity type is P-type, and the second conductivity type is N-type.
[0018] As described above, the super junction device and the manufacturing method of the present invention have the following beneficial effects:
[0019] The present invention bonds a second substrate having an inverted trapezoidal groove formed by etching to a third substrate, thins the back side to expose the bottom of the inverted trapezoidal groove, and then etches from the bottom of the groove with a smaller width to increase the size of the bottom of the groove, thereby making the groove rectangular, thereby reducing the charge difference between the P-type column and the N-type column in the super junction structure, allowing the super junction device to achieve charge balance, thereby improving the voltage resistance performance of the super junction device and reducing the on-resistance of the super junction device.
[0020] The present invention adopts a hard mask having the same pattern as that of etching the inverted trapezoidal groove, directly etches the bottom of the inverted trapezoidal groove to make the groove rectangular, does not need to perform photolithography, and can greatly save process costs.
[0021] The present invention forms an oxide layer on the first substrate in advance, and after removing the first substrate, retains the oxide layer to cover the groove, and then adopts an etching method to remove the oxide layer to expose the groove. Compared with directly grinding to expose the groove, the retained oxide layer can provide support for the groove and its sidewalls during grinding, which can effectively avoid the risk of groove sidewall collapse that is easily caused by direct grinding to expose the groove, thereby improving process stability.
[0022] The super junction device manufactured by the present invention has the advantages of high process stability, strong voltage resistance and low on-resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figures 1 to 12 Shown is a schematic structural diagram of each step of a method for manufacturing a super junction device according to an embodiment of the present invention.
[0024] Component number description
[0025] 101 Second substrate
[0026] 102 Groove
[0027] 103 Third substrate
[0028] 105 Oxide layer
[0029] 106 Hard Mask
[0030] 107 First Substrate
[0031] 201 Leakage Area
[0032] 202 Drain electrode
[0033] 203 N-type column
[0034] 204 P-type column
[0035] 205 Body Area
[0036] 206 Source Area
[0037] 207 Contact Zone
[0038] 208 Gate structure
[0039] 209 Insulation layer
[0040] 210 Electrode lead structure DETAILED DESCRIPTION
[0041] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0042] For example, when describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional view showing the device structure will not be partially enlarged according to the general scale, and the schematic view is only an example, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional space dimensions of length, width and depth should be included.
[0043] For ease of description, spatially relative terms such as "under", "below", "below", "below", "above", "on", etc. may be used herein to describe the relationship of one element or feature shown in the drawings to other elements or features. It will be understood that these spatially relative terms are intended to encompass other orientations of the device in use or operation in addition to the orientation depicted in the drawings. In addition, when a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or one or more intervening layers may also be present.
[0044] In the context of the present application, a structure in which a first feature is described as being "above" a second feature may include embodiments in which the first and second features are formed in direct contact, and may also include embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.
[0045] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and therefore the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0046] The key to superjunction devices achieving high withstand voltage and low on-resistance is to achieve PN charge balance by forming N-type and P-type conductive areas in the substrate. Therefore, the ideal P-type conductive area is a rectangle, but due to the limitation of the etching process, the etched groove can only be an inverted trapezoidal structure, which results in a large difference in charge between the P-type column and the N-type column at different depths, which is not conducive to charge balance and has a certain impact on the withstand voltage of the device.
[0047] In order to solve the problem that there is a large difference in charge between the P-type column 204 and the N-type column 203, which is not conducive to charge balance, this embodiment provides a method for manufacturing a super junction device, and the manufacturing method includes the following steps:
[0048] like Figure 1-2 As shown, firstly, step 1) is performed to provide a first substrate 107 , wherein the first substrate 107 includes a first main surface and a second main surface opposite to each other, and an oxide 105 is formed on the first main surface of the first substrate 107 .
[0049] The first substrate 107 may be a semiconductor substrate such as a silicon substrate, a silicon-germanium substrate, or a germanium substrate. In the present embodiment, the first substrate 107 is a silicon substrate.
[0050] For example, an oxide layer 105 may be formed on the first main surface of the first substrate 107 by using a thermal oxidation process, and the thickness of the oxide layer 107 is between 100 nanometers and 1000 nanometers. Preferably, the thickness of the oxide layer 107 is 200 nm.
