A tough SLA photosensitive resin for 3D printing and its preparation method

By converting polycarbonate polyol into polycarbonate acrylate and combining it with other resin components, SLA toughness photosensitive resin for 3D printing was prepared, which solved the problem in the existing technology of the decrease in hardness and tensile strength caused by the increase in toughness, and achieved The material's high toughness and stability are suitable for rapid prototyping and anti-aging of 3D printed products.

CN114675491BActive Publication Date: 2024-10-15SUZHOU XINLEIMENG INTELLIGENT MFG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210484546.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-06
Publication Date
2024-10-15
Estimated Expiration
2042-05-06

AI Technical Summary

Technical Problem

When improving the toughness of existing 3D printing photocurable resins, it is easy to cause a decrease in hardness and tensile strength, which limits its large-scale application.

Method used

Convert polycarbonate polyol into polycarbonate acrylate, and use it as the main resin to introduce SLA photocuring system, combining epoxy resin, acrylate oligomer, photoinitiator, modifying additives and auxiliaries, through ester chemical reaction to prepare SLA tough photosensitive resin for 3D printing.

Benefits of technology

It achieves high toughness and stability of the material, maintains hardness and tensile strength, and ensures the rapid prototyping and anti-aging properties of 3D printed products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003628715690000111
    Figure BDA0003628715690000111
  • Figure BDA0003628715690000121
    Figure BDA0003628715690000121
  • Figure BDA0003628715690000122
    Figure BDA0003628715690000122
Patent Text Reader

Abstract

The present invention discloses a SLA tough photosensitive resin for 3D printing, comprising the following raw materials in parts by weight: 40-60% epoxy resin oligomer, 10-35% acrylate oligomer, 7% photoinitiator, 5% modified additive, 3% auxiliary agent, the sum of the mass percentages of the above components is 100%, and the acrylate oligomer includes polycarbonate acrylate. The preparation method of the photosensitive resin is: epoxy resin oligomer, acrylate oligomer, photoinitiator, modified additive, and auxiliary agent are fully mixed according to a certain weight percentage; fully stirred at room temperature for 60-120 minutes to obtain the SLA tough photosensitive resin for 3D printing. The SLA tough photosensitive resin for 3D printing of the present invention has the advantages of low viscosity, low shrinkage, and fast printing rate, and has stable mechanical properties and excellent anti-aging performance, which ensures the rapid prototyping of 3D printed products, and the final product has excellent yellowing resistance and better strength and size retention characteristics in a humid environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of 3D printing materials, and in particular to a SLA tough photosensitive resin for 3D printing and a preparation method thereof. Background Art

[0002] 3D printing is an additive manufacturing method. It is a technology that uses 3D digital model files as the basis, uses powdered metal or plastic and other bondable materials, and constructs objects by printing layer by layer. 3D printing has the advantages of short manufacturing cycle, material saving and energy saving. For the molding of complex structures, it has irreplaceable advantages over traditional technologies. It can be highly integrated with computer artificial intelligence, which has brought revolutionary impacts to traditional manufacturing and is one of the iconic technologies of the new round of industrial revolution. Typical 3D printing processes include: stereolithography (SLA), laminated object manufacturing (LOM), fused deposition modeling (FDM), selective laser sintering (SLS), etc. Among various 3D printing technologies, light-curing 3D printing technology has become the most widely used 3D printing technology due to its high molding accuracy, fast speed, low surface roughness, and environmental friendliness. It can be widely used in aerospace, consumer products, ships, medical rapid prototyping and DIY design.

[0003] In the laser forming SLA resin industry, since photosensitive resin does not require processing techniques such as heating and high pressure, but is formed into a preset model by stacking layers, it has the defects of brittleness and poor mechanical properties, which limits its large-scale application.

[0004] At present, the market usually adds polycarbonate polyols to the photosensitive resin formula system to improve the toughness and impact strength of 3D printed parts. Polycarbonate diol has hydroxyl groups (-OH) at both ends of the molecular chain, and the main chain of the molecule contains aliphatic alkylene and carbonate (-OC=OO-) repeating units. Its main purpose is to form the soft segment in the polyurethane molecular structure and improve the flexibility and toughness of PU.

