Semiconductor structure and method for forming semiconductor structure

By designing conductive structures and thicker barrier layers in semiconductor structures, the leakage problem caused by atomic diffusion in the conductive layer is solved, thereby improving the performance of the semiconductor structure.

CN114649294BActive Publication Date: 2024-11-19SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011521350.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-21
Publication Date
2024-11-19
Estimated Expiration
2040-12-21

AI Technical Summary

Technical Problem

In the existing technology, the manufacturing process of local interconnect structure of semiconductor structure needs to be improved, and the performance of the formed semiconductor structure needs to be further improved, especially the leakage problem caused by atomic diffusion in the conductive layer has not been effectively solved.

Method used

A conductive structure is formed within the opening, including an adhesive layer located on the bottom surface and part of the sidewall surface of the opening, and a conductive layer located on the adhesive layer. The top surface of the adhesive layer is lower than the top surface of the dielectric layer, and the top surface of the conductive layer is lower than the top surface of the adhesive layer. A thick barrier layer is formed on the adhesive layer and the conductive layer to block the atomic diffusion of the conductive layer.

Benefits of technology

By combining a thick barrier layer and an adhesive layer, atomic diffusion in the conductive layer is effectively blocked, leakage is reduced, and the performance of the semiconductor structure is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114649294B_ABST
    Figure CN114649294B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the semiconductor structure, the structure comprising: a substrate; a dielectric layer located on the substrate and an opening located in the dielectric layer; a conductive structure located in the opening, the conductive structure comprising an adhesion layer located on the bottom surface and part of the sidewall surface of the opening, and a conductive layer located on the adhesion layer, the top surface of the adhesion layer is lower than the top surface of the dielectric layer, and the top surface of the conductive layer is lower than the top surface of the adhesion layer; a barrier layer located on the adhesion layer and on the conductive layer. The performance of the semiconductor structure is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the semiconductor structure. Background Art

[0002] The metal interconnection structure is an indispensable structure in semiconductor devices, which is used to realize the interconnection between active areas, between transistors, or between metal lines of different layers, and complete the transmission and control of signals. Therefore, in the semiconductor manufacturing process, the formation of the metal interconnection structure has a great influence on the performance of semiconductor devices and the semiconductor manufacturing cost. In order to increase the density of devices, the size of semiconductor devices in integrated circuits has been continuously reduced. In order to realize the electrical connection of each semiconductor device, a multi-layer interconnection structure is usually required.

[0003] Generally, in the back-end interconnection process of the semiconductor device manufacturing process, the first metal layer (M1) needs to form an electrical connection with the active device structure (including the source and drain regions and the gate structure region) of the lower layer. Therefore, before forming the first metal layer, it is usually necessary to pre-form a local interconnection structure (Local Interconnect) of the semiconductor device. The local interconnection structure includes: a zeroth metal layer (M0) electrically connected to the source and drain regions of the lower layer, and a zeroth gate metal layer (M0G) electrically connected to the gate structure.

[0004] However, the manufacturing process of the local interconnect structure in the prior art needs to be improved, and the performance of the formed semiconductor structure needs to be further improved. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the semiconductor structure, so as to improve the performance of the semiconductor structure.

[0006] In order to solve the above technical problems, the technical solution of the present invention provides a semiconductor structure, including: a substrate; a dielectric layer located on the substrate and an opening located in the dielectric layer; a conductive structure located in the opening, the conductive structure including an adhesion layer located on the bottom surface and a portion of the side wall surface of the opening, and a conductive layer located on the adhesion layer, the top surface of the adhesion layer is lower than the top surface of the dielectric layer, and the top surface of the conductive layer is lower than the top surface of the adhesion layer; a barrier layer located on the adhesion layer and on the conductive layer.

[0007] Optionally, the adhesion layer is higher than the conductive layer by more than 2 nanometers.

[0008] Optionally, the barrier layer has a thickness greater than 5 nanometers.

[0009] Optionally, the adhesion layer has a thickness greater than 5 nanometers.

[0010] Optionally, the material of the conductive layer includes metal; the metal includes cobalt.

[0011] Optionally, the material of the adhesion layer includes metal nitride; and the metal nitride includes titanium nitride.

[0012] Optionally, the material of the barrier layer includes a dielectric material; the dielectric material includes a combination of one or more of silicon nitride, silicon carbide, silicon oxycarbide and silicon oxynitride.

