Polarizing plate and image display device using the same

By using a polyvinyl alcohol-based resin layer in the polarizing plate to adsorb iodine and combine it with a urea compound layer, adjusting the moisture content, and using a transparent protective film and adhesive layer in the image display device, the transmission rate of the polarizing plate under high temperature environment is solved. The problem of reduction achieves high-temperature durability and polarization stability.

CN114746780BActive Publication Date: 2024-11-15SUMITOMO CHEM CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202080078958.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-15
Filing Date
2020-10-29
Publication Date
2024-11-15
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

In a high temperature environment, when the polarizing plate is used in the interlayer filling structure of the image display device, the transmittance is easily reduced, resulting in a decrease in the visibility of the picture, and it is difficult for the prior art to effectively suppress this problem.

Method used

Polarizing elements that absorb iodine and oriented iodine by using a polyvinyl alcohol-based resin layer, combine the urea-based compound layer to adjust the moisture content of the polarizing plate between 30% and 50% relative humidity of 20°C, and use transparency in the image display device. The protective film and adhesive layer are formed to ensure the high-temperature durability of the polarizing plate.

Benefits of technology

The transmittance of the polarizing plate under high temperature environment is effectively suppressed, the high-temperature durability and polarization stability of the image display device are improved, and the orthogonal light leakage is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003641097680000201
    Figure BDA0003641097680000201
  • Figure BDA0003641097680000231
    Figure BDA0003641097680000231
  • Figure BDA0003641097680000232
    Figure BDA0003641097680000232
Patent Text Reader

Abstract

The object of the present invention is to provide a polarizing plate which can suppress the decrease of transmittance in a high temperature environment even when used in an image display device composed of an interlayer filling structure. The present invention provides a polarizing plate, which has a polarizing element formed by adsorbing iodine on a polyvinyl alcohol resin layer and orienting the iodine, and a transparent protective film, the polarizing plate having a urea compound-containing layer containing at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives, and the moisture content of the polarizing element is greater than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, and is less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing plate and an image display device in which one surface of the polarizing plate is bonded to an image display unit and the other surface is bonded to a transparent member such as a touch panel or a front panel. Background Art

[0002] Liquid crystal display devices (LCDs) are not only used for liquid crystal televisions, but are also widely used in personal computers, mobile devices such as mobile phones, and in-vehicle applications such as navigation systems. Typically, a liquid crystal display device has a liquid crystal panel component with polarizing plates bonded to both sides of a liquid crystal unit using an adhesive, and displays by controlling the light from a backlight component using the liquid crystal panel component. In addition, in recent years, organic EL display devices have also been widely used in televisions, mobile devices such as mobile phones, and in-vehicle applications such as navigation systems, similar to liquid crystal display devices. In an organic EL display device, in order to suppress the situation where external light is reflected by a metal electrode (cathode) and observed as a mirror surface, a circular polarizing plate (a laminate comprising a polarizing element and a λ / 4 plate) is sometimes arranged on the visible side surface of the image display panel.

[0003] As mentioned above, polarizing plates are increasingly being installed in vehicles as components of liquid crystal display devices and organic EL display devices. Polarizing plates used in vehicle-mounted image display devices are more often exposed to high-temperature environments than other mobile devices such as televisions and mobile phones, and are required to have less change in characteristics under high temperatures (high-temperature durability).

[0004] On the other hand, for the purpose of preventing damage to the image display panel caused by impact from the external surface, there are more and more structures in which a front panel such as a transparent resin plate or a glass plate is further provided on the visible side relative to the polarizing plate of the image display panel (also referred to as a "window layer", etc.). In addition, in display devices having a touch panel, the following structure is widely adopted, that is, a touch panel is further provided on the visible side relative to the polarizing plate of the image display panel, and a front panel is further provided on the visible side relative to the touch panel.

[0005] In this structure, if there is an air layer between the image display panel and transparent components such as the front panel and the touch panel, reflection glare of external light caused by reflection of light at the interface of the air layer will be generated, and the visibility of the picture tends to decrease. Therefore, the following structure is being promoted, that is, the space between the polarizing plate arranged on the visible side surface of the image display panel and the transparent component is filled with a layer other than the air layer (hereinafter sometimes referred to as "interlayer filler") (hereinafter sometimes referred to as "interlayer filling structure"), preferably a structure filled with a material having a refractive index close to these materials. As an interlayer filler, an adhesive or a UV curing adhesive is used for the purpose of suppressing the reduction of visibility caused by reflection at the interface and bonding and fixing the components together (for example, refer to Patent Document 1).

[0006] The above-mentioned interlayer filling structure is being widely used in mobile devices such as mobile phones that are often used outdoors. In addition, due to the increase in visibility requirements in recent years, in vehicle-mounted applications such as car navigation devices, research is also being conducted on the use of an interlayer filling structure in which a front panel is arranged on the surface of an image display panel and the space between the panels is filled with an adhesive layer or the like.

[0007] However, it has been reported that when such a structure is adopted, the result of the heating durability test (200 hours at 95°C, etc.) is that a significant decrease in transmittance can be observed in the central part of the polarizing plate surface. On the other hand, if it is a single polarizing plate, even if it is placed at 95°C for 1000 hours, no significant decrease in transmittance is observed. Based on these results, it has also been reported that a significant decrease in the transmittance of the polarizing plate in a high temperature environment is a problem unique to the case where an image display device using an interlayer filling structure is exposed to a high temperature environment. The interlayer filling structure is a structure in which one side of the polarizing plate is bonded to the image display unit and the other side is bonded to a transparent member such as a touch panel or a front panel (Patent Document 2).

[0008] In addition, in the above-mentioned Patent Document 2, the polarizing plate whose transmittance is significantly reduced in the interlayer filling structure has a Raman spectroscopic measurement at 1100 cm -1 Nearby (from =CC= key) and 1500cm -1 There is a peak near (derived from the -C=C- bond), so it is considered that a polyene structure (-C=C) is formed. n -, which is presumably caused by polyenylation of the polyvinyl alcohol constituting the polarizing element due to dehydration (Patent Document 2, paragraph

[0012] ).

[0009] As a solution to this problem, Patent Document 2 proposes a method of suppressing a decrease in transmittance by setting the moisture content per unit area of ​​the polarizing plate to a predetermined amount or less and setting the saturated water absorption of a transparent protective film adjacent to the polarizing element to a predetermined amount or less.

[0010] However, even with such a method, the effect of suppressing the decrease in transmittance in the high-temperature durability test is not sufficient.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 11-174417

[0014] Patent Document 2: Japanese Patent Application Publication No. 2014-102353 Summary of the invention

[0015] Problems to be solved by the invention

[0016] The present invention provides the following polarizing plate, image display device, and method for producing the polarizing plate.

[0017] [1] A polarizing plate comprising a polarizing element in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin layer, and a transparent protective film.

[0018] The polarizing plate comprises a urea compound-containing layer including at least one urea compound selected from urea, urea derivatives, thiourea, and thiourea derivatives.

[0019] The moisture content of the polarizing element is equal to or higher than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and equal to or lower than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0020] [2] A polarizing plate comprising a polarizing element in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin layer, and a transparent protective film.