[0005] Compared with traditional polyester polyols and polyether polyols, thermoplastic polyurethane synthesized from polycarbonate diols has better hydrolysis resistance, heat resistance, weather resistance, and resistance to oxidative degradation. In addition, the polycarbonate group has a high polarity, so polycarbonate polyols as the polyurethane soft segment structure will have a strong intermolecular force, giving it excellent mechanical properties. Therefore, polycarbonate polyols are widely used in the production of high-end polyurethane products. Compared with other polyether and polyester polyurethanes, polycarbonate polyurethanes have the best performance.

[0006] In 3D printing photocurable resins, polycarbonate polyols are generally added as a small amount of additives, which can improve the mechanical properties of the material, but they cannot be introduced into the material as the main structure to improve the performance of the material. If the addition amount is >3%, a large amount of polycarbonate will not participate in the photocuring reaction (this is because polycarbonate polyols can neither participate in the cationic curing epoxy system nor the free radical curing acrylate system), and will remain in the system, which will cause the hardness and tensile strength of the material to drop significantly.

[0007] The present invention aims to convert polycarbonate polyol into polycarbonate acrylate and introduce it as a main resin into a light-curing SLA resin system, thereby improving the toughness of the material without losing the hardness, tensile strength and other properties of the material. Summary of the invention

[0008] To solve the above problems, the object of the present invention is to provide a SLA tough photosensitive resin for 3D printing and a preparation method thereof. The photosensitive resin material has a fast curing rate, high printing accuracy, and the printed parts have good stability and high toughness.

[0009] To achieve the above-mentioned object, the present invention provides a SLA tough photosensitive resin for 3D printing, wherein the SLA tough photosensitive resin comprises the following raw materials in parts by weight: 40-60% epoxy resin oligomer, 10-35% acrylate oligomer, 7% photoinitiator, 5% modification additive, 3% auxiliary agent, and the sum of the mass percentages of the above components is 100%, and the acrylate oligomer comprises polycarbonate acrylate.

[0010] The above-mentioned SLA tough photosensitive resin for 3D printing, preferably, the polycarbonate acrylate is obtained by esterification reaction of polycarbonate polyether polyol and acrylic acid.

[0011] In the above-mentioned SLA tough photosensitive resin for 3D printing, preferably, the molar ratio of the polycarbonate polyether polyol to acrylic acid is 1:2-6.

[0012] In the above-mentioned SLA tough photosensitive resin for 3D printing, preferably, an inhibitor and a catalyst are also added in the esterification reaction between the polycarbonate polyether polyol and acrylic acid.

[0013] The above-mentioned SLA tough photosensitive resin for 3D printing, preferably, the epoxy resin oligomer is one or a mixture of several of bisphenol A epoxy resin (DYD-128), 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate (2021P), hydrogenated bisphenol A epoxy resin (HE-2025), and 3-ethyl-3-oxetanemethanol (M0X-101).

[0014] The above-mentioned SLA tough photosensitive resin for 3D printing, preferably, the acrylate oligomer also includes one or a mixture of several of epoxy acrylate (CN104NS), trimethylolpropane triacrylate (SR351NS), ethoxylated trimethylolpropane triacrylate (SR499NS), propoxylated neopentyl glycol diacrylate (SR9003NS).

[0015] In the above-mentioned SLA tough photosensitive resin for 3D printing, preferably, the photoinitiator is a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate (1176) and / or hydroxycyclohexyl phenyl ketone (184).

[0016] In the above-mentioned SLA toughened photosensitive resin for 3D printing, preferably, the modified additive is a core-shell toughened modified resin (EPX-125).

[0017] In the above-mentioned SLA tough photosensitive resin for 3D printing, preferably, the auxiliary agent is one or a mixture of carboxyl-terminated liquid nitrile rubber (CTBN), hydroxyl-terminated liquid nitrile rubber (HTBN), and polyether polyol (LEP4801).

[0018] The present invention also provides a method for preparing the above-mentioned SLA tough photosensitive resin for 3D printing, which comprises the following steps: (1) fully mixing epoxy resin oligomer, acrylate oligomer, photoinitiator, modification additive and auxiliary agent according to a certain weight percentage; (2) fully stirring at room temperature for 60 to 120 minutes to obtain the SLA tough photosensitive resin for 3D printing.

[0019] The beneficial effects of the present invention are:

[0020] The SLA tough photosensitive resin for 3D printing of the present invention has the advantages of low viscosity, low shrinkage, and fast printing rate, and has stable mechanical properties and excellent anti-aging properties, thereby ensuring the rapid prototyping of 3D printed products.