[0013] Optionally, the substrate includes: a base; a gate structure located on the base; source and drain doped regions located in the base on both sides of the gate structure; the conductive structure is located on the source and drain doped regions; and the dielectric layer is located on the top and side walls of the gate structure.

[0014] Correspondingly, the technical solution of the present invention also provides a method for forming a semiconductor structure, comprising: providing a substrate; forming a dielectric layer and an opening in the dielectric layer on the substrate; forming a conductive structure in the opening, the conductive structure comprising an adhesion layer located on the bottom surface and a portion of the side wall surface of the opening, and a conductive layer located on the adhesion layer, the top surface of the adhesion layer is lower than the top surface of the dielectric layer, and the top surface of the conductive layer is lower than the top surface of the adhesion layer; forming a barrier layer on the adhesion layer and the conductive layer.

[0015] Optionally, the method for forming the conductive structure includes: forming an initial conductive structure in an opening, the initial conductive structure including an initial adhesion layer located on a side wall surface and a bottom surface of the opening, and an initial conductive layer located on the initial adhesion layer, the dielectric layer exposing a top surface of the initial conductive structure; removing a portion of the initial adhesion layer to form an adhesion layer, the top surface of the adhesion layer being lower than the top surface of the dielectric layer; after forming the adhesion layer, removing a portion of the initial conductive layer to form a conductive structure, the conductive structure including an adhesion layer and a conductive layer located on the adhesion layer, the top surface of the conductive layer being lower than the top surface of the adhesion layer.

[0016] Optionally, the process of removing part of the initial adhesion layer includes a wet etching process, and the etching rate of the initial adhesion layer by the wet etching process is greater than the etching rate of the initial conductive layer; the process parameters of the wet etching process include: the etching liquid is a mixed solution of hydrogen peroxide and ammonia water, and the temperature is greater than 60 degrees Celsius.

[0017] Optionally, the process of removing part of the initial conductive layer includes a first step and a second step of a cycle, wherein the first step oxidizes the surface of the initial conductive layer, and the second step removes the oxidized initial conductive layer; the process of the first step includes a wet etching solution, and the process of the second step includes a wet etching solution.

[0018] Optionally, the wet etching process parameters of the first step include: the etching solution is a mixed solution of hydrogen peroxide and ammonia water, and the temperature is 10 degrees Celsius to 30 degrees Celsius; the wet etching process parameters of the second step include: the etching solution is a mixed solution of hydrofluoric acid and water with a volume ratio of 1:2000, and the temperature is 10 degrees Celsius to 30 degrees Celsius.

[0019] Optionally, the adhesion layer is higher than the conductive layer by more than 2 nanometers.

[0020] Optionally, the barrier layer has a thickness greater than 5 nanometers.

[0021] Optionally, the adhesion layer has a thickness greater than 5 nanometers.

[0022] Optionally, the material of the conductive layer includes metal; the metal includes cobalt.

[0023] Optionally, the material of the adhesion layer includes metal nitride; and the metal nitride includes titanium nitride.

[0024] Optionally, the material of the barrier layer includes a dielectric material; the dielectric material includes a combination of one or more of silicon nitride, silicon carbide, silicon oxycarbide and silicon oxynitride.

[0025] Optionally, the method for forming the barrier layer includes: forming a barrier material layer on the adhesion layer, the conductive layer and the dielectric layer; and planarizing the barrier material layer until the top surface of the dielectric layer is exposed to form the barrier layer.

[0026] Optionally, the reaction temperature for forming the barrier material layer is less than 500 degrees Celsius.

[0027] Optionally, the substrate includes: a base; a gate structure located on the base; source and drain doped regions located in the base on both sides of the gate structure; the conductive structure is located on the source and drain doped regions; and the dielectric layer is located on the top and side walls of the gate structure.

[0028] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0029] The semiconductor structure of the technical solution of the present invention has a conductive structure in the opening, and the conductive structure includes an adhesion layer located on the bottom surface of the opening and part of the side wall surface, and a conductive layer located on the adhesion layer, the top surface of the adhesion layer is lower than the top surface of the dielectric layer, the top surface of the conductive layer is lower than the top surface of the adhesion layer, and there is a barrier layer on the adhesion layer and the conductive layer. On the one hand, the thickness of the barrier layer is relatively thick, so that the barrier layer can block and weaken the diffusion ability of the atoms of the conductive layer, and can shorten the diffusion distance of the atoms of the conductive layer, thereby reducing the atoms of the conductive layer from passing through the barrier layer to diffuse into the semiconductor structure formed subsequently, thereby causing leakage of the semiconductor structure; on the other hand, the adhesion layer plays a good diffusion barrier role for the atoms of the conductive layer, the top surface of the conductive layer is lower than the top surface of the adhesion layer, and the adhesion layer higher than the conductive layer can make the distance of the atoms of the conductive layer diffusing from the barrier layer to the dielectric layer longer, thereby reducing the situation where the atoms of the conductive layer are prone to leakage after entering the dielectric layer. In summary, the performance of the semiconductor structure is improved.