[0021] The polarizing plate comprises a urea compound-containing layer including at least one urea compound selected from urea, urea derivatives, thiourea, and thiourea derivatives.

[0022] The moisture content of the polarizing plate is equal to or higher than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and equal to or lower than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0023] [3] The polarizing plate according to [1] or [2], wherein the layer containing a urea compound contains at least one urea compound selected from urea derivatives and thiourea derivatives.

[0024] [4] The polarizing plate according to any one of [1] to [3], wherein the layer containing the urea compound is in contact with the polarizing element.

[0025] [5] The polarizing plate according to any one of [1] to [4], wherein the layer containing the urea compound is an adhesive layer.

[0026] [6] The polarizing plate according to [5], wherein the layer containing a urea compound comprises a polyvinyl alcohol resin.

[0027] [7] The polarizing plate according to [6], wherein in the layer containing a urea compound, a total content of the urea compound is 0.1 parts by mass or more and 400 parts by mass or less based on 100 parts by mass of the polyvinyl alcohol resin.

[0028] [8] The polarizing plate according to any one of [5] to [7], wherein the thickness of the layer containing the urea compound is 0.01 to 7 μm.

[0029] [9] A polarizing plate comprising a polarizing element in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin layer, and a transparent protective film.

[0030] The polarizing element comprises at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives,

[0031] The moisture content of the polarizing element is equal to or higher than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and equal to or lower than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0032]

[10] A polarizing plate comprising a polarizing element in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin layer, and a transparent protective film.

[0033] The polarizing element comprises at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives,

[0034] The moisture content of the polarizing plate is equal to or higher than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and equal to or lower than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0035]

[11] The polarizing plate according to any one of [1] to

[10] , wherein the polarizing plate is used in an image display device.

[0036] In the image display device, layers other than the air layer are provided in contact with both surfaces of the polarizing plate.

[0037]

[12] An image display device comprising an image display unit, a first adhesive layer laminated on a visible side surface of the image display unit, and a polarizing plate according to any one of [1] to

[11] laminated on a visible side surface of the first adhesive layer.

[0038]

[13] The image display device according to

[12] , further comprising a second pressure-sensitive adhesive layer laminated on the visible side surface of the polarizing plate, and a transparent member laminated on the visible side surface of the second pressure-sensitive adhesive layer.

[0039]

[14] The image display device according to

[13] , wherein the transparent member is a glass plate or a transparent resin plate.

[0040]

[15] The image display device according to

[13] , wherein the transparent component is a touch panel.

[0041]

[16] A method for producing a polarizing plate, which is the method for producing a polarizing plate according to [1] or [9],

[0042] The manufacturing method includes a moisture content adjustment step of adjusting the moisture content of the polarizing element to be greater than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30% and less than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0043]

[17] A method for producing a polarizing plate, which is the method for producing a polarizing plate according to [2] or

[10] ,

[0044] The manufacturing method includes a moisture content adjustment step of adjusting the moisture content of the polarizing plate to be greater than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30% and less than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0045] Effects of the Invention

[0046] According to the present invention, a polarizing plate can be provided, which has little reduction in transmittance in a high-temperature environment and excellent high-temperature durability even when used in an image display device composed of interlayer filling. In addition, an image display device is provided, which suppresses the reduction in transmittance in a high-temperature environment by using the polarizing plate of the present invention. DETAILED DESCRIPTION

[0047] 《First Implementation Method》

[0048] The polarizing plate of the first embodiment of the present invention comprises a polarizing element formed by adsorbing iodine on a polyvinyl alcohol resin layer and orienting the iodine, a urea compound layer comprising at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives, and a transparent protective film. The polarizing plate of this embodiment has at least one of the following (a) and (b) features.

[0049] (a) The moisture content of the polarizing element is not less than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and not more than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0050] (b) The moisture content of the polarizing plate is equal to or higher than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, and equal to or lower than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%.

[0051] By making the polarizing plate of the present embodiment have at least one of the above (a) and (b) characteristics and have a layer containing a urea compound, even when the component of the image display device formed by interlayer filling is exposed to a high-temperature environment for a long time, a decrease in monomer transmittance can be suppressed. By making the polarizing plate of the present embodiment have a layer containing a urea compound, even when the polarizing plate is exposed to a high-temperature environment, a decrease in polarization degree can be suppressed. When two polarizing plates are arranged and used in a relationship forming an orthogonal Nicol prism, if the polarization degree of the polarizing plate decreases, light leakage (hereinafter also referred to as "orthogonal light leakage (Japanese: ク口ス拔け)") is likely to occur. However, according to the present invention, even when exposed to a high-temperature environment, the polarization degree is not easily reduced, so orthogonal light leakage is also easily suppressed.

[0052] [Polarizing element]

[0053] As the polarizing element of the present invention in which a polyvinyl alcohol (hereinafter also referred to as PVA) - based resin layer adsorbs iodine and the iodine is oriented, a known polarizing element can be used. As such a polarizing element, it is generally formed by using a PVA - based resin film, dyeing the PVA - based resin film with iodine, and performing uniaxial stretching.

[0054] As described above, the PVA - based resin generally uses a resin obtained by saponifying a polyvinyl acetate - based resin. The saponification degree is about 85 mol% or more, preferably about 90 mol% or more, and more preferably about 99 mol% - 100 mol%. As the polyvinyl acetate - based resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers capable of copolymerizing with it can be cited, for example, ethylene - vinyl acetate copolymer, etc. As other monomers capable of copolymerizing, for example, unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, etc. can be cited. The degree of polymerization of the PVA - based resin is 1000 - 10000, preferably 1500 - 5000. The PVA - based resin can be modified, for example, it can be polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc. modified by aldehydes.

[0055] The method for manufacturing the polarizing element is not particularly limited. A typical method is a method of producing a polyvinyl alcohol-based resin film that is pre-wound into a roll and then stretched, dyed, cross-linked, etc.; a method comprising a process of preparing a laminate of a polyvinyl alcohol-based resin and a stretching resin substrate and stretching the laminate. In the present invention, any of these methods can be used. The methods for manufacturing these polarizing elements are described in paragraphs

[0109] to

[0128] of Japanese Patent Publication No. 2014-48497, and these methods can be used in this embodiment. In addition, the thickness of the polarizing element of this embodiment is preferably 3 to 35 μm, more preferably 4 to 30 μm, and further preferably 5 to 25 μm.

[0056] (Feature (a))

[0057] In the case of feature (a), the moisture content of the polarizing element is greater than the equilibrium moisture content at a temperature of 20°C and relative humidity of 30%, and is less than the equilibrium moisture content at a temperature of 20°C and relative humidity of 50%. More preferably, it is less than the equilibrium moisture content at a temperature of 20°C and relative humidity of 45%, further preferably less than the equilibrium moisture content at a temperature of 20°C and relative humidity of 42%, and most preferably less than the equilibrium moisture content at a temperature of 20°C and relative humidity of 38%. If it is less than the equilibrium moisture content at a temperature of 20°C and relative humidity of 30%, the operability of the polarizing element is reduced and it is easy to break. If the moisture content of the polarizing element is greater than the equilibrium moisture content at a temperature of 20°C and relative humidity of 50%, the transmittance of the polarizing element is easy to reduce. It is speculated that if the moisture content of the polarizer is high, the polyeneization of the PVA-based resin is easy to advance. The above moisture content of the polarizing element is the moisture content of the polarizing element in the polarizing plate.

