A method for purifying primary ferrite products
Through the step-by-step treatment of acetic acid and alkali liquid, impurities in ferrite primary products are effectively removed, the grade and quality of finished ferrite are improved, and the problem of poor impurity removal effect in the prior art is solved. It is suitable for high frequency , low-loss materials, and in line with the concept of green metallurgy.
Patent Information
- Application Number
- CN202011536172.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-12-23
AI Technical Summary
In the prior art, the impurity removal effect in ferrite primary products has poor results, resulting in poor quality and it is difficult to meet the needs of high-frequency and low-loss materials.
The step-by-step treatment of acetic acid and alkali liquid is adopted to remove impurities in the ferrite through solid-liquid separation and multiple treatments, improve the purification effect, and ensure the high quality of the finished ferrite.
It significantly improves the grade of ferrite, reduces the impurity content, is suitable for high-frequency and low-loss materials application fields, and is recycled for leaching medium, which conforms to the concept of green metallurgy and reduces costs.
Smart Images

Figure CN114655994B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ferrite, and in particular to a method for purifying a primary ferrite product. Background Art
[0002] At present, ferrite is an important raw material for high-performance soft magnetic materials. Its resistivity is much greater than that of metal magnetic materials. It can effectively suppress the generation of eddy currents and is widely used in low-loss and high-frequency fields, especially in the fifth-generation mobile communication technology (5G) industry. Ferrite products, which are byproducts of my country's steel industry, contain relatively high levels of impurities such as silicon, calcium, magnesium, manganese, chlorine, and aluminum, resulting in low ferrite quality, making it difficult to meet the demand for high-quality ferrite preparation.
[0003] For example, CN103950988A provides a method for removing impurities from cold-rolled silicon steel red iron oxide, which comprises preparing a 30-60% by mass NaOH aqueous solution, and then alkali-washing the cold-rolled silicon steel red iron oxide for 2-5 hours at a temperature of 140-200°C with the above-mentioned NaOH aqueous solution whose mass is 3-5 times that of the cold-rolled silicon steel red iron oxide, and then separating the solid, washing with water and drying to obtain pure red iron oxide. The method of the present invention has a simple process and low cost, can effectively remove impurities such as SiO2 in red iron oxide, and has strong practicality. The method removes silicon from cold-rolled silicon steel red iron oxide containing 2.0%-7.0% SiO2 (mass percentage) by adopting high pressure and high alkali concentration. This method has high cost and complicated processing process, and does not mention a deep removal method for low silicon content.
[0004] CN103848460A discloses a method for removing silicon from iron oxide powder, a byproduct of iron oxide powder regenerated from pickling waste liquid in a steel plant. It is a method for reducing the impurity silicon content in iron oxide powder and obtaining high-purity iron oxide powder. It includes roasting, alkali leaching, cooling, water washing, suction filtration, drying and water glass recovery, wherein the roasting temperature is 600-800℃, the time is 2-3h; the high-pressure reactor is used for alkali leaching, the concentration of the alkali leaching NaOH solution is 20-40%, the alkali leaching solid-liquid ratio is 1:3-1:4, the temperature is 150-180℃, and the time is 2-3h; the water washing solid-liquid ratio is 1:3-1:5, and the water washing stirring rate is 200-360r / min. The iron oxide powder after silicon removal can be used as a raw material for preparing inorganic pigments, catalysts, permanent magnetic ferrites, and soft magnetic ferrite materials. The method has the advantages of low cost, no pollution, safe and simple operation, simple required equipment, and strong controllability.
[0005] However, the prior art has problems such as poor removal effect of impurities in primary ferrite products, or poor quality of ferrite after impurities are removed. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for purifying a primary ferrite product, which achieves effective removal of impurities, improves the grade of ferrite, and makes the purified ferrite product have good performance.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for purifying a primary ferrite product, the method comprising the following steps:
[0009] (1) mixing the primary ferrite product and the solution containing acetic acid and performing a first treatment to obtain a filter residue through solid-liquid separation;
[0010] (2) The filter residue obtained in step (1) is mixed with alkaline solution and subjected to a second treatment to obtain a purified ferrite product through solid-liquid separation.