[0030] Furthermore, the range where the adhesion layer is higher than the conductive layer is greater than 2 nanometers. When the range where the adhesion layer is higher than the conductive layer is smaller, the diffusion distance of the atoms of the conductive layer from the barrier layer to the dielectric layer becomes shorter, and the atoms of the conductive layer easily diffuse from the interface between the barrier layer and the conductive layer to the dielectric layer, thereby the blocking effect on the atoms of the conductive layer is insufficient.

[0031] Furthermore, the thickness range of the blocking layer is greater than 5 nanometers. When the thickness of the blocking layer is small, the thickness of the blocking layer is smaller than the diffusion distance of the atoms of the conductive layer. The atoms of the conductive layer will diffuse through the blocking layer into the subsequently formed semiconductor structure, thereby making the blocking effect of the blocking layer on the atoms of the conductive layer insufficient.

[0032] The method for forming a semiconductor structure of the technical solution of the present invention is to first form a conductive structure in an opening, wherein the conductive structure includes an adhesion layer located on the bottom surface and part of the sidewall surface of the opening, and a conductive layer located on the adhesion layer, wherein the top surface of the adhesion layer is lower than the top surface of the dielectric layer, and the top surface of the conductive layer is lower than the top surface of the adhesion layer, and then a barrier layer is formed on the adhesion layer and the conductive layer. On the one hand, the thickness of the barrier layer is relatively thick, so that the barrier layer can block and weaken the diffusion ability of the atoms of the conductive layer, and can shorten the diffusion distance of the atoms of the conductive layer, thereby reducing the atoms of the conductive layer from passing through the barrier layer to diffuse into the semiconductor structure formed subsequently, thereby causing leakage of the semiconductor structure; on the other hand, the adhesion layer plays a good diffusion barrier role for the atoms of the conductive layer, and the top surface of the conductive layer is lower than the top surface of the adhesion layer. The adhesion layer higher than the conductive layer can make the distance of the atoms of the conductive layer diffusing from the barrier layer to the dielectric layer longer, thereby reducing the situation where the atoms of the conductive layer are prone to leakage after entering the dielectric layer. In summary, the performance of the semiconductor structure is improved.

[0033] Furthermore, the range where the adhesion layer is higher than the conductive layer is greater than 2 nanometers. When the range where the adhesion layer is higher than the conductive layer is smaller, the diffusion distance of the atoms of the conductive layer from the barrier layer to the dielectric layer becomes shorter, and the atoms of the conductive layer easily diffuse from the interface between the barrier layer and the conductive layer to the dielectric layer, thereby the blocking effect on the atoms of the conductive layer is insufficient.

[0034] Furthermore, the thickness range of the blocking layer is greater than 5 nanometers. When the thickness of the blocking layer is small, the thickness of the blocking layer is smaller than the diffusion distance of the atoms of the conductive layer. The atoms of the conductive layer will diffuse through the blocking layer into the subsequently formed semiconductor structure, thereby making the blocking effect of the blocking layer on the atoms of the conductive layer insufficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 and Figure 2 is a schematic cross-sectional structural diagram of a semiconductor structure forming process in one embodiment;

[0036] Figures 3 to 8 It is a schematic cross-sectional structure diagram of the semiconductor structure forming process in an embodiment of the present invention. DETAILED DESCRIPTION

[0037] As described in the background art, the manufacturing process of the local interconnect structure in the prior art needs to be improved, and the performance of the formed semiconductor structure needs to be further improved. Now, an analysis and description will be given in conjunction with specific embodiments.

[0038] Figure 1 and Figure 2It is a schematic cross-sectional structure diagram of a semiconductor structure forming process in one embodiment.

[0039] Please refer to Figure 1 , providing a substrate 100; forming a gate structure 101 on the substrate 100; forming source-drain doped regions 102 in the substrate on both sides of the gate structure 101; forming a dielectric layer 103 on the substrate 100; forming an opening (not shown) in the dielectric layer 103, wherein the opening exposes the surface of the source-drain doped region 102; and forming an initial first conductive structure 104 in the opening.