[0058] As a method for confirming whether the moisture content of the polarizing element is above the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, and below the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%, the following method can be exemplified. When the polarizing element is stored in an environment adjusted to the above-mentioned temperature and relative humidity ranges and there is no change in mass for a certain period of time, it is considered to be in equilibrium with the environment. Alternatively, the equilibrium moisture content of the polarizing element in an environment adjusted to the above-mentioned temperature and relative humidity ranges is calculated in advance, and the moisture content of the polarizing element is compared with the pre-calculated equilibrium moisture content for confirmation.

[0059] There is no particular limitation on the method for manufacturing a polarizing element having a moisture content that is higher than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30% and lower than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%. For example, there can be a method of storing the polarizing element in an environment adjusted to the above temperature and relative humidity range for 10 minutes to 3 hours, or a method of heat-treating the polarizing element at a temperature of 30°C to 90°C.

[0060] As other preferred methods for manufacturing polarizing elements with the above-mentioned moisture content, there can be cited a method of storing a laminate having a protective film laminated on at least one side of the polarizing element or a polarizing plate formed using the polarizing element in an environment adjusted to the above-mentioned temperature and relative humidity range for more than 10 minutes and less than 120 hours; or a method of performing a heat treatment at a temperature of more than 30°C and less than 90°C. When manufacturing an image display device using an interlayer filling structure, an image display panel having a polarizing plate laminated on an image display unit can be stored in an environment adjusted to the above-mentioned temperature and relative humidity range for more than 10 minutes and less than 3 hours, or heated at a temperature of more than 30°C and less than 90°C, and then the front panel can be attached.

[0061] Regarding the moisture content of the polarizing element, it is preferred to adjust the moisture content to the above-mentioned numerical range in a single polarizing element or in a laminate of a polarizing element and a protective film, and at the material stage used to form a polarizing plate. In the case where the moisture content is adjusted after the polarizing plate is formed, the curl becomes too large, and it is easy to cause a bad condition when it is bonded to the image display unit. By forming a polarizing plate using a polarizing element whose moisture content is adjusted to the above-mentioned moisture content at the material stage before forming the polarizing plate, a polarizing plate having a polarizing element whose moisture content satisfies the above-mentioned numerical range can be easily formed. It is also possible to adjust the moisture content of the polarizing element in the polarizing plate to the above-mentioned numerical range when the polarizing plate is bonded to the image display unit. In this case, since the polarizing plate is bonded to the image display unit, curling is not easy to occur.

[0062] (Feature (b))

[0063] In the case of feature (b), the moisture content of the polarizing plate is greater than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, and is less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%. The moisture content of the polarizing plate is preferably less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 45%, more preferably less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 42%, and further preferably less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 38%. If the moisture content of the polarizing plate is less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, the operability of the polarizing plate is reduced and it is easy to break. If the moisture content of the polarizing plate is greater than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%, the transmittance of the polarizing element is easily reduced. It is speculated that if the moisture content of the polarizing plate is high, the polyeneization of the PVA-based resin is easily promoted.

[0064] As a method for confirming whether the moisture content of the polarizing plate is above the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, and below the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%, the following method can be exemplified. When the polarizing plate is stored in an environment adjusted to the above temperature and relative humidity ranges, and there is no change in mass for a certain period of time, it is considered to be in equilibrium with the environment. Alternatively, the equilibrium moisture content of the polarizing plate in an environment adjusted to the above temperature and relative humidity ranges is calculated in advance, and the moisture content of the polarizing plate is compared with the pre-calculated equilibrium moisture content to confirm.

[0065] There is no particular limitation on the method for manufacturing a polarizing plate having a moisture content that is higher than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30% and lower than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%. For example, there can be a method of storing the polarizing plate in an environment adjusted to the above temperature and relative humidity range for 10 minutes to 3 hours, or a method of performing a heat treatment at a temperature of 30°C to 90°C.

[0066] When making an image display device using an interlayer filling structure, a polarizing plate can be stacked on an image display unit, and the resulting image display panel can be stored in an environment adjusted to the above-mentioned temperature and relative humidity range for more than 10 minutes and less than 3 hours, or heated at more than 30°C and less than 90°C, and then bonded to a front panel.

[0067] [Layer containing urea compound]

[0068] The polarizing plate of the present invention has a layer containing a urea compound, which contains at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives. The layer containing a urea compound is not limited as long as it is a layer containing a urea compound, but for example, an adhesive layer and a curing layer can be cited. The layer containing a urea compound may or may not be in contact with a polarizing element, but preferably in contact with a polarizing element from the viewpoint of being able to further suppress the decrease in transmittance under a high temperature environment.

[0069] In the present invention, from the viewpoint of productivity, it is preferred that the adhesive layer is a layer containing a urea compound. The adhesive layer is formed by the following adhesive. As an adhesive layer belonging to the layer containing a urea compound, an adhesive layer for bonding a polarizing element to a protective film can be exemplified. It should be noted that the configuration of the case where the layer containing a urea compound is other than the adhesive layer will be described later.

[0070] <Adhesive Layer>

[0071] Any appropriate adhesive can be used as the adhesive forming the adhesive layer for bonding the protective film to the polarizing element. Specifically, water-based adhesives, solvent-based adhesives, active energy ray-curable adhesives, etc. can be used as the adhesive, but water-based adhesives are preferred.

[0072] When the adhesive layer is a layer containing a urea compound, the adhesive contains at least one urea compound selected from the group consisting of urea, urea derivatives, thiourea, and thiourea derivatives.

[0073] The thickness of the adhesive during coating can be set to any appropriate value. For example, it can be set in such a way that an adhesive layer having a desired thickness is obtained after curing or heating (drying). The thickness of the adhesive layer is preferably 0.01 μm to 7 μm, more preferably 0.01 μm to 5 μm, further preferably 0.01 μm to 2 μm, and most preferably 0.01 μm to 1 μm.

[0074] (Water-based adhesive)

[0075] In addition, as the above-mentioned water-based adhesive, any appropriate water-based adhesive can be used. Among them, it is preferred to use a water-based adhesive containing a PVA-based resin (PVA-based adhesive). From the aspect of adhesiveness, the average polymerization degree of the PVA-based resin contained in the water-based adhesive is preferably about 100 to 5500, and more preferably 1000 to 4500. From the aspect of adhesiveness, the average saponification degree is preferably about 85 mol% to 100 mol%, and more preferably 90 mol% to 100 mol%.