[0021] The preparation method has simple and efficient steps and is easy to promote and apply.

[0022] The SLA tough photosensitive resin product for 3D printing of the present invention has excellent yellowing resistance and better strength and size retention properties in a humid environment. DETAILED DESCRIPTION

[0023] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0024] The invention discloses an SLA tough photosensitive resin for 3D printing, which comprises the following raw materials in parts by weight: 40-60% of epoxy resin oligomer, 10-35% of acrylate oligomer, 7% of photoinitiator, 5% of modification additive, and 3% of auxiliary agent, wherein the sum of the mass percentages of the above components is 100%, wherein the acrylate oligomer comprises polycarbonate acrylate.

[0025] Polycarbonate acrylate (POLYPCE-DA) is obtained by esterification of polycarbonate polyether polyol and acrylic acid.

[0026] The molecular weight of the polycarbonate polyether polyol is preferably 1000-4000, the molar ratio of the polycarbonate polyether polyol to acrylic acid is preferably 1:2-6, and an inhibitor and a catalyst are also added to the above-mentioned esterification reaction, the inhibitor preferably includes one or more of p-hydroxyanisole, hydroquinone, and p-tert-butylphenol, and the catalyst is one or more of p-toluenesulfonic acid, methanesulfonic acid, and solid superacid. When the inhibitor is preferably a mixture, the present invention has no special limitation on the mass ratio of each substance in the mixture, and a mixture of any mass ratio can be used.

[0027] The preparation method of polycarbonate acrylate is as follows:

[0028] (a) POLYPCE, polymerization inhibitor, catalyst and cyclohexane are mixed and added into a three-necked flask equipped with a water separator, a thermometer, a stirrer and a reflux condenser, and then an appropriate amount of acrylic acid is added to carry out esterification reaction at 100°C to 120°C for 9 to 16 hours.

[0029] (b) The obtained esterification reaction product is subjected to alkali washing and water washing, and the organic phase is taken and rotary evaporated in a vacuum rotary evaporator until a constant weight is reached, and then the residual solvent is removed by an oil pump for 2 hours to obtain polycarbonate acrylate.

[0030] Among them, the usage ratio of POLYPCE to cyclohexane solvent is preferably 50g-100g:100-200ml; the molar ratio of POLYPCE to inhibitor is preferably 1:0.03-0.06; and the molar ratio of POLYPCE to catalyst is preferably 1:0.05-0.1.

[0031] It is worth noting that the temperature of the rotary evaporation in the preparation method of polycarbonate acrylate is not particularly limited, as long as it can remove cyclohexane in the esterification reactants.

[0032] The epoxy resin oligomer is selected from one or a mixture of bisphenol A epoxy resin (DYD-128), 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate (2021P), hydrogenated bisphenol A epoxy resin (HE-2025), 3-ethyl-3-oxetanol (MOX-101). When the epoxy resin oligomer is preferably a mixture, the present invention has no particular limitation on the mass ratio of each substance in the mixture, and a mixture of any mass ratio can be used.

[0033] The acrylate oligomer also includes one or a mixture of epoxy acrylate (CN104NS), trimethylolpropane triacrylate (SR351NS), ethoxylated trimethylolpropane triacrylate (SR499NS), propoxylated neopentyl glycol diacrylate (SR9003NS). When the acrylate oligomer is preferably a mixture, the present invention has no particular limitation on the mass ratio of the various substances in the mixture, and a mixture of any mass ratio can be used.

[0034] The photoinitiator is a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate (1176) and / or hydroxycyclohexylphenyl ketone (184).

[0035] The modified additive is a core-shell toughened modified resin (EPX-125).

[0036] The auxiliary agent is one or a mixture of carboxyl-terminated liquid nitrile rubber (CTBN), hydroxyl-terminated liquid nitrile rubber (HTBN), and polyether polyol (LEP4801). When the auxiliary agent is preferably a mixture, the present invention has no particular limitation on the mass ratio of the various substances in the mixture, and a mixture of any mass ratio can be used.

[0037] The present invention discloses a method for preparing a SLA tough photosensitive resin for 3D printing. The SLA tough photosensitive resin of the present invention is applied and implemented in accordance with the following steps: (1) fully mixing an epoxy resin oligomer, an acrylate oligomer, a photoinitiator, a modifying additive, and an auxiliary agent according to a certain weight percentage; and (2) fully stirring at room temperature for 60 to 120 minutes to obtain the SLA tough photosensitive resin for 3D printing.