[0040] Please refer to Figure 2 , the initial first conductive structure 104 is etched back to form a first conductive structure 105 and a groove (not shown) located in the dielectric layer 103; a protective layer 106 is formed on the top surface of the first conductive structure 105; and a barrier layer 107 is formed on the protective layer 106.

[0041] During the formation of the semiconductor structure, the material of the barrier layer 107 is different from that of the dielectric layer 103. The barrier layer 107 is used for the subsequent formation of a second conductive structure electrically connected to the gate structure 101, so that the second conductive structure can be self-aligned and formed on the gate structure. The initial first conductive structure 104 is crystalline after annealing, and the surface crystalline state of the first conductive structure 105 formed after back etching is damaged. In addition, the material of the initial first conductive structure 104 is usually cobalt, and the atoms of metal cobalt are relatively active, so the cobalt atoms of the first conductive structure 105 with damaged surface crystalline state are easy to migrate to the barrier layer 107, making the electrical properties of the semiconductor structure unstable and there is a risk of leakage. Therefore, a protective layer 106 is usually formed on the surface of the first conductive structure 105 to prevent the cobalt atoms of the first conductive structure 105 from diffusing into the barrier layer 107. The material of the protective layer 106 is usually titanium, which has good stability. The formation process of the protective layer 106 usually adopts a selective deposition process or a selective electroplating process.

[0042] However, the existing selective deposition process or selective electroplating process will also grow the protection layer 106 on the sidewall of the groove, and it is difficult to form the protection layer 106 located only on the surface of the first conductive structure 105. When the protection layer 106 is located on the sidewall of the groove, since the protection layer 106 is conductive, the protection layer 106 is easy to contact with the second conductive structure formed subsequently and cause a short circuit, thereby affecting the performance of the semiconductor structure.

[0043] In order to solve the above problems, the technical solution of the present invention provides a semiconductor structure and a method for forming the semiconductor structure, wherein a conductive structure is first formed in an opening, wherein the conductive structure includes an adhesion layer located on the bottom surface and part of the sidewall surface of the opening, and a conductive layer located on the adhesion layer, wherein the top surface of the adhesion layer is lower than the top surface of the dielectric layer, and the top surface of the conductive layer is lower than the top surface of the adhesion layer, and then a barrier layer is formed on the adhesion layer and the conductive layer. On the one hand, the barrier layer is thicker, so that the barrier layer can block and weaken the diffusion ability of the atoms of the conductive layer, and can shorten the diffusion distance of the atoms of the conductive layer, thereby reducing the atoms of the conductive layer from passing through the barrier layer to diffuse into the semiconductor structure formed subsequently, thereby causing leakage of the semiconductor structure; on the other hand, the adhesion layer plays a good diffusion barrier role for the atoms of the conductive layer, and the top surface of the conductive layer is lower than the top surface of the adhesion layer. The adhesion layer higher than the conductive layer can make the distance of the atoms of the conductive layer diffusing from the barrier layer to the dielectric layer longer, thereby reducing the situation where the atoms of the conductive layer are prone to leakage after entering the dielectric layer. In summary, the performance of the semiconductor structure is improved.

[0044] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0045] Figures 3 to 8 It is a schematic cross-sectional structure diagram of the semiconductor structure forming process in an embodiment of the present invention.

[0046] Please refer to Figure 3 , providing a substrate; forming a dielectric layer 203 on the substrate.

[0047] The substrate includes: a base 200 ; a gate structure 201 located on the base 200 ; source and drain doped regions 202 located in the base 200 on both sides of the gate structure 201 ; and the dielectric layer 203 located on the top and sidewalls of the gate structure 201 .

[0048] In this embodiment, the gate structure 201 includes a gate dielectric layer (not shown) and a gate layer (not shown) located on the gate dielectric layer. The gate dielectric layer is made of silicon oxide or a low-K (K less than 3.9) material; the gate layer is made of polysilicon.

[0049] In other embodiments, the gate structure further includes a work function layer (not shown), and the work function layer is located between the gate dielectric layer and the gate layer.

[0050] In other embodiments, the material of the gate dielectric layer includes a high dielectric constant material, the dielectric constant of the high dielectric constant material is greater than 3.9, and the high dielectric constant material includes aluminum oxide or hafnium oxide; the material of the gate layer includes a metal, and the metal includes tungsten; the material of the work function layer includes an N-type work function material or a P-type work function material, the N-type work function material includes titanium aluminum, and the P-type work function material includes titanium nitride or tantalum nitride.