[0076] As the PVA resin contained in the above-mentioned water-based adhesive, a PVA resin containing acetoacetyl groups is preferred, because the PVA resin layer has excellent adhesion to the protective film and excellent durability. The PVA resin containing acetoacetyl groups can be obtained, for example, by reacting the PVA resin with diketene using an optional method. The acetoacetyl modification degree of the PVA resin containing acetoacetyl groups is typically 0.1 mol% or more, preferably about 0.1 mol% to 20 mol%.

[0077] The resin concentration of the water-based adhesive is preferably 0.1% by weight to 15% by weight, and more preferably 0.5% by weight to 10% by weight.

[0078] (crosslinking agent, solvent)

[0079] The water-soluble PVA-based adhesive that can be preferably used in the present invention can also contain a crosslinking agent as needed in addition to the above-mentioned PVA-based resin and urea-based compound. A known crosslinking agent can be used as the crosslinking agent. For example, water-soluble epoxy compounds, dialdehydes, isocyanates, etc. can be cited.

[0080] When the PVA-based resin is an acetoacetyl group-containing PVA-based resin, the crosslinking agent is preferably any of glyoxal, glyoxylate, and methylolmelamine, more preferably any of glyoxal and glyoxylate, and particularly preferably glyoxal.

[0081] The water-soluble PVA-based adhesive of the present invention may contain an organic solvent. In this case, alcohols are preferred from the viewpoint of miscibility with water, and methanol or ethanol is more preferred among alcohols.

[0082] In the present invention, some urea derivatives have low solubility in water, but sufficient solubility in alcohol. In this case, after dissolving in alcohol to prepare an alcohol solution of the urea derivative, the alcohol solution of the urea derivative is added to the PVA aqueous solution to prepare the adhesive, which is also one of the preferred methods.

[0083] (Active energy ray-curable adhesive)

[0084] As the above-mentioned active energy ray-curable adhesive, any appropriate adhesive can be used as long as it is an adhesive that can be cured by irradiation with active energy rays. As active energy ray-curable adhesives, for example, ultraviolet curable adhesives, electron beam curable adhesives, etc. can be cited. As specific examples of the curing type of active energy ray-curable adhesives, free radical curing types, cation curing types, anion curing types, and combinations thereof (for example, blends of free radical curing types and cation curing types) can be cited.

[0085] As the above-mentioned active energy ray-curable adhesive, for example, an adhesive containing a compound (such as a monomer and / or an oligomer) having a free radical polymerizable group such as a (meth)acrylate group or a (meth)acrylamide group as a curing component can be cited. Specific examples of the above-mentioned active energy ray-curable adhesive and a curing method thereof are described in Japanese Patent Application Publication No. 2012-144690.

[0086] (Urea compounds)

[0087] When the adhesive layer is a layer containing a urea compound, the adhesive layer contains at least one urea compound selected from the group consisting of urea, urea derivatives, thiourea, and thiourea derivatives.

[0088] As a method for making the adhesive layer contain a urea compound, it is preferable to make the above-mentioned adhesive contain a urea compound. It should be noted that during the process of forming the adhesive layer from the adhesive through a drying step, a part of the urea compound may move from the adhesive layer to the polarizing element, etc.

[0089] Urea compounds include water-soluble urea compounds and sparingly water-soluble urea compounds, and any urea compound may be used in the present invention. When sparingly water-soluble urea compounds are used in a water-soluble adhesive, it is preferred to design a dispersion method so that turbidity does not increase after forming an adhesive layer.

[0090] When the adhesive is a water-based adhesive containing a PVA resin, the amount of the urea compound added is preferably 0.1 to 400 parts by mass, more preferably 1 to 200 parts by mass, and even more preferably 3 to 100 parts by mass, relative to 100 parts by mass of PVA.

[0091] (Urea derivatives)

[0092] The urea derivative is a compound in which at least one of the four hydrogen atoms in the urea molecule is substituted with a substituent. In this case, the substituent is not particularly limited, but is preferably a substituent containing a carbon atom, a hydrogen atom, and an oxygen atom.

[0093] Specific examples of urea derivatives include, for monosubstituted urea, methyl urea, ethyl urea, propyl urea, butyl urea, isobutyl urea, N-octadecyl urea, 2-hydroxyethyl urea, hydroxy urea, acetyl urea, allyl urea, 2-propynyl urea, cyclohexyl urea, phenyl urea, 3-hydroxyphenyl urea, (4-methoxyphenyl) urea, benzyl urea, benzoyl urea, o-tolyl urea, and p-tolyl urea.

[0094] Examples of disubstituted ureas include 1,1-dimethylurea, 1,3-dimethylurea, 1,1-diethylurea, 1,3-diethylurea, 1,3-bis(hydroxymethyl)urea, 1,3-tert-butylurea, 1,3-dicyclohexylurea, 1,3-diphenylurea, 1,3-bis(4-methoxyphenyl)urea, 1-acetyl-3-methylurea, 2-imidazolidinone (ethylene urea), and tetrahydro-2-pyrimidinone (propylene urea).

[0095] Examples of the tetrasubstituted urea include tetramethylurea, 1,1,3,3-tetraethylurea, 1,1,3,3-tetrabutylurea, 1,3-dimethoxy-1,3-dimethylurea, 1,3-dimethyl-2-imidazolidinone, and 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone.

[0096] (Thiocarbamide derivatives)

[0097] The thiourea derivative is a compound in which at least one of the four hydrogen atoms in the thiourea molecule is substituted with a substituent. In this case, the substituent is not particularly limited, but preferably a substituent containing a carbon atom, a hydrogen atom, and an oxygen atom.

[0098] Specific examples of thiourea derivatives include, for monosubstituted thiourea, N-methylthiourea, ethylthiourea, propylthiourea, isopropylthiourea, 1-butylthiourea, cyclohexylthiourea, N-acetylthiourea, N-allylthiourea, (2-methoxyethyl)thiourea, N-phenylthiourea, (4-methoxyphenyl)thiourea, N-(2-methoxyphenyl)thiourea, N-(1-naphthyl)thiourea, (2-pyridyl)thiourea, o-tolylthiourea, and p-tolylthiourea.

[0099] Examples of the disubstituted thiourea include 1,1-dimethylthiourea, 1,3-dimethylthiourea, 1,1-diethylthiourea, 1,3-diethylthiourea, 1,3-dibutylthiourea, 1,3-diisopropylthiourea, 1,3-dicyclohexylthiourea, N,N-diphenylthiourea, N,N'-diphenylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1-benzyl-3-phenylthiourea, 1-methyl-3-phenylthiourea, N-allyl-N'-(2-hydroxyethyl)thiourea and ethylenethiourea.

[0100] Examples of trisubstituted thiourea include trimethylthiourea, and examples of tetrasubstituted thiourea include tetramethylthiourea and 1,1,3,3-tetraethylthiourea.

[0101] In view of the fact that the decrease in transmittance under high temperature environment can be suppressed when used for an image display device composed of an interlayer filling structure, and the decrease in polarization degree is small (the aspect of orthogonal light leakage is suppressed), among urea compounds, urea derivatives or thiourea derivatives are preferred, and urea derivatives are more preferred. Among urea derivatives, monosubstituted urea or disubstituted urea is preferred, and monosubstituted is more preferred. Among disubstituted ureas, there are 1,1-substituted urea and 1,3-substituted urea, and 1,3-substituted urea is more preferred.