[0038] Next, several embodiments of the method for preparing the SLA tough photosensitive resin for 3D printing according to the present invention will be given.

[0039] Example 1

[0040] First, prepare polycarbonate acrylate: weigh 110g of POLYPCE1885, 17g of acrylic acid, 0.4g of p-hydroxyanisole and 1.1g of p-toluenesulfonic acid monohydrate, add them into a three-necked flask equipped with a water separator, a thermometer, a stirrer and a reflux condenser, and carry out esterification reaction at 120°C for 14h, wash the obtained esterification reactant with alkali and water, take the organic phase, and rotary evaporate it in a vacuum rotary evaporator until a constant weight is reached, and then use an oil pump for 2h to remove the residual solvent.

[0041] Preparation of SLA tough photosensitive resin for 3D printing: weigh 5 g of the above-prepared polycarbonate acrylate, 30 g of SR499NS (ethoxylated trimethylolpropane triacrylate), 20 g of DYD-128 (bisphenol A epoxy resin), 10 g of 2021P (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), 10 g of HE-2025 (hydrogenated bisphenol A epoxy resin), 10 g of MOX-101 (3-ethyl-3-oxetanecarbinol) and 10 g of 100 μg of 1 ... g, LEP4801 (polyether polyol) 3g, EPX-125 (core-shell toughened modified resin) 5g, 1176 (a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate) 4g, 184 (hydroxycyclohexyl phenyl ketone) 3g, mix them thoroughly, and stir at room temperature for 60-120 minutes until the photoinitiator and the additive are completely dissolved to obtain the SLA tough photosensitive resin for 3D printing.

[0042] Example 2

[0043] First, prepare polycarbonate acrylate: weigh 120g of POLYPCE1726, 20g of acrylic acid, 0.5g of p-hydroxyanisole and 1.4g of p-toluenesulfonic acid monohydrate, add them into a three-necked flask equipped with a water separator, a thermometer, a stirrer and a reflux condenser, and carry out esterification reaction at 120°C for 14h, wash the obtained esterification reactant with alkali and water, take the organic phase, and rotary evaporate it in a vacuum rotary evaporator until a constant weight is reached, and then use an oil pump for 2h to remove the residual solvent.

[0044] Preparation of SLA tough photosensitive resin for 3D printing: weigh 15 g of the above-prepared polycarbonate acrylate, 20 g of SR499NS (ethoxylated trimethylolpropane triacrylate), 20 g of DYD-128 (bisphenol A epoxy resin), 10 g of 2021P (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), 10 g of HE-2025 (hydrogenated bisphenol A epoxy resin), 10 g of MOX-101 (3-ethyl-3-oxetanecarbinol) g, LEP4801 (polyether polyol) 3g, EPX-125 (core-shell toughened modified resin) 5g, 1176 (a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate) 4g, 184 (hydroxycyclohexyl phenyl ketone) 3g, mix them thoroughly, and stir at room temperature for 60-120 minutes until the photoinitiator and the additive are completely dissolved to obtain the SLA tough photosensitive resin for 3D printing.

[0045] Example 3

[0046] First, prepare polycarbonate acrylate: weigh 140g of POLYPCE1885, 22g of acrylic acid, 0.6g of p-hydroxyanisole and 1.5g of p-toluenesulfonic acid monohydrate, add them into a three-necked flask equipped with a water separator, a thermometer, a stirrer and a reflux condenser, and carry out esterification reaction at 120°C for 9h, wash the obtained esterification reactant with alkali and water, take the organic phase, and rotary evaporate it in a vacuum rotary evaporator until a constant weight is reached, and then use an oil pump for 2h to remove the residual solvent.

[0047] Preparation of SLA tough photosensitive resin for 3D printing: weigh 20g of the above-prepared polycarbonate acrylate, 15g of SR499NS (ethoxylated trimethylolpropane triacrylate), 20g of DYD-128 (bisphenol A epoxy resin), 10g of 2021P (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), 10g of HE-2025 (hydrogenated bisphenol A epoxy resin), 10g of MOX-101 (3-ethyl-3-oxetanecarbinol) and 10g of 100% bisphenol A epoxy resin. g, LEP4801 (polyether polyol) 3g, EPX-125 (core-shell toughened modified resin) 5g, 1176 (a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate) 4g, 184 (hydroxycyclohexyl phenyl ketone) 3g, mix them thoroughly, and stir at room temperature for 60-120 minutes until the photoinitiator and the additive are completely dissolved to obtain the SLA tough photosensitive resin for 3D printing.