[0051] The source-drain doping region 202 has doping ions therein, and the doping ions are of N-type or P-type. The N-type ions include phosphorus ions, arsenic ions, or antimony ions. The P-type ions include boron ions, boron fluoride ions, or indium ions.

[0052] In this embodiment, the material of the substrate 200 is silicon.

[0053] In other embodiments, the material of the substrate includes silicon carbide, silicon germanium, a multinary semiconductor material composed of group III-V elements, silicon on insulator (SOI) or germanium on insulator (GOI). Among them, the multinary semiconductor material composed of group III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP.

[0054] In other embodiments, the substrate further has a fin structure, the gate structure spans the fin structure, and the source and drain doping regions are located in the fin structure on both sides of the gate structure.

[0055] The material of the dielectric layer 203 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbon nitride. In this embodiment, the material of the dielectric layer 203 includes silicon oxide.

[0056] The method and process for forming the gate structure 201 , the source-drain doped regions 202 and the dielectric layer 203 are common technical means in the art and will not be described in detail herein.

[0057] Please refer to Figure 4 , an opening 204 is formed in the dielectric layer 203 .

[0058] In this embodiment, the opening 204 exposes the surface of the source-drain doped region 202 .

[0059] In other embodiments, the opening may also expose the surface of the gate structure.

[0060] The method for forming the opening 204 includes: forming a patterned layer (not shown) on the dielectric layer 203, wherein the patterned layer exposes the surface of the dielectric layer 203 on the source-drain doped region 202; etching the dielectric layer 203 using the patterned layer as a mask until the surface of the source-drain doped region 202 is exposed, thereby forming the opening 204 in the dielectric layer 203.

[0061] The process of etching the dielectric layer 203 includes a dry etching process or a wet etching process. In this embodiment, the process of etching the dielectric layer 203 includes a dry etching process. The dry etching process can form an opening 204 with good sidewall morphology and good dimensional accuracy.

[0062] After the opening 204 is formed, the patterned layer is removed.

[0063] Next, a conductive structure is formed in the opening 204, the conductive structure comprising an adhesion layer 207 located on the bottom surface and part of the sidewall surface of the opening 204, and a conductive layer 208 located on the adhesion layer 207, the top surface of the adhesion layer 207 is lower than the top surface of the dielectric layer 203, and the top surface of the conductive layer 208 is lower than the top surface of the adhesion layer 207. For the formation process of the conductive structure, please refer to Figures 5 to 7 .

[0064] Please refer to Figure 5 An initial conductive structure is formed in the opening 204, wherein the initial conductive structure includes an initial adhesion layer 205 located on the sidewall surface and the bottom surface of the opening 204, and an initial conductive layer 206 located on the initial adhesion layer 205, and the dielectric layer 203 exposes the top surface of the initial conductive structure.

[0065] In this embodiment, the initial conductive structure is located on the source-drain doped region 202 .

[0066] The method for forming the initial conductive structure includes: forming an adhesion material layer (not shown) on the side wall surface and bottom surface of the opening 204 and the surface of the dielectric layer 203; forming a conductive material layer (not shown) on the adhesion material layer; and planarizing the conductive material layer and the adhesion material layer until the surface of the dielectric layer 203 is exposed to form the initial conductive structure.

[0067] The adhesive material layer provides a material layer for an adhesive layer formed subsequently; and the conductive material layer provides a material layer for a conductive layer formed subsequently.

[0068] In this embodiment, the material of the conductive material layer includes metal; the metal includes cobalt. The material of the adhesion material layer includes metal nitride; the metal nitride includes titanium nitride.

[0069] The adhesion material layer provides a seed layer for forming a conductive material layer and serves as an interface transition between the conductive material layer and the dielectric layer 203. The adhesion material layer is also used to block atoms of the conductive material layer from diffusing into the dielectric layer 203 to prevent the insulating effect of the dielectric layer 203 from being affected.

[0070] In this embodiment, the thickness of the adhesion material layer is greater than 5 nanometers. The adhesion material layer within this thickness range has a good effect of blocking atoms of the conductive material layer from diffusing into the dielectric layer 203 .

[0071] Please refer to Figure 6 , removing a portion of the initial adhesion layer 205 to form an adhesion layer 207 , wherein the top surface of the adhesion layer 207 is lower than the top surface of the dielectric layer 203 .