[0011] The purification method provided by the present invention can react well by adopting a specific treatment medium, and effectively removes impurities in the primary ferrite product through multiple step-by-step treatments, thereby improving the purification effect. By adopting acetic acid for the first treatment and then performing an alkali treatment, the impurities in the ferrite are fully dissolved without affecting the performance of the product ferrite, and the quality of the finished ferrite is significantly improved. The ferrite is suitable for high-frequency and low-loss material application fields.
[0012] The mixing method of the materials in the present invention can be to pour the alkali solution or the alkali-containing mother solution or the alkali-containing salt solution into a three-necked beaker, and then add the ferrite; or the ferrite is first put into a three-necked beaker, and then the alkali solution or the alkali-containing mother solution or the alkali-containing salt solution mother solution is poured into the three-necked beaker, preferably the alkali solution or the alkali-containing mother solution or the alkali-containing salt solution is poured into the three-necked beaker, and then the ferrite is added; the addition is carried out under stirring, and the speed is 30-800r / min, and the subsequent first treatment and the second treatment maintain the stirring speed for reaction, which is a conventional means in the reaction process. Solid-liquid separation is carried out by centrifugation, suction filtration or filter pressing.
[0013] As a preferred technical solution of the present invention, the solid-to-liquid ratio g / mL of the ferrite primary product and the acetic acid-containing solution in the mixing of step (1) is 1:(0.5-10), for example, it can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5 or 1:10, but is not limited to the listed values, and other unlisted values within the range are also applicable. In the present invention, if too much acid solution is used in the first treatment, it will lead to increased costs, and the acetic acid evaporation treatment capacity is large.
[0014] As a preferred technical solution of the present invention, the molar concentration of acetic acid in the acetic acid-containing solution in step (1) is 1-15 mol / L, for example, it can be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0015] As a preferred technical solution of the present invention, the pH value of the solution obtained by mixing the ferrite primary product and the acetic acid-containing solution in step (1) is 1-2, for example, it can be 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0016] In the present invention, the pH is controlled to be 1-2 to ensure the impurity removal effect while controlling the cost.
[0017] As a preferred technical solution of the present invention, the temperature of the first treatment in step (1) is 20-110°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C or 110°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0018] As a preferred technical solution of the present invention, the time of the first treatment in step (1) is 30-300 min, for example, it can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 100 min, 120 min, 140 min, 160 min, 180 min, 200 min, 220 min, 240 min, 260 min, 280 min or 300 min, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0019] As a preferred technical solution of the present invention, the alkali solution in step (2) includes sodium hydroxide solution and / or potassium hydroxide solution.
[0020] Preferably, the mass concentration of the alkali solution in step (2) is 0.1-500 g / L, for example, it can be 0.1 g / L, 0.5 g / L, 1 g / L, 5 g / L, 10 g / L, 50 g / L, 100 g / L, 150 g / L, 200 g / L, 250 g / L, 300 g / L, 350 g / L, 400 g / L, 450 g / L or 500 g / L, but is not limited to the listed values, and other values not listed within the range are equally applicable.
[0021] As a preferred technical solution of the present invention, the solid-to-liquid ratio of the filter residue and the alkali solution in the mixing of step (2) is 1:(0.5-10) g / mL, for example, it can be 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0022] As a preferred technical solution of the present invention, the reaction temperature of the second treatment in step (2) is 20-110°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C or 110°C, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0023] Preferably, the reaction time of the second treatment in step (2) is 30-300 min, for example, it can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 100 min, 120 min, 140 min, 160 min, 180 min, 200 min, 220 min, 240 min, 260 min, 280 min or 300 min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0024] As a preferred technical solution of the present invention, the purification method comprises the following steps:
[0025] (1) mixing a primary ferrite product and a solution containing acetic acid and then performing a first treatment to obtain a filter residue through solid-liquid separation; the solid-liquid ratio of the primary ferrite product and the solution containing acetic acid in the mixture is 1:(0.5-10) in g / mL; the molar concentration of acetic acid in the solution containing acetic acid is 0.01-15 mol / L; the pH value of the solution obtained after the primary ferrite product and the solution containing acetic acid are mixed is 1-2; the temperature of the first treatment is 20-110° C., and the time is 30-300 min;
[0026] (2) The filter residue obtained in step (1) is mixed with an alkali solution and subjected to a second treatment to obtain a purified ferrite product through solid-liquid separation; the alkali solution comprises a sodium hydroxide solution and / or a potassium hydroxide solution; the mass concentration of the alkali solution is 0.1-500 g / L; the solid-liquid ratio of the filter residue to the alkali solution in the mixture is 1:(0.5-10) in g / mL; the reaction temperature of the second treatment is 20-110° C., and the reaction time of the second treatment is 30-300 min.