[0048] Example 4

[0049] First, prepare polycarbonate acrylate: weigh 150g of POLYPCE1726, 14g of acrylic acid, 0.7g of p-hydroxyanisole and 1.7g of p-toluenesulfonic acid monohydrate, add them into a three-necked flask equipped with a water separator, a thermometer, a stirrer and a reflux condenser, and carry out esterification reaction at 120°C for 9h, wash the obtained esterification reactant with alkali and water, take the organic phase, and rotary evaporate it in a vacuum rotary evaporator until a constant weight is reached, and then use an oil pump for 2h to remove the residual solvent.

[0050] Preparation of SLA tough photosensitive resin for 3D printing: weigh 25 g of the above-prepared polycarbonate acrylate, 10 g of SR499NS (ethoxylated trimethylolpropane triacrylate), 20 g of DYD-128 (bisphenol A epoxy resin), 10 g of 2021P (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), 10 g of HE-2025 (hydrogenated bisphenol A epoxy resin), 10 g of MOX-101 (3-ethyl-3-oxetanecarbinol) g, LEP4801 (polyether polyol) 3g, EPX-125 (core-shell toughened modified resin) 5g, 1176 (a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate) 4g, 184 (hydroxycyclohexyl phenyl ketone) 3g, mix them thoroughly, and stir at room temperature for 60-120 minutes until the photoinitiator and the additive are completely dissolved to obtain the SLA tough photosensitive resin for 3D printing.

[0051] Example 5

[0052] First, prepare polycarbonate acrylate: weigh 140g of POLYPCE1885, 32g of acrylic acid, 0.6g of p-hydroxyanisole and 1.4g of p-toluenesulfonic acid monohydrate, add them into a three-necked flask equipped with a water separator, a thermometer, a stirrer and a reflux condenser, and carry out esterification reaction at 120°C for 9h, wash the obtained esterification reactant with alkali and water, take the organic phase, and rotary evaporate it in a vacuum rotary evaporator until a constant weight is reached, and then use an oil pump for 2h to remove the residual solvent.

[0053] Preparation of SLA tough photosensitive resin for 3D printing: weigh 15g of the above-prepared polycarbonate acrylate, 5g of SR9003NS (propoxylated neopentyl glycol diacrylate), 5g of SR499NS (ethoxylated trimethylolpropane triacrylate), 30g of DYD-128 (bisphenol A epoxy resin), 10g of 2021P (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), 10g of HE-2025 (hydrogenated bisphenol A epoxy resin), 10g of MOX-101 (3-ethyl -3-Oxetanecarbinol) 10g, LEP4801 (polyether polyol) 3g, EPX-125 (core-shell toughened modified resin) 5g, 1176 (a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate) 4g, 184 (hydroxycyclohexyl phenyl ketone) 3g, mix them thoroughly, and stir at room temperature for 60-120 minutes until the photoinitiator and the additive are completely dissolved to obtain the SLA tough photosensitive resin for 3D printing.

[0054] Example 6

[0055] First, prepare polycarbonate acrylate: weigh 150g of POLYPCE1726, 25g of acrylic acid, 0.6g of p-hydroxyanisole and 1.7g of p-toluenesulfonic acid monohydrate, add them into a three-necked flask equipped with a water separator, a thermometer, a stirrer and a reflux condenser, and carry out esterification reaction at 120°C for 9h, wash the obtained esterification reactant with alkali and water, take the organic phase, and rotary evaporate it in a vacuum rotary evaporator until a constant weight is reached, and then use an oil pump for 2h to remove the residual solvent.