[0051] like Figure 3 and Figure 4 As shown, step 2) is then performed to provide a second substrate 101, wherein the second substrate 101 includes a first main surface and a second main surface relative to each other, and the first main surface of the first substrate 107 (i.e., the surface having the oxide layer 105) is bonded to the second main surface of the second substrate 101, and then the second substrate 101 is thinned from the first main surface of the second substrate 101.
[0052] In this embodiment, the second substrate 101 may be a semiconductor substrate such as a silicon substrate, a germanium silicon substrate, or a germanium substrate. In this embodiment, the second substrate 101 is an N-type lightly doped silicon substrate. The thinning method may be a chemical mechanical polishing process. Figure 5 As shown, step 3) is then performed, based on a photomask, a groove 102 penetrating to the oxide layer 105 is etched on the first main surface of the second substrate 101 by a photolithography-etching process, and the groove 102 is in an inverted trapezoidal shape.
[0053] The etching method may be, for example, one of ordinary plasma etching, reactive ion etching RIE and deep silicon etching ICP. Since the groove 102 has a high aspect ratio, such as 10:1 or more, and due to the limitation of the etching process, the sidewall of the etched groove 102 is inclined inward from the top of the groove 102 to the bottom of the groove 102, so that the groove 102 is in an inverted trapezoidal shape. For example, the bottom width of the inverted trapezoidal groove 102 is between one quarter and three quarters of the top width. In a specific implementation process, the bottom width of the inverted trapezoidal groove 102 is one quarter of the top width.
[0054] According to the size requirements of the device, the thickness of the second substrate 101 after thinning is between 1 and 50 microns, the depth of the groove 102 is between 1 and 50 microns, the top width of the groove 102 is between 1 and 6 microns, and the interval between the grooves 102 is between 1 and 10 microns. Preferably, the thickness of the second substrate 101 after thinning is between 30 and 45 microns, for example, it can be specifically 40 microns, the depth of the groove 102 is between 30 and 45 microns, for example, it can be specifically 40 microns, the top width of the groove 102 is between 4 and 5 microns, for example, it can be specifically 5 microns, and the interval between the grooves 102 is between 5 and 6 microns, for example, it can be specifically 6 microns.
[0055] like Figure 6-7 As shown, step 4 is then performed to provide a third substrate 103 and bond the first main surface of the second substrate 101 to the third substrate 103 .
[0056] The third substrate 103 is made of the same material as the second substrate 101 . In this embodiment, the third substrate 103 is an N-type lightly doped silicon substrate.
[0057] In this embodiment, the bonding method of the second substrate 101 and the third substrate 103 may be a silicon-silicon direct bonding process.
[0058] like Figure 8-Figure 9 As shown, step 5 is then performed to remove the first substrate 107 and remove the oxide layer 105 by etching to expose the trench 102 .
[0059] As an example, a method for removing the first substrate 107 may be etching removal, grinding removal, smart-cut removal, laser lift-off removal, etc.
[0060] In this embodiment, the etching solution used in the wet etching has a high selectivity to silicon dioxide and silicon. For example, the etching solution may be hydrofluoric acid (HF).
[0061] The present invention forms an oxide layer 105 on the first substrate 107 in advance. After removing the first substrate 107, the oxide layer 105 is retained to cover the groove 102. Then, the oxide layer 105 is removed by etching to expose the groove 102. Compared with directly grinding to expose the groove 102, the retained oxide layer 105 can provide support for the groove 102 and its side walls during grinding, which can effectively avoid the risk of collapse of the side walls of the groove 102 that is easily caused by direct grinding to expose the groove 102, thereby improving process stability.
[0062] like Figure 10-11As shown, step 6) is then performed. Based on the hard mask plate 106 having the same photomask pattern as that of step 3), after the hard mask plate 106 is aligned with the groove 102, the bottom of the groove 102 is directly etched to increase the bottom width of the groove 102 so that the shape of the groove 102 is roughly rectangular.