[0027] In the present invention, the filtrate obtained in step (1) is evaporated and absorbed before being converted into an acid-containing mother liquor for recycling. In step (2), a calcium compound is added to the filtrate obtained, including any one or a combination of at least two calcium-containing compounds such as calcium oxide, calcium hydroxide, and calcium chloride; an alkaline leaching medium containing the calcium compound is added for precipitation for a period of time, and a calcium slag containing aluminum and silicon is formed in the lower layer, and the supernatant after removing aluminum and silicon is recycled.
[0028] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0029] (1) In view of the low impurity content of the primary ferrite product, the present invention selectively removes silicon, calcium, magnesium, manganese, aluminum and chlorine through an acid method combined with an alkali method to improve the grade of ferrite, which is suitable for high-frequency and low-loss material application fields. The leached medium can be recycled after post-treatment, which conforms to the concept of green metallurgy and reduces costs. The equipment used is relatively conventional, simple and easy to operate, has a wide range of applications, and is very practical.
[0030] (2) The optimal specific chemical composition (mass percentage) of the ferrite after quality improvement treatment is: Fe2O3≥99.52%, SiO2≤0.005%, Al2O3≤0.006%, CaO≤0.008%, MgO≤0.005%, MnO≤0.03%, Cl≤0.05%, achieving its high value. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the purification method provided in Example 1 of the present invention.
[0032] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0033] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0034] Example 1
[0035] This embodiment provides a method for purifying a primary ferrite product. Figure 1 As shown, the following steps are included:
[0036] The main chemical components (mass percentage) of the primary ferrite product are: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0037] (2) Under stirring at a speed of 30 r / min, add ferrite to a three-necked flask into which 1 mol / L acetic acid has been injected at a liquid-solid ratio of 0.5:1 mL / g, ensure that the pH value of the liquid phase is 4, set the reaction temperature constant at 20°C, keep the stirring speed unchanged, and keep it for 30 minutes after reaching the heating temperature;
[0038] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0039] (4) Under stirring at a speed of 30 r / min, add the above solution to a three-necked flask into which 0.1 g / L NaOH solution has been injected, at a liquid-to-solid ratio of mL / g of 0.5:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 20°C, keep the stirring speed unchanged, and keep it for 30 minutes after reaching the heating temperature;
[0040] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0041] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0042] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 70°C. The alkaline medium is recycled after adding calcium oxide to remove aluminum and silicon.
[0043] The main composition of the obtained ferrite product is shown in Table 1.
[0044] Example 2
[0045] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0046] The chemical composition of the primary ferrite product is (mass percentage): Fe2O3 97.8%, SiO2 0.19%, Al2O30.11%, CaO 0.06%, MnO 0.34%, Cl 0.85%;
[0047] (2) Under stirring at a speed of 800 r / min, add ferrite to a three-necked flask into which 15 mol / L acetic acid has been injected at a liquid-to-solid ratio of 10:1, ensuring that the pH value of the liquid phase is 1.0, set the reaction temperature constant at 110°C, keep the stirring speed unchanged, and maintain it for 300 minutes after reaching the heating temperature;
[0048] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0049] (4) Under stirring at a speed of 800 r / min, add the above solution to a three-necked flask into which 80 g / L NaOH solution has been injected at a liquid-to-solid ratio of 10:1 mL / g to obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 110°C, keep the stirring speed unchanged, and keep it for 300 min after reaching the heating temperature;
[0050] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0051] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0052] (7) The acidic medium is converted into an acid-containing mother liquor after evaporation and absorption and then recycled. The volatilization temperature of acetic acid is 150°C. The alkaline medium is recycled after adding calcium oxide to remove aluminum and silicon.