[0056] Preparation of SLA tough photosensitive resin for 3D printing: weigh 15g of the above-prepared polycarbonate acrylate, 5g of SR9003NS (propoxylated neopentyl glycol diacrylate), 30g of SR499NS (ethoxylated trimethylolpropane triacrylate), 15g of DYD-128 (bisphenol A epoxy resin), 5g of 2021P (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), 10g of HE-2025 (hydrogenated bisphenol A epoxy resin), and 10g of MOX-101 (3-ethyl -3-Oxetanecarbinol) 10g, LEP4801 (polyether polyol) 3g, EPX-125 (core-shell toughened modified resin) 5g, 1176 (a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate) 4g, 184 (hydroxycyclohexyl phenyl ketone) 3g, mix them thoroughly, and stir at room temperature for 60-120 minutes until the photoinitiator and the additive are completely dissolved to obtain the SLA tough photosensitive resin for 3D printing.

[0057] The mass percentages of the components in the above examples 1-6 are shown in Table 1 below:

[0058] Table 1

[0059]

[0060]

[0061] The samples prepared in the above six embodiments were subjected to performance tests including but not limited to the following: tensile strength (ASTMD638 standard), tensile modulus (ASTMD638 standard), flexural strength (ASTMD790 standard), flexural modulus (ASTMD790 standard), water absorption (ASTM D570-98 standard), hardness (ASTMD2240 standard), elongation at break (ASTMD638 standard), notched impact strength (ASTMD256 standard), heat deformation temperature (ASTMD648@66PS standard), glass transition temperature (DMA), etc. The corresponding test results are shown in Table 2:

[0062] Table 2

[0063]

[0064]

[0065] It can be seen from Table 2 that the photosensitive resins in Examples 1 to 6 all exhibit high heat resistance and hardness after curing. In particular, the product of Example 2 has more excellent mechanical properties, the best balance between hardness and toughness, and excellent impact strength.

[0066] It is worth noting that when the proportion of POLY PCE-DA in the acrylate oligomer increases, although the hardness of the final product is appropriately reduced, the impact strength and toughness will be improved.

[0067] Compared with the common tough photosensitive resins on the market, the present invention adds POLY PCE-DA. Although the hardness is slightly reduced, the toughness is effectively improved. In addition, the photosensitive resin has small shrinkage after curing, low water absorption and high strength. It can be used in the production of master molds, concept models, general components and functional components in industrial fields such as automobiles, medical treatment and consumer electronics.

[0068] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A SLA tough photosensitive resin for 3D printing, characterized in that: The SLA tough photosensitive resin comprises the following raw materials in parts by weight: 50% epoxy resin oligomer, 35% acrylate oligomer, 7% photoinitiator, 5% modification additive, 3% auxiliary agent, the sum of the mass percentages of the above components is 100%, and the acrylate oligomer comprises polycarbonate acrylate; The polycarbonate acrylate is obtained by esterification reaction of polycarbonate polyether polyol and acrylic acid, and the molar ratio of the polycarbonate polyether polyol to acrylic acid is 1:2-6.

2. The SLA tough photosensitive resin for 3D printing according to claim 1, characterized in that: In the esterification reaction of the polycarbonate polyether polyol and acrylic acid, a polymerization inhibitor and a catalyst are also added.

3. The SLA tough photosensitive resin for 3D printing according to claim 1, characterized in that: The epoxy resin oligomer is one of bisphenol A epoxy resin, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, hydrogenated bisphenol A epoxy resin, 3-ethyl-3-oxetanol, or a mixture of several thereof.

4. The SLA tough photosensitive resin for 3D printing according to claim 1, characterized in that: The acrylate oligomer also includes one or a mixture of epoxy acrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated neopentyl glycol diacrylate.

5. The SLA tough photosensitive resin for 3D printing according to claim 1, characterized in that: The photoinitiator is a mixture of diphenyl-(4-phenylthio)phenylsulfonium hexafluoroantimonate and diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate and / or hydroxycyclohexyl phenyl ketone.

6. The SLA tough photosensitive resin for 3D printing according to claim 1, characterized in that: The modified additive is a core-shell toughened modified resin.

7. The SLA tough photosensitive resin for 3D printing according to claim 1, characterized in that: The auxiliary agent is one or a mixture of carboxyl-terminated liquid nitrile rubber, hydroxyl-terminated liquid nitrile rubber, and polyether polyol.

8. The method for preparing the SLA tough photosensitive resin for 3D printing according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: (1) fully mixing epoxy resin oligomer, acrylate oligomer, photoinitiator, modification additive and auxiliary agent according to a certain weight percentage; and (2) fully stirring at room temperature for 60 to 120 minutes to obtain SLA tough photosensitive resin for 3D printing.