[0063] The etching method shown can be one of ordinary plasma etching, reactive ion etching RIE and deep silicon etching ICP. The etching depth can be set to be the same as the depth of the groove 102 to ensure that the morphology of the groove 102 is roughly rectangular, and the roughly rectangular means that the groove 102 is roughly rectangular, which may include a certain degree of morphological change caused by errors caused by technical or process limitations, and such morphological changes should not be excluded from the scope of the claims of this application.
[0064] The present invention uses a hard mask 106 having the same pattern as that of the inverted trapezoidal groove 102 to directly etch the bottom of the inverted trapezoidal groove 102 to make the groove 102 rectangular, without the need for photolithography, which can greatly save process costs.
[0065] like Fig.12 As shown, step 7 is then performed: the second substrate 101 is doped with the first conductivity type, and a semiconductor material layer doped with the second conductivity type is filled in the trench 102 to form a super junction structure together with the second substrate 101.
[0066] For example, the second conductive type doped semiconductor material layer may be a P-type silicon layer, and the P-type silicon layer and the N-type doped second substrate 101 are arranged together to form a super junction structure in which the P-type columns 204 and the N-type columns 203 are alternately arranged.
[0067] The present invention bonds a second substrate 101 having an inverted trapezoidal groove 102 formed by etching to a third substrate 103, thins the back side to expose the bottom of the inverted trapezoidal groove 102, and then etches from the bottom of the groove 102 with a smaller width to increase the size of the bottom of the groove 102, so that the groove 102 is rectangular, thereby reducing the charge difference between the P-type column 204 and the N-type column 203 in the super junction structure, allowing the super junction device to achieve charge balance, thereby improving the voltage resistance performance of the super junction device and reducing the on-resistance of the super junction device.
[0068] like Fig.12 As shown, step 8) is then performed to form a second conductivity type body region 205 on the super junction structure.
[0069] For example, the P-type body region 205 may be formed on the super junction structure by an ion implantation process.
[0070] like Fig.12As shown, step 9) is then performed to form a first conductivity type source region 206 in the second conductivity type body region 205 .
[0071] For example, an N-type source region 206 may be formed in the P-type body region 205 by photolithography and ion implantation. In this step, a P-type contact region 207 may be formed in the N-type source region 206 by ion implantation to facilitate subsequent electrical extraction of the N-type source region 206.
[0072] like Fig.12 As shown, step 10 is then performed to form a gate structure 208 on the first conductivity type source region 206 and the second conductivity type body region 205 .
[0073] like Fig.12 As shown, step 11) is finally performed to form an insulating layer 209 and an electrode lead structure 210.
[0074] It should be noted that, in the present embodiment, a first conductive type drain region 201 is formed in the third substrate 103, and a first conductive type drift region may also be formed on the first conductive type drain region 201. After the first conductive type drift is bonded with the second substrate 101, they jointly form the drift region of the super junction device, and a drain electrode 202 is also formed on the first conductive type drain region 201.
[0075] In this embodiment, the first conductivity type is N type, and the second conductivity type is P type. Of course, in other embodiments, the first conductivity type may also be P type, and the second conductivity type may also be N type.
[0076] like Fig.12 As shown, this embodiment also provides a super junction device, which includes: a first conductive type drain region 201; a super junction structure, located on the first conductive type drain region, including an N-type column 203 and a P-type column 204 arranged in sequence, and the morphology of the P-type column includes a roughly rectangular upper part and an inverted trapezoidal lower part; a second conductive type body region 205, formed on the super junction structure; a first conductive type source region 206, formed in the second conductive type body region 205; a gate structure 208, formed on the first conductive type source region 206 and the second conductive type body region 205; an insulating layer 209 and an electrode lead-out structure 210, located on the first conductive type source region 206 and the gate structure 208.
[0077] In this embodiment, the super junction device further includes a second conductivity type contact region 207 formed in the first conductivity type source region 206 .
[0078] In this embodiment, the depth of the super junction structure is between 30 and 45 microns.
[0079] In this embodiment, the first conductivity type is N type, and the second conductivity type is P type. Of course, in other embodiments, the first conductivity type may also be P type, and the second conductivity type may also be N type.