[0102] [Transparent protective film]

[0103] The transparent protective film used in the present invention (hereinafter also referred to as "protective film") is bonded to at least one side of the polarizing element via an adhesive layer. The transparent protective film is bonded to one side or both sides of the polarizing element, and more preferably bonded to both sides. In one embodiment, the protective film is bonded to the polarizing element via an adhesive layer as a layer containing a urea compound.

[0104] In addition, in the structure in which transparent protective films are bonded to both sides of the polarizing element via adhesive layers, only one side of the adhesive layers on both sides of the polarizing element may be the layer containing the urea compound of the present invention, but it is more preferred that both sides of the adhesive layers are the layers containing the urea compound of the present invention.

[0105] In recent years, in response to the demand for thinner polarizing plates, polarizing plates having a protective film only on one side of a polarizing element have been developed. In this configuration, the protective film is preferably laminated via an adhesive layer as the layer containing a urea compound of the present invention.

[0106] As a method for producing a polarizing plate having a protective film only on one side of a polarizing element, one method can be considered in which a polarizing plate having protective films bonded to both sides via adhesive layers is first produced and then the protective film on one side is peeled off. When using such a production method, it does not matter which adhesive layer is the layer containing the urea compound of the present invention, and it is more preferable to use the layer containing the urea compound of the present invention on both sides of the polarizing element.

[0107] When the urea compound-containing layer of the present invention is used as an adhesive layer only on one side of a polarizing element, it is preferred that the adhesive layer on the film side not to be peeled is the urea compound-containing layer of the present invention.

[0108] The protective film may have other optical functions at the same time, and may be formed into a laminated structure in which other layers are laminated.

[0109] From the viewpoint of optical properties, the protective film is preferably thin, but if it is too thin, the strength decreases and the processability is poor. The appropriate film thickness is 5 to 100 μm, preferably 10 to 80 μm, and more preferably 15 to 70 μm.

[0110] As the protective film, films such as cellulose acylate resin films, films made of polycarbonate resins, films made of cycloolefin resins such as norbornene, (meth)acrylic polymer films, and polyester resin films such as polyethylene terephthalate can be used.

[0111] In the case of a structure having protective films on both sides of the polarizing element, when bonding using a water-based adhesive such as a PVA adhesive, from the perspective of moisture permeability, it is preferred that the protective film on at least one side is either a cellulose acylate film or a (meth) acrylic polymer film, among which a cellulose acylate film is preferred.

[0112] At least one of the protective films may have a phase difference function for the purpose of viewing angle compensation or the like. In this case, the film itself may have the phase difference function, may have a phase difference layer separately, or may be a combination of both.

[0113] In addition, although the structure which directly bonds the film which has a phase difference function to a polarizing element via an adhesive is demonstrated, a structure which bonds via a binder or an adhesive via another protective film bonded to a polarizing element may be sufficient.

[0114] [Polarizing Plate Manufacturing Method]

[0115] The method for manufacturing a polarizing plate of the present embodiment has a lamination process and a moisture content adjustment process, in which a polarizing element and a layer containing a urea compound containing at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives are laminated. In the moisture content adjustment process, when manufacturing a polarizing plate having feature (a), the moisture content of the polarizing element is adjusted so that the moisture content of the polarizing element is greater than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, and less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%. The moisture content of the polarizing element can be adjusted according to the above-mentioned description of the moisture content of the polarizing element. In the moisture content adjustment process, when manufacturing a polarizing plate having feature (b), the moisture content of the polarizing plate is adjusted so that the moisture content of the polarizing plate is greater than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 30%, and less than the equilibrium moisture content at a temperature of 20°C and a relative humidity of 50%. The moisture content of the polarizing plate can be adjusted according to the above-mentioned description of the moisture content of the polarizing plate. The order of the lamination step and the moisture content adjustment step is not limited, and the lamination step and the moisture content adjustment step may be performed in parallel.

[0116] [Configuration of Image Display Device]

[0117] The polarizing plate of the present invention is used for various image display devices such as liquid crystal display devices and organic EL display devices. For image display devices, in the case of an interlayer filling structure that is constructed in a manner that the two sides of the polarizing plate contact the layers other than the air layer, the transmittance is easily reduced under a high temperature environment. In an image display device using the polarizing plate of the present invention, even if the interlayer filling structure is used, the reduction in the transmittance of the polarizing plate under a high temperature environment can be suppressed. As an image display device, an example can be given of a structure having an image display unit, a first adhesive layer stacked on the visible side surface of the image display unit, and a polarizing plate stacked on the visible side surface of the first adhesive layer. The image display device may also have a second adhesive layer stacked on the visible side surface of the polarizing plate, and a transparent component stacked on the surface of the second adhesive layer. In particular, the polarizing plate of the present invention can be suitably used for an image display device having the following interlayer filling structure, that is, a transparent component is arranged on the visible side of the image display device, the polarizing plate and the image display unit are bonded by the first adhesive layer, and the polarizing plate and the transparent component are bonded by the second adhesive layer. In this specification, either or both of the first adhesive layer and the second adhesive layer may be referred to as “adhesive layer.” It should be noted that the member used for laminating the polarizing plate and the image display unit or laminating the polarizing plate and the transparent member is not limited to the adhesive layer, but may also be an adhesive layer.

[0118] <Image Display Unit>

[0119] As the image display unit, a liquid crystal unit and an organic EL unit can be cited. As the liquid crystal unit, any of a reflective liquid crystal unit utilizing external light, a transmissive liquid crystal unit utilizing light from a light source such as a backlight, and a semi-transmissive and semi-reflective liquid crystal unit utilizing both light from the outside and light from the light source can be used. In the case where the liquid crystal unit is a liquid crystal unit utilizing light from a light source, the image display device (liquid crystal display device) is also configured with a polarizing plate on the side opposite to the visible side of the image display unit (liquid crystal unit), and a light source is also configured. The polarizing plate on the light source side is preferably bonded to the liquid crystal unit via an appropriate adhesive layer. As the driving mode of the liquid crystal unit, for example, a driving mode of any type such as a VA mode, an IPS mode, a TN mode, a STN mode, and a bending orientation (π type) can be used.

[0120] As the organic EL unit, an organic EL unit in which a transparent electrode, an organic light-emitting layer and a metal electrode are sequentially stacked on a transparent substrate to form a light-emitting body (organic electroluminescent light-emitting body) can be suitably used. The organic light-emitting layer is a laminate of various organic thin films, for example, a laminate of a hole injection layer containing a triphenylamine derivative or the like and a light-emitting layer containing a fluorescent organic solid such as anthracene, a laminate of these light-emitting layers and an electron injection layer containing a perylene derivative or the like, or a laminate of a hole injection layer, a light-emitting layer, and an electron injection layer can be used.