[0053] The main composition of the obtained ferrite product is shown in Table 1.
[0054] Example 3
[0055] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0056] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.32%, Cl 0.85%;
[0057] (2) Under stirring at a speed of 600 r / min, add ferrite to a three-necked flask into which 2 mol / L acetic acid has been injected at a liquid-to-solid ratio of 7:1, mL / g, to ensure that the pH value of the liquid phase is 3.4, set the reaction temperature constant at 50°C, keep the stirring speed unchanged, and maintain it for 180 minutes after reaching the heating temperature;
[0058] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0059] (4) Under stirring at a speed of 600 r / min, add the above solution to a three-necked flask into which 40 g / L NaOH solution has been injected at a liquid-to-solid ratio of 7:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 50° C., keep the stirring speed unchanged, and keep it for 180 minutes after reaching the heating temperature;
[0060] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0061] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0062] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 130°C. The alkaline medium is recycled after adding calcium hydroxide to remove aluminum and silicon.
[0063] The main composition of the obtained ferrite product is shown in Table 1.
[0064] Example 4
[0065] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0066] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0067] (2) Under stirring at a speed of 300 r / min, add ferrite to a three-necked flask into which 5 mol / L acetic acid has been injected at a liquid-solid ratio of 6.2:1 mL / g, ensure that the pH value of the liquid phase is 2.0, set the reaction temperature constant at 90°C, keep the stirring speed unchanged, and maintain it for 180 minutes after reaching the heating temperature;
[0068] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0069] (4) Under stirring at a speed of 300 r / min, add the above solution to a three-necked flask into which 40 g / L KOH solution has been injected at a liquid-to-solid ratio of 6.2:1 mL / g to obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 90°C, keep the stirring speed unchanged, and keep it for 180 min after reaching the heating temperature;
[0070] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0071] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0072] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 120°C. The alkaline medium is recycled after adding calcium chloride to remove aluminum and silicon.
[0073] The main composition of the obtained ferrite product is shown in Table 1.
[0074] Example 5
[0075] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0076] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0077] (2) Under stirring at a speed of 450 r / min, add ferrite to a three-necked flask into which 5 mol / L acetic acid has been injected at a liquid-solid ratio of 5.5:1, ensuring that the pH value of the liquid phase is 2.0, set the reaction temperature constant at 95°C, keep the stirring speed unchanged, and keep it for 240 minutes after reaching the heating temperature;
[0078] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0079] (4) Under stirring at a speed of 450 r / min, add the above solution to a three-necked flask into which 50 g / L Na2CO3 solution has been injected, at a liquid-to-solid ratio of 5.5:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 95°C, keep the stirring speed unchanged, and keep it for 240 min after reaching the heating temperature;
[0080] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0081] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0082] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 80°C. The alkaline medium is recycled after adding calcium oxide to remove aluminum and silicon.
[0083] The main composition of the obtained ferrite product is shown in Table 1.
[0084] Example 6
[0085] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0086] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0087] (2) Under stirring at a speed of 600 r / min, add ferrite to a three-necked flask into which 6 mol / L acetic acid has been injected at a liquid-solid ratio of 5.5:1 mL / g, ensure that the pH value of the liquid phase is 2.0, set the reaction temperature constant at 95°C, keep the stirring speed unchanged, and maintain it for 240 minutes after reaching the heating temperature;
[0088] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0089] (4) Under stirring at a speed of 600 r / min, add the above solution to a three-necked flask into which 50 g / L K2CO3 solution has been injected, at a liquid-to-solid ratio of 5.5:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 95°C, keep the stirring speed unchanged, and keep it for 240 min after reaching the heating temperature;
[0090] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0091] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0092] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 70°C. The alkaline medium is recycled after adding calcium oxide to remove aluminum and silicon.