[0072] In this embodiment, the process of removing part of the initial adhesion layer 205 includes a wet etching process, and the etching rate of the initial adhesion layer 205 in the wet etching process is greater than the etching rate of the initial conductive layer 206. The process parameters of the wet etching process include: the etching solution is a mixed solution of hydrogen peroxide and ammonia water, and the temperature is greater than 60 degrees Celsius.

[0073] In other embodiments, the process of removing a portion of the initial adhesion layer includes a dry etching process.

[0074] Please refer to Figure 7 After forming the adhesion layer 207 , a portion of the initial conductive layer 206 is removed to form a conductive structure, wherein the conductive structure includes the adhesion layer 207 and a conductive layer 208 located on the adhesion layer 207 , and the top surface of the conductive layer 208 is lower than the top surface of the adhesion layer 207 .

[0075] The top surface of the conductive layer 208 is lower than the top surface of the adhesion layer 207. The adhesion layer 207 has a good diffusion barrier effect on the atoms of the conductive layer 208. The adhesion layer 207, which is higher than the conductive layer 208, can make the diffusion distance of the atoms of the conductive layer 208 from the subsequently formed barrier layer to the dielectric layer 203 longer, thereby reducing the situation where the atoms of the conductive layer 208 are prone to leakage after entering the dielectric layer 203.

[0076] The process of removing a portion of the initial conductive layer 206 includes a first step and a second step in a cycle, wherein the first step oxidizes the surface of the initial conductive layer 206 , and the second step removes the oxidized initial conductive layer 206 .

[0077] In this embodiment, the process of the first step includes a wet etching solution, and the process of the second step includes a wet etching solution.

[0078] The wet etching process parameters of the first step include: the etching solution is a mixed solution of hydrogen peroxide and ammonia water, and the temperature is 10 degrees Celsius to 30 degrees Celsius; the wet etching process parameters of the second step include: the etching solution is a mixed solution of hydrofluoric acid and water with a volume ratio of 1:2000, and the temperature is 10 degrees Celsius to 30 degrees Celsius.

[0079] In this embodiment, the range of the adhesion layer 207 being higher than the conductive layer 208 is greater than 2 nanometers. If the range of the adhesion layer 207 being higher than the conductive layer is smaller, the distance for the atoms of the conductive layer 208 to diffuse from the subsequently formed barrier layer into the dielectric layer 203 becomes shorter, and the atoms of the conductive layer 208 are easily diffused from the interface between the barrier layer and the conductive layer 208 into the dielectric layer 203, thereby the blocking effect on the atoms of the conductive layer 208 is insufficient.

[0080] Please refer to Figure 8 , a barrier layer 209 is formed on the adhesion layer 207 and the conductive layer 208 .

[0081] The thickness of the blocking layer 209 is relatively thick, so that the blocking layer 209 can block and weaken the diffusion ability of the atoms of the conductive layer 208, and can shorten the diffusion distance of the atoms of the conductive layer 208, thereby reducing the diffusion of the atoms of the conductive layer 208 through the blocking layer 209 to the subsequently formed semiconductor structure, thereby causing leakage of the semiconductor structure.

[0082] The method for forming the barrier layer 209 includes: forming a barrier material layer (not shown) on the adhesion layer 207 , the conductive layer 208 and the dielectric layer 203 ; and planarizing the barrier material layer until the top surface of the dielectric layer 203 is exposed to form the barrier layer 209 .

[0083] The material of the barrier layer 209 includes a dielectric material; the dielectric material includes a combination of one or more of silicon nitride, silicon carbide, silicon oxycarbide and silicon oxynitride. In this embodiment, the material of the barrier layer 209 includes silicon nitride.

[0084] In this embodiment, the reaction temperature for forming the barrier material layer is less than 500 degrees Celsius. If the reaction temperature is higher, the diffusion distance of the atoms of the conductive layer 208 becomes longer, so that the atoms of the conductive layer 208 have the risk of diffusing out of the barrier layer 209 .

[0085] In this embodiment, the thickness of the barrier layer 209 is greater than 5 nanometers. If the thickness of the barrier layer 209 is small, the thickness of the barrier layer 209 is smaller than the diffusion distance of the atoms of the conductive layer 208, and the atoms of the conductive layer 208 will diffuse through the barrier layer 209 into the subsequently formed semiconductor structure, so that the barrier layer 209 has insufficient blocking effect on the atoms of the conductive layer 208.