[0121] <Attachment of Image Display Unit and Polarizing Plate>

[0122] In laminating the image display unit and the polarizing plate, an adhesive layer (adhesive sheet) can be appropriately used. Among them, from the viewpoint of operability, etc., a method of laminating a polarizing plate with an adhesive layer having an adhesive layer attached to one surface of the polarizing plate and the image display unit is preferred. The attachment of the adhesive layer to the polarizing plate can be carried out in an appropriate manner. As an example, for example, there can be cited: a method of preparing an adhesive solution in which about 10 to 40 weight % of a base polymer or a combination thereof is dissolved or dispersed in a solvent formed by a single substance or a mixture of appropriate solvents such as toluene and ethyl acetate, and directly attaching it to the polarizing plate by an appropriate development method such as a casting method and a coating method; or a method of forming an adhesive layer on a spacer as described above and transferring it to the polarizing plate, etc.

[0123] <Adhesive Layer>

[0124] The adhesive layer is described in paragraphs

[0103] to

[0143] of JP-A-2018-025765, and these adhesives can be used in the present invention.

[0125] <Transparent components>

[0126] As a transparent member disposed on the visible side of the image display device, a front panel (window layer), a touch panel, etc. can be cited. As the front panel, a front panel with appropriate mechanical strength and thickness is used. As such a front panel, for example, a transparent resin plate such as an acrylic resin or a polycarbonate resin, or a glass plate, etc. can be cited. Functional layers such as an anti-reflection layer can also be stacked on the visible side of the front panel. In addition, when the front panel is a transparent resin plate, a hard coating layer can be stacked to improve physical strength, and a low moisture permeability layer can be stacked to reduce moisture permeability.

[0127] As the touch panel, various touch panels such as resistive film type, electrostatic capacitance type, optical type, ultrasonic type, etc., glass plates with touch sensor functions, transparent resin plates, etc. can be used. In the case of using an electrostatic capacitance type touch panel as a transparent member, it is preferred to further provide a front panel formed of a glass or transparent resin plate on the visible side relative to the touch panel.

[0128] <Lamination of polarizing plate and transparent member>

[0129] In laminating the polarizing plate and the transparent member, an adhesive or a UV curable adhesive can be used appropriately. When an adhesive is used, the adhesive can be attached in an appropriate manner. As a specific attachment method, for example, the attachment method of the adhesive layer used in laminating the aforementioned image display unit and the polarizing plate can be cited.

[0130] When a UV curing adhesive is used, in order to prevent the adhesive solution before curing from spreading, the following method can be appropriately used, that is, a dam material is provided in a manner surrounding the peripheral portion on the image display panel, a transparent member is placed on the dam material, and the adhesive solution is injected. After the injection of the adhesive solution, alignment and degassing are performed as needed, and then UV light is irradiated to perform curing.

[0131] Next, the layer containing the urea compound other than the adhesive layer will be described.

[0132] [Layer containing urea compound (other than adhesive layer)]

[0133] The layer containing a urea compound preferably contains at least one urea compound and a binder. Examples of the binder include polymer binders, thermosetting resin binders, and active energy ray-curable resin binders. Any of these binders can be preferably used in the present invention.

[0134] The thickness of the layer containing the urea compound is preferably 0.1 to 20 μm, more preferably 0.5 to 15 μm, and further preferably 1 to 10 μm.

[0135] The layer containing the urea compound may be directly laminated on the polarizing element or laminated via another layer. However, it is preferably laminated directly on the polarizing element so as to be in contact with the polarizing element in order to easily suppress a decrease in transmittance under a high temperature environment.

[0136] For a polarizing plate having a layer containing a urea compound other than an adhesive layer, it is preferred to have a transparent protective film on at least one surface of the polarizing element via the adhesive layer in order to improve the physical strength of the polarizing plate. In this case, the adhesive layer may or may not contain a urea compound, but it is more preferred to contain it.

[0137] As described in the description of the protective film, in recent years, in response to the demand for thinner polarizing plates, polarizing plates having a protective film only on one side of a polarizing element (hereinafter also referred to as "polarizing plates with a protective film on one side") have been developed.

[0138] In such a configuration, attempts have been made to laminate a cured layer on the surface of the polarizing element that does not have a protective film in order to improve physical strength and the like (for example, Japanese Patent Application Laid-Open No. 2011-221185).

[0139] In this embodiment, it is also one of the preferred methods to make such a solidified layer contain a urea compound as a layer containing a urea compound. Usually, such a solidified layer is formed by a curable composition containing an organic solvent, but paragraphs

[0020] to

[0042] of Japanese Patent Publication No. 2017-075986 describe a method of forming such a solidified layer from an aqueous solution of an active energy ray-curable polymer composition. Urea compounds are mostly water-soluble, so it is also one of the preferred methods of this embodiment to make such a composition contain a water-soluble urea compound and form a layer containing a urea compound.

[0140] <<Second Implementation Method>>

[0141] The polarizing plate of the second embodiment of the present invention comprises a polarizing element and a transparent protective film, wherein the polarizing element is formed by adsorbing iodine on a polyvinyl alcohol resin layer and orienting the iodine, and comprises at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives. The polarizing plate of this embodiment has at least one of the following (a) and (b).

[0142] (a) The moisture content of the polarizing element is not less than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and not more than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0143] (b) The moisture content of the polarizing plate is not less than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and not more than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 50%.

[0144] By making the polarizing plate of this embodiment have at least one of the above-mentioned (a) and (b) characteristics, and further making the polarizing element contain a urea-based compound, even when it is used for an image display device composed of interlayer filling and exposed to a high temperature environment for a long time, the decrease in the single transmittance can be suppressed. In the polarizing plate of this embodiment, by making the polarizing element contain a urea-based compound, even if the polarizing plate is exposed to a high temperature environment, the decrease in polarization degree can be suppressed, and it is also easy to suppress orthogonal light leakage.

[0145] The features of (a) and (b) described above are the same as the features of (a) and (b) of the first embodiment.

[0146] In the method for producing a polarizing element of the present embodiment, in the method for producing a polarizing element described in the first embodiment, there is a step of making the polarizing element contain a urea compound. As a method for making the polarizing element contain a urea compound, a polarizing element containing a urea compound can be obtained by making the polarizing element through a step of applying a solution containing a urea compound on at least one side of the polarizing element and drying it. In the manufacturing process of the polarizing element, the urea compound can also be contained in the polarizing element by a method of immersing a PVA-based resin layer in a treatment solution containing a urea compound, or by a method of spraying, flowing or dripping the treatment solution onto the PVA-based resin layer. Among them, it is preferred to use a method of immersing the PVA-based resin layer in a treatment solution containing a urea compound.

[0147] The process of immersing the PVA resin layer in a treatment solution containing a urea compound can be performed simultaneously with the swelling, stretching, dyeing, cross-linking, cleaning and other processes in the manufacturing method of the polarizing element, or can be set separately from these processes. The process of making the PVA resin layer contain a urea compound is preferably performed after the PVA resin layer is dyed with iodine, and more preferably simultaneously with the cross-linking process after dyeing. According to this method, the color tone changes little, and the influence on the optical properties of the polarizing element can be reduced.

[0148] The type and content of the urea compound contained in the polarizing element of this embodiment are the same as those of the first embodiment except that the urea compound-containing layer of the first embodiment is an optional component.