[0093] The main composition of the obtained ferrite product is shown in Table 1.
[0094] Example 7
[0095] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0096] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0097] (2) Under stirring at a speed of 600 r / min, add ferrite to a three-necked flask into which 8 mol / L acetic acid has been injected at a liquid-to-solid ratio of 5:1, mL / g, to ensure that the pH value of the liquid phase is 1.4, set the reaction temperature constant at 75°C, keep the stirring speed unchanged, and maintain it for 60 minutes after reaching the heating temperature;
[0098] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0099] (4) Under stirring at a speed of 600 r / min, into a three-necked flask into which a 30 g / L Na2CO3+30 g / LNaOH mixed solution (the volume ratio of sodium carbonate solution and sodium hydroxide solution is 1:1) has been injected, the mixed solution is added at a liquid-solid ratio of 5:1 mL / g to obtain a filter cake after solid-liquid reaction and separation. The reaction temperature is set constant at 75°C, the stirring speed is kept unchanged, and the heating temperature is maintained for 60 min after reaching the heating temperature;
[0100] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0101] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0102] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 90°C. The alkaline medium is added with a mixture of calcium oxide and calcium chloride to remove aluminum and silicon and then recycled.
[0103] The main composition of the obtained ferrite product is shown in Table 1.
[0104] Example 8
[0105] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0106] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0107] (2) Under stirring at a speed of 600 r / min, add ferrite to a three-necked flask into which 8 mol / L acetic acid has been injected at a liquid-to-solid ratio of 5:1, mL / g, to ensure that the pH value of the liquid phase is 1.4, set the reaction temperature constant at 75°C, keep the stirring speed unchanged, and maintain it for 60 minutes after reaching the heating temperature;
[0108] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0109] (4) Under stirring at a speed of 600 r / min, into a three-necked flask into which a 35 g / L K2CO3+35 g / LKOH mixed solution (the volume ratio of potassium carbonate solution and potassium hydroxide solution is 1:1) has been injected, the above mixed solution is added at a liquid-solid ratio of 5:1 mL / g, and after reaction and solid-liquid separation, a filter cake is obtained. The reaction temperature is set constant at 75°C, the stirring speed is kept unchanged, and it is maintained for 60 minutes after reaching the heating temperature;
[0110] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0111] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0112] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 90°C. The alkaline medium is recycled after adding calcium hydroxide to remove aluminum and silicon.
[0113] The main composition of the obtained ferrite product is shown in Table 1.
[0114] Example 9
[0115] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0116] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O30.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl: 0.85%;
[0117] (2) Under stirring at a speed of 30 r / min, add ferrite to a three-necked flask into which 4 mol / L acetic acid has been injected at a liquid-solid ratio of 0.8:1, ensuring that the pH value of the liquid phase is 1.8, set the reaction temperature constant at 20°C, keep the stirring speed unchanged, and keep it for 30 minutes after reaching the heating temperature;
[0118] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0119] (4) Under stirring at a speed of 30 r / min, add the above solution to a three-necked flask into which 20 g / L NaOH solution has been injected, at a liquid-to-solid ratio of mL / g of 0.8:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 20°C, keep the stirring speed unchanged, and keep it for 30 minutes after reaching the heating temperature;
[0120] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0121] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0122] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 110°C. The alkaline medium is recycled after adding calcium hydroxide to remove aluminum and silicon.
[0123] The main composition of the obtained ferrite product is shown in Table 1.
[0124] Example 10
[0125] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0126] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0127] (2) Under stirring at a speed of 30 r / min, add ferrite to a three-necked flask into which 7 mol / L acetic acid has been injected at a liquid-solid ratio of 0.8:1 mL / g, ensure that the pH value of the liquid phase is 1.6, set the reaction temperature constant at 20°C, keep the stirring speed unchanged, and keep it for 30 minutes after reaching the heating temperature;
[0128] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0129] (4) Under stirring at a speed of 30 r / min, add the above solution to a three-necked flask into which 60 g / L NaOH solution has been injected at a liquid-to-solid ratio of 0.8:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 20°C, keep the stirring speed unchanged, and keep it for 30 minutes after reaching the heating temperature;
[0130] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0131] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0132] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 120°C. The alkaline medium is recycled after adding calcium oxide to remove aluminum and silicon.