[0086] Accordingly, the embodiment of the present invention further provides a semiconductor structure, please continue to refer to Figure 8 ,include:

[0087] substrate;

[0088] A dielectric layer 203 located on the substrate and an opening (not shown) located in the dielectric layer 203;

[0089] A conductive structure located in the opening, the conductive structure comprising an adhesion layer 207 located on a bottom surface and a portion of a sidewall surface of the opening, and a conductive layer 208 located on the adhesion layer 207, wherein a top surface of the adhesion layer 207 is lower than a top surface of the dielectric layer 203, and a top surface of the conductive layer 208 is lower than a top surface of the adhesion layer 207;

[0090] A barrier layer 209 is located on the adhesion layer 207 and on the conductive layer 208 .

[0091] In this embodiment, the adhesion layer 207 is higher than the conductive layer 208 by more than 2 nanometers.

[0092] In this embodiment, the thickness of the barrier layer 209 is greater than 5 nanometers.

[0093] In this embodiment, the thickness of the adhesion layer 207 is greater than 5 nanometers.

[0094] In this embodiment, the material of the conductive layer includes metal; the metal includes cobalt.

[0095] In this embodiment, the material of the adhesion layer 208 includes metal nitride; the metal nitride includes titanium nitride.

[0096] In this embodiment, the material of the barrier layer 209 includes a dielectric material; the dielectric material includes a combination of one or more of silicon nitride, silicon carbide, silicon oxycarbide and silicon oxynitride.

[0097] In this embodiment, the substrate includes: a base 200; a gate structure 201 located on the base; source and drain doped regions 202 located in the base 200 on both sides of the gate structure; the conductive structure is located on the source and drain doped regions 202; and the dielectric layer 203 is located on the top and sidewalls of the gate structure 201.

[0098] The semiconductor structure has a conductive structure in the opening, and the conductive structure includes an adhesion layer 207 located on the bottom surface and part of the side wall surface of the opening, and a conductive layer 208 located on the adhesion layer 207, the top surface of the adhesion layer 207 is lower than the top surface of the dielectric layer 203, the top surface of the conductive layer 208 is lower than the top surface of the adhesion layer 207, and a barrier layer 209 is provided on the adhesion layer 207 and the conductive layer 208. On the one hand, the thickness of the barrier layer 209 is relatively thick, so that the barrier layer 209 can block and weaken the diffusion ability of the atoms of the conductive layer 208, and can shorten the diffusion distance of the atoms of the conductive layer 208, thereby reducing the atoms of the conductive layer 208 from diffusing through the barrier layer 209 to the subsequently formed semiconductor structure, thereby causing leakage of the semiconductor structure; on the other hand, the adhesion layer 207 plays a good diffusion barrier role for the atoms of the conductive layer 208, and the top surface of the conductive layer 208 is lower than the top surface of the adhesion layer 207. The adhesion layer 207, which is higher than the conductive layer 208, can make the distance of the atoms of the conductive layer 208 diffusing from the barrier layer 209 to the dielectric layer 203 longer, thereby reducing the situation where the atoms of the conductive layer are prone to leakage after entering the dielectric layer 203. In summary, the performance of the semiconductor structure is improved.

[0099] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A semiconductor structure, characterized in that: include: substrate; a dielectric layer on the substrate and an opening in the dielectric layer; A conductive structure located in the opening, the conductive structure comprising an adhesion layer located on a bottom surface and a portion of a sidewall surface of the opening, and a conductive layer located on the adhesion layer, wherein a top surface of the adhesion layer is lower than a top surface of the dielectric layer, and a top surface of the conductive layer is lower than a top surface of the adhesion layer; A barrier layer is located on the adhesion layer and the conductive layer, and the barrier layer is located in the dielectric layer.

2. The semiconductor structure according to claim 1, wherein: The adhesion layer is higher than the conductive layer by more than 2 nanometers.

3. The semiconductor structure according to claim 1, wherein: The thickness of the barrier layer is in the range of greater than 5 nanometers.

4. The semiconductor structure according to claim 1, wherein: The thickness of the adhesion layer is in the range of greater than 5 nanometers.

5. The semiconductor structure according to claim 1, wherein: The material of the conductive layer includes metal; the metal includes cobalt.

6. The semiconductor structure according to claim 1, wherein: The material of the adhesion layer includes metal nitride; the metal nitride includes titanium nitride.

7. The semiconductor structure according to claim 1, wherein: The material of the barrier layer includes a dielectric material; the dielectric material includes a combination of one or more of silicon nitride, silicon carbide, silicon oxycarbide and silicon oxynitride.