[0149] [Urea compound solution]

[0150] The solvent of the solution containing the urea compound used in this embodiment is preferably water, an organic solvent or a mixture thereof, and more preferably water or a mixed solvent of water and alcohol. In addition, in the case of a mixed solvent of water and alcohol, the alcohol is preferably methanol or ethanol. As described in the first embodiment, the urea compound is preferably water-soluble because the urea compound is not easily precipitated on the surface of the polarizing element after drying.

[0151] [Polarizing Plate Manufacturing Method]

[0152] The method for producing a polarizing plate according to the present embodiment includes a water content adjustment step. The water content adjustment step is the same as that of the method for producing a polarizing plate according to the first embodiment.

[0153] Example

[0154] Hereinafter, the present invention will be specifically described based on the examples. The materials, reagents, amounts and ratios thereof, operations, etc. shown in the following examples may be appropriately changed without departing from the gist of the present invention. Therefore, the present invention is not limited or restricted by the following examples.

[0155] (Production of Polarizing Element 1)

[0156] A polyvinyl alcohol film with a thickness of 40 μm formed of polyvinyl alcohol having an average degree of polymerization of about 2400 and a saponification degree of 99.9 mol% or more was uniaxially stretched to about 5 times in a dry manner, and then immersed in pure water at 60°C for 1 minute while maintaining the tension state, and then immersed in an aqueous solution with a weight ratio of iodine / potassium iodide / water of 0.05 / 5 / 100 at 28°C for 60 seconds. Thereafter, it was immersed in an aqueous solution with a weight ratio of potassium iodide / boric acid / water of 8.5 / 8.5 / 100 at 72°C for 300 seconds. Then, after washing with pure water at 26°C for 20 seconds, it was dried at 65°C to obtain a polarizing element with a thickness of 15 μm in which iodine was adsorbed and oriented on the polyvinyl alcohol.

[0157] (Preparation of PVA solution for adhesive)

[0158] 50 g of a modified PVA-based resin containing an acetoacetyl group (manufactured by Mitsubishi Chemical Corporation: GOHSENX Z-410) was dissolved in 950 g of pure water, and the mixture was heated at 90° C. for 2 hours and then cooled to room temperature to obtain a PVA solution for an adhesive.

[0159] (Preparation of urea compound solution)

[0160] 10 g of urea was added to 90 g of pure water to obtain a 10 wt% urea aqueous solution (solution 1). Similarly, according to Table 1, urea was replaced with the urea compounds described in Table 1 to prepare urea solutions 2 to 4.

[0161] [Table 1]

[0162]

[0163] Urea, methylurea, ethylurea, and tetrahydro-2-pyrimidinone used above were all reagents produced by Tokyo Chemical Industry Co., Ltd.

[0164] (Preparation of Adhesive 1 for Polarizing Plates)

[0165] The PVA solution for adhesive prepared above, urea solution 1, pure water and methanol were mixed so that the PVA concentration was 3.0%, the methanol concentration was 20% and the urea concentration was 0.5%, thereby obtaining an adhesive 1 for polarizing plates.

[0166] (Preparation of Adhesive 2 for Polarizing Plates)

[0167] Similarly, the adhesive PVA solution, the urea solution 2 shown in Table 1, pure water and methanol were mixed so that the PVA concentration was 3.0%, the methanol concentration was 20% and the methyl urea concentration was 0.7%, thereby obtaining an adhesive 2 for polarizing plates.

[0168] (Preparation of Adhesive 3 for Polarizing Plates)

[0169] Similarly, the adhesive PVA solution, urea solution 3 shown in Table 1, pure water and methanol were mixed so that the PVA concentration was 3.0%, the methanol concentration was 20% and the ethyl urea concentration was 1.0%, thereby obtaining an adhesive 3 for polarizing plates.

[0170] (Preparation of Adhesive 4 for Polarizing Plates)

[0171] Similarly, the adhesive PVA solution, urea solution 4 shown in Table 1, pure water and methanol were mixed so that the PVA concentration was 3.0%, the methanol concentration was 20% and the tetrahydro-2-pyrimidinone concentration was 1.5%, thereby obtaining an adhesive 4 for polarizing plates.

[0172] (Preparation of Adhesive 5 for Polarizing Plates)

[0173] Similarly, the PVA solution for an adhesive, pure water and methanol were mixed so that the PVA concentration was 3.0% and the methanol concentration was 20%, thereby obtaining an adhesive 5 for polarizing plates.

[0174] (Saponification of Cellulose Acylate Film)

[0175] A commercially available cellulose acylate film TD40 (manufactured by Fujifilm Corporation: film thickness 40 μm) was immersed in a 1.5 mol / L NaOH aqueous solution (saponification solution) maintained at 55°C for 2 minutes, then washed with water, and then immersed in a 0.05 mol / L sulfuric acid aqueous solution at 25°C for 30 seconds, and then washed with water under running water for 30 seconds to make the film neutral. Thereafter, water removal with an air knife was repeated three times, and after the water was removed, the film was retained in a drying zone at 70°C for 15 seconds for drying, thereby producing a saponified film.

[0176] (Production of Polarizing Plate 1)

[0177] The saponified cellulose acylate film prepared above was laminated to both sides of the polarizing element 1 via the polarizing plate adhesive 1 using a roll laminator, the thickness of the adhesive layer after drying was adjusted to 100 nm on both sides, and then dried at 60° C. for 10 minutes to obtain a polarizing plate 1 with cellulose acylate films on both sides.

[0178] (Production of Polarizing Plates 2 to 5)

[0179] Polarizing plates 2 to 5 were produced in the same manner as in the polarizing plate 1 except that the polarizing plate adhesive 1 was replaced with the polarizing plate adhesives 2 to 5 .

[0180] (Adjustment of Moisture Content of Polarizing Plate (Polarizing Element))

[0181] The polarizing plates 1 to 5 obtained above were stored for 72 hours at a temperature of 20°C and a relative humidity of 30%, 35%, 40%, 45%, 50% or 55%. The moisture content was measured using the Karl Fischer method after 66 hours, 69 hours and 72 hours of storage. Under any humidity conditions, the moisture content did not change after 66 hours, 69 hours and 72 hours of storage. Therefore, the moisture content of the polarizing plates 1 to 5 can be regarded as the same as the equilibrium moisture content of the 72-hour storage environment used in this experimental example. When the moisture content of the polarizing plate reaches equilibrium under a certain storage environment, the moisture content of the polarizing element in the polarizing plate can also be regarded as reaching equilibrium under the storage environment. In addition, when the moisture content of the polarizing element in the polarizing plate reaches equilibrium under a certain storage environment, the moisture content of the polarizing plate can also be regarded as reaching equilibrium under the storage environment.

[0182] (Production of Optical Laminated Body 1)

[0183] With reference to the example of Japanese Patent Publication No. 2018-025765, an acrylic adhesive (manufacturer: LINTEC, model: #7) was applied to both sides of the polarizing plate 1 prepared above, thereby preparing an optical laminate 1 having adhesive layers (first adhesive layer and second adhesive layer) with a thickness of 25 μm on both sides.