[0133] The main composition of the obtained ferrite product is shown in Table 1.
[0134] Embodiment 11
[0135] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0136] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0137] (2) Under stirring at a speed of 800 r / min, add ferrite to a three-necked flask into which 10 mol / L acetic acid has been injected at a liquid-to-solid ratio of 8:1, ensuring that the pH value of the liquid phase is 1.0, set the reaction temperature constant at 98°C, keep the stirring speed unchanged, and maintain it for 300 minutes after reaching the heating temperature;
[0138] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0139] (4) Under stirring at a speed of 800 r / min, add the above solution to a three-necked flask into which 80 g / L NaOH solution has been injected at a liquid-to-solid ratio of 8:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 98°C, keep the stirring speed unchanged, and keep it for 300 min after reaching the heating temperature;
[0140] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0141] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0142] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 130°C. The alkaline medium is recycled after adding calcium oxide to remove aluminum and silicon.
[0143] The main composition of the obtained ferrite product is shown in Table 1.
[0144] Example 12
[0145] This embodiment provides a method for purifying a primary ferrite product, comprising the following steps:
[0146] The chemical composition (mass percentage) of the primary ferrite product is: Fe2O3 97.8%, SiO2: 0.19%, Al2O3 0.11%, CaO 0.06%, MgO 0.03%, MnO 0.34%, Cl 0.85%;
[0147] (2) Under stirring at a speed of 800 r / min, add ferrite to a three-necked flask into which 15 mol / L acetic acid has been injected at a liquid-to-solid ratio of 8:1, ensuring that the pH value of the liquid phase is 1.0, set the reaction temperature constant at 98°C, keep the stirring speed unchanged, and maintain it for 300 minutes after reaching the heating temperature;
[0148] (3) After the reaction, the ferrite and the acid are separated into solid and liquid by suction filtration;
[0149] (4) Under stirring at a speed of 800 r / min, add the above solution to a three-necked flask into which 80 g / L NaOH solution has been injected at a liquid-to-solid ratio of 8:1, and obtain a filter cake after reaction and solid-liquid separation. Set the reaction temperature to be constant at 98°C, keep the stirring speed unchanged, and keep it for 300 min after reaching the heating temperature;
[0150] (5) After the reaction, the ferrite and the alkali are separated into solid and liquid by suction filtration;
[0151] (6) The final filter cake is then washed with heated ultrapure water, filtered, and dried to obtain the finished ferrite;
[0152] (7) The acidic medium is converted into an acid-containing mother liquor for recycling after evaporation and absorption. The volatilization temperature of acetic acid is 140°C. The alkaline medium is recycled after adding calcium oxide to remove aluminum and silicon.
[0153] The main composition of the obtained ferrite product is shown in Table 1.
[0154] Comparative Example 1
[0155] The only difference from Example 1 is that the acetic acid in step (1) is replaced by sulfuric acid of equal concentration. The main composition of the obtained ferrite product is shown in Table 1.
[0156] Comparative Example 2
[0157] The only difference from Example 1 is that the acetic acid in step (1) is replaced by a sodium hydroxide solution of equal concentration. The main composition of the obtained ferrite product is shown in Table 1.
[0158] Comparative Example 3
[0159] The only difference from Example 1 is that the pH of the liquid phase in step (2) is 3. The main composition of the obtained ferrite product is shown in Table 1.