8. The semiconductor structure according to claim 1, wherein: The substrate comprises: a base; a gate structure located on the base; source and drain doping regions located in the base on both sides of the gate structure; the conductive structure is located on the source and drain doping regions; and the dielectric layer is located on the top and sidewalls of the gate structure.

9. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; forming a dielectric layer and an opening in the dielectric layer on a substrate; forming a conductive structure in the opening, the conductive structure comprising an adhesion layer located on a bottom surface and a portion of a sidewall surface of the opening, and a conductive layer located on the adhesion layer, wherein a top surface of the adhesion layer is lower than a top surface of the dielectric layer, and a top surface of the conductive layer is lower than a top surface of the adhesion layer; A barrier layer is formed on the adhesion layer and the conductive layer, and the barrier layer is located in the dielectric layer.

10. The method for forming a semiconductor structure according to claim 9, wherein: The method for forming the conductive structure comprises: forming an initial conductive structure in an opening, the initial conductive structure comprising an initial adhesion layer located on a side wall surface and a bottom surface of the opening, and an initial conductive layer located on the initial adhesion layer, the dielectric layer exposing the top surface of the initial conductive structure; removing a portion of the initial adhesion layer to form an adhesion layer, the top surface of the adhesion layer being lower than the top surface of the dielectric layer; after forming the adhesion layer, removing a portion of the initial conductive layer to form a conductive structure, the conductive structure comprising an adhesion layer and a conductive layer located on the adhesion layer, the top surface of the conductive layer being lower than the top surface of the adhesion layer.

11. The method for forming a semiconductor structure according to claim 10, wherein: The process of removing part of the initial adhesion layer comprises a wet etching process, wherein the etching rate of the initial adhesion layer by the wet etching process is greater than the etching rate of the initial conductive layer; The process parameters of the wet etching process include: the etching solution is a mixed solution of hydrogen peroxide and ammonia water, and the temperature is greater than 60 degrees Celsius.

12. The method for forming a semiconductor structure according to claim 10, wherein: The process of removing part of the initial conductive layer comprises a first step and a second step of a cycle, wherein the first step oxidizes the surface of the initial conductive layer, and the second step removes the oxidized initial conductive layer; The process of the first step includes a wet etching solution, and the process of the second step includes a wet etching solution.

13. The method for forming a semiconductor structure according to claim 12, wherein: The wet etching process parameters of the first step include: the etching solution is a mixed solution of hydrogen peroxide and ammonia water, and the temperature is 10 degrees Celsius to 30 degrees Celsius; the wet etching process parameters of the second step include: the etching solution is a mixed solution of hydrofluoric acid and water with a volume ratio of 1:2000, and the temperature is 10 degrees Celsius to 30 degrees Celsius.

14. The method for forming a semiconductor structure according to claim 9, wherein: The adhesion layer is higher than the conductive layer by more than 2 nanometers.

15. The method for forming a semiconductor structure according to claim 9, wherein: The thickness of the barrier layer is in the range of greater than 5 nanometers.

16. The method for forming a semiconductor structure according to claim 9, wherein: The thickness of the adhesion layer is in the range of greater than 5 nanometers.

17. The method for forming a semiconductor structure according to claim 9, wherein: The material of the conductive layer includes metal; the metal includes cobalt.

18. The method for forming a semiconductor structure according to claim 9, wherein: The material of the adhesion layer includes metal nitride; the metal nitride includes titanium nitride.

19. The method for forming a semiconductor structure according to claim 9, wherein: The material of the barrier layer includes a dielectric material; the dielectric material includes a combination of one or more of silicon nitride, silicon carbide, silicon oxycarbide and silicon oxynitride.

20. The method for forming a semiconductor structure according to claim 9, wherein: The method for forming the barrier layer comprises: forming a barrier material layer on the adhesion layer, the conductive layer and the dielectric layer; and planarizing the barrier material layer until the top surface of the dielectric layer is exposed to form the barrier layer.

21. The method for forming a semiconductor structure according to claim 20, wherein: The reaction temperature for forming the barrier material layer is less than 500 degrees Celsius.

22. The method for forming a semiconductor structure according to claim 9, wherein: The substrate comprises: a base; a gate structure located on the base; source and drain doping regions located in the base on both sides of the gate structure; the conductive structure is located on the source and drain doping regions; and the dielectric layer is located on the top and sidewalls of the gate structure.