[0080] As described above, the super junction device and the manufacturing method of the present invention have the following beneficial effects:
[0081] The present invention bonds a second substrate having an inverted trapezoidal groove formed by etching to a third substrate, thins the back side to expose the bottom of the inverted trapezoidal groove, and then etches from the bottom of the groove with a smaller width to increase the size of the bottom of the groove, thereby making the groove rectangular, thereby reducing the charge difference between the P-type column and the N-type column in the super junction structure, allowing the super junction device to achieve charge balance, thereby improving the voltage resistance performance of the super junction device and reducing the on-resistance of the super junction device.
[0082] The present invention adopts a hard mask having the same pattern as that of etching the inverted trapezoidal groove, directly etches the bottom of the inverted trapezoidal groove to make the groove rectangular, does not need to perform photolithography, and can greatly save process costs.
[0083] The present invention forms an oxide layer on the first substrate in advance, and after removing the first substrate, retains the oxide layer to cover the groove, and then adopts an etching method to remove the oxide layer to expose the groove. Compared with directly grinding to expose the groove, the retained oxide layer can provide support for the groove and its sidewalls during grinding, which can effectively avoid the risk of groove sidewall collapse that is easily caused by direct grinding to expose the groove, thereby improving process stability.
[0084] The super junction device manufactured by the present invention has the advantages of high process stability, strong voltage resistance and low on-resistance.
[0085] Therefore, the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.
[0086] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for manufacturing a super junction device, characterized in that: The production method comprises: 1) providing a first substrate, wherein the first substrate comprises a first main surface and a second main surface opposite to each other, and forming an oxide layer on the first main surface; 2) providing a second substrate, wherein the second substrate comprises a first main surface and a second main surface opposite to each other, bonding the first main surface of the first substrate to the second main surface of the second substrate, and thinning the second substrate from the first main surface of the second substrate; 3) Based on a photomask, a groove penetrating to the oxide layer is etched on the first main surface of the second substrate by a photolithography-etching process, wherein the groove is in an inverted trapezoidal shape; 4) providing a third substrate, and bonding the first main surface of the second substrate to the third substrate; 5) removing the first substrate and removing the oxide layer by etching to expose the bottom of the inverted trapezoidal trench; 6) Based on a hard mask plate having the same photomask pattern as that in step 3), after aligning the hard mask plate with the trench, directly etching the bottom of the trench to increase the bottom width of the trench so that the morphology of the trench is roughly rectangular; 7) The second substrate is doped with the first conductivity type, and a semiconductor material layer doped with the second conductivity type is filled in the trench to form a super junction structure together with the second substrate.
2. The method for manufacturing a super junction device according to claim 1, characterized in that: The bottom width of the groove in step 3) is between one quarter and three quarters of the top width.
3. The method for manufacturing a super junction device according to claim 1, characterized in that: The thickness of the second substrate after thinning is between 1 and 50 microns, the depth of the groove is between 1 and 50 microns, the top width of the groove is between 1 and 6 microns, and the interval between the grooves is between 1 and 10 microns.
4. The method for manufacturing a super junction device according to claim 3, characterized in that: The thickness of the second substrate after thinning is between 30 and 45 microns, the depth of the groove is between 30 and 45 microns, the top width of the groove is between 4 and 5 microns, and the interval between the grooves is between 5 and 6 microns.
5. The method for manufacturing a super junction device according to claim 1, characterized in that: The etching method of step 3) and step 6) includes one of reactive ion etching (RIE) and deep silicon etching (ICP).
6. The method for manufacturing a super junction device according to claim 1, characterized in that: The thickness of the oxide layer is between 100 nanometers and 1000 nanometers.
7. The method for manufacturing a super junction device according to claim 1, characterized in that: Also includes the steps: 8) forming a second conductivity type body region on the super junction structure; 9) forming a first conductivity type source region in the second conductivity type body region; 10) Fabricating a gate structure on the first conductive type source region and the second conductive type body region; 11) forming an insulating layer and an electrode lead structure; Wherein, the second substrate includes a first conductivity type drain region.
8. The method for manufacturing a super junction device according to claim 7, characterized in that: Step 9) also includes the step of forming a second conductivity type contact region in the first conductivity type source region.