[0160] Table 1
[0161] composition <![CDATA[Fe2O3 / %]]> <![CDATA[SiO2 / %]]> <![CDATA[Al2O3 / %]]> CaO / % MgO / % MnO / % Cl / % Example 1 98.89 0.075 0.054 0.018 0.018 0.032 0.08 Example 2 99.52 0.005 0.006 0.008 0.005 0.003 0.05 Example 3 98.94 0.015 0.013 0.026 0.026 0.001 0.05 Example 4 99.15 0.092 0.012 0.015 0.011 0.014 0.048 Example 5 99.23 0.065 0.011 0.011 0.009 0.013 0.039 Example 6 99.33 0.062 0.010 0.009 0.008 0.011 0.039 Example 7 99.39 0.058 0.009 0.009 0.008 0.010 0.042 Example 8 99.41 0.055 0.008 0.009 0.008 0.009 0.042 Example 9 98.93 0.075 0.053 0.028 0.022 0.102 0.039 Example 10 99.01 0.025 0.091 0.028 0.012 0.112 0.038 Embodiment 11 99.42 0.038 0.009 0.009 0.008 0.016 0.05 Example 12 99.46 0.039 0.007 0.008 0.005 0.004 0.044 Comparative Example 1 97.95 0.175 0.154 0.05 0.03 0.32 0.082 Comparative Example 2 97.92 0.184 0.103 0.06 0.03 0.34 0.082 Comparative Example 3 97.94 0.185 0.104 0.059 0.029 0.31 0.083
[0162] It can be seen from the results of the above embodiments and comparative examples that the impurity content of the primary ferrite product is low. The present invention selectively removes silicon, calcium, magnesium, manganese, aluminum and chlorine by acid method combined with alkali method to improve the grade of ferrite, which is suitable for high-frequency and low-loss material application fields. The leached medium can be recycled after post-treatment, which conforms to the concept of green metallurgy and reduces costs. The equipment used is relatively conventional, simple and easy to operate, has a wide range of applications, and is very practical.
[0163] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0164] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0165] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0166] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for purifying a primary ferrite product, characterized in that: The purification method comprises the following steps: (1) mixing the primary ferrite product and the solution containing acetic acid and performing a first treatment to obtain a filter residue through solid-liquid separation; (2) mixing the filter residue obtained in step (1) with an alkali solution and performing a second treatment to obtain a purified ferrite product through solid-liquid separation; In step (1), the solid-to-liquid ratio of the primary ferrite product to the solution containing acetic acid is 1:(0.5-10) in g / mL; the molar concentration of acetic acid in the solution containing acetic acid is 1-15 mol / L; the pH value of the solution obtained after the primary ferrite product and the solution containing acetic acid are mixed is 1-2; The alkali solution in step (2) includes sodium hydroxide solution and / or potassium hydroxide solution, the mass concentration of the alkali solution is 0.1-500 g / L, and the solid-to-liquid ratio of the filter residue and the alkali solution in the mixture in step (2) is 1:(0.5-10) in g / mL.
2. The purification method according to claim 1, characterized in that: The temperature of the first treatment in step (1) is 20-110°C.
3. The purification method according to claim 1, characterized in that: The time of the first treatment in step (1) is 30-300 min.
4. The purification method according to claim 1, characterized in that: The reaction temperature of the second treatment in step (2) is 20-110°C.
5. The purification method according to claim 1, characterized in that: The reaction time of the second treatment in step (2) is 30-300 min.
6. The purification method according to any one of claims 1 to 5, characterized in that: The purification method comprises the following steps: (1) mixing a primary ferrite product and a solution containing acetic acid, and then performing a first treatment to obtain a filter residue through solid-liquid separation; the solid-liquid ratio of the primary ferrite product and the solution containing acetic acid in the mixture is 1:(0.5-10) in g / mL; the molar concentration of acetic acid in the solution containing acetic acid is 1-15 mol / L; the pH value of the solution obtained after the primary ferrite product and the solution containing acetic acid are mixed is 1-2; the temperature of the first treatment is 20-110° C., and the time is 30-300 min; (2) The filter residue obtained in step (1) is mixed with an alkali solution and subjected to a second treatment to obtain a purified ferrite product through solid-liquid separation; the alkali solution comprises a sodium hydroxide solution and / or a potassium hydroxide solution; the mass concentration of the alkali solution is 0.1-500 g / L; the solid-liquid ratio of the filter residue to the alkali solution in the mixture is 1:(0.5-10) in g / mL; the reaction temperature of the second treatment is 20-110° C., and the reaction time of the second treatment is 30-300 min.