[0184] (Production of Optical Laminated Bodies 2 to 5)

[0185] Optical layered bodies 2 to 5 were produced in the same manner as in the optical layered body 1 except that the polarizing plate 1 was replaced with the polarizing plates 2 to 5 .

[0186] [Examples 1 to 9, Comparative Examples 1 to 6]

[0187] In Examples 1 to 9 and Comparative Examples 1 to 6, the optical layered bodies shown in Table 2 were used and stored for 72 hours at a temperature of 20° C. and a relative humidity of 35%, 40%, 45%, 50%, or 55% in such a manner that the moisture content of the optical layered bodies used was the equilibrium moisture content of the environment shown in Table 2. The moisture content of the optical layered bodies can be considered to be in equilibrium with the moisture content of the storage environment, and the moisture content of the polarizing plate and the polarizing element in the optical layered bodies can also be considered to be the same as the moisture content of the optical layered bodies.

[0188] (Polarizing plate 1 for inspection)

[0189] An acrylic adhesive (manufacturer: LINTEC (Strain), model: #7) was laminated only on one side of the polarizing plate 1 to produce a polarizing plate for inspection 1. The polarizing plate for inspection 1 produced in the above manner was cut into a size of 50 mm×100 mm so that the short side was parallel to the absorption axis, and the surface of the adhesive layer was bonded to an alkali-free glass (trade name "EAGLE XG", manufactured by Corning) to produce a sample 1 for orthogonal evaluation.

[0190] [Evaluation of single body transmittance after high temperature durability test (105°C)]

[0191] The optical layered bodies 1 to 5 prepared above were cut into a size of 50 mm×100 mm so that the long sides were parallel to the absorption axis, and the surfaces of the first and second adhesive layers were bonded to alkali-free glass (trade name “EAGLEXG”, manufactured by Corning) to prepare evaluation samples.

[0192] The evaluation sample was subjected to a temperature of 50°C and a pressure of 5 kgf / cm 2After 1 hour of autoclave treatment under the conditions of (490.3 kPa), the samples were placed in an environment of 23°C and 55% relative humidity for 24 hours. After that, the transmittance (initial value) was measured, and the samples were stored in a heated environment of 105°C, and the transmittance was measured every 50 hours until 100 to 200 hours. The evaluation was performed based on the time when the transmittance decreased by 5% or more relative to the initial value using the following criteria. The results are shown in Table 2.

[0193]

[0194] [Evaluation of cross light leakage after high temperature durability test]

[0195] After evaluating the single transmittance evaluation sample after high temperature durability for 200 hours, the optical laminate and the orthogonal evaluation sample 1 that was not placed in a heated environment were arranged in an orthogonal Nicol prism state and placed on a backlight. The surrounding light was shielded and the orthogonal light leakage was evaluated visually according to the following criteria. It should be noted that for samples whose single transmittance decreased by more than 5%, they were excluded from the evaluation of orthogonal light leakage due to coloration caused by polyene.

[0196]

[0197] [Table 2]

[0198]

Claims

1. A polarizing plate comprising a polarizing element in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin layer, and a transparent protective film, The polarizing plate comprises a urea compound-containing layer including at least one urea compound selected from urea, urea derivatives, thiourea, and thiourea derivatives. The moisture content of the polarizing element is equal to or higher than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and equal to or lower than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 35%.

2. A polarizing plate comprising a polarizing element formed by adsorbing iodine on a polyvinyl alcohol-based resin layer and orienting the iodine, and a transparent protective film, The polarizing plate comprises a urea compound-containing layer including at least one urea compound selected from urea, urea derivatives, thiourea, and thiourea derivatives. The moisture content of the polarizing plate is equal to or higher than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and is equal to or lower than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 35%.

3. The polarizing plate according to claim 1 or 2, in, The layer containing a urea compound contains at least one urea compound selected from urea derivatives and thiourea derivatives.

4. The polarizing plate according to claim 1 or 2, in, The layer containing a urea-based compound is in contact with the polarizing element.

5. The polarizing plate according to claim 1 or 2, in, The layer containing the urea compound is an adhesive layer.

6. The polarizing plate according to claim 5, in, The urea compound-containing layer includes a polyvinyl alcohol-based resin.

7. The polarizing plate according to claim 6, in, In the urea compound-containing layer, the total content of the urea compound is 0.1 parts by mass or more and 400 parts by mass or less relative to 100 parts by mass of the polyvinyl alcohol resin.

8. The polarizing plate according to claim 6 or 7, in, The thickness of the layer containing the urea compound is 0.01 μm to 7 μm.

9. A polarizing plate comprising a polarizing element formed by adsorbing iodine on a polyvinyl alcohol-based resin layer and orienting the iodine, and a transparent protective film, The polarizing element comprises at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives, The moisture content of the polarizing element is equal to or higher than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and equal to or lower than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 35%.

10. A polarizing plate comprising a polarizing element in which iodine is adsorbed and oriented on a polyvinyl alcohol-based resin layer, and a transparent protective film. The polarizing element comprises at least one urea compound selected from urea, urea derivatives, thiourea and thiourea derivatives, The moisture content of the polarizing plate is equal to or higher than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30%, and is equal to or lower than the equilibrium moisture content at a temperature of 20° C. and a relative humidity of 35%.

11. The polarizing plate according to any one of claims 1 to 2 and 9 to 10, in, The polarizing plate is used in an image display device. In the image display device, layers other than the air layer are provided in contact with both surfaces of the polarizing plate. 12 . An image display device comprising an image display unit, a first pressure-sensitive adhesive layer laminated on a visible-side surface of the image display unit, and the polarizing plate according to claim 1 laminated on the visible-side surface of the first pressure-sensitive adhesive layer. 13 . The image display device according to claim 12 , further comprising a second pressure-sensitive adhesive layer laminated on the visible-side surface of the polarizing plate, and a transparent member laminated on the visible-side surface of the second pressure-sensitive adhesive layer.

14. The image display device according to claim 13, in, The transparent member is a glass plate or a transparent resin plate.

15. The image display device according to claim 13, in, The transparent component is a touch panel.

16. A method for producing a polarizing plate, which is the method for producing a polarizing plate according to claim 1 or 9, The manufacturing method includes a moisture content adjustment step of adjusting the moisture content of the polarizing element to be greater than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30% and less than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 35%.

17. A method for producing a polarizing plate, which is the method for producing a polarizing plate according to claim 2 or 10, The manufacturing method includes a moisture content adjustment step of adjusting the moisture content of the polarizing plate to be greater than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 30% and less than an equilibrium moisture content at a temperature of 20° C. and a relative humidity of 35%.

Citation Information

Patent Citations

  • Liquid crystal panel support, electronic equipment having the same and manufacture of the same equipment

    JP1999174417A

  • Adhesive polarization plate and image display device

    JP2011221185A

  • Active energy ray-curing adhesive agent composition, polarization plate, optical film and image display device

    JP2012144690A

  • Polarizing film with adhesive layer and image display device

    JP2014048497A

  • Polarizing plate and image display device, and manufacturing method of those