A method for preparing carbonyl iron powder modified electromagnetic wave absorbing composite fiber material

By modifying the combination of carbonyl iron powder and graphene oxide, combined with PV particles and spray plate technology, composite fiber materials with high-efficiency electromagnetic wave absorption performance were prepared, which solved the shortcomings of existing fiber materials in electromagnetic wave absorption and realized electromagnetic waves. Effective absorption and attenuation effects.

CN114786458BActive Publication Date: 2024-11-15CHENGDU SANHONG HI-TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210542336.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-18
Publication Date
2024-11-15
Estimated Expiration
2042-05-18

AI Technical Summary

Technical Problem

Existing fiber materials have poor performance in the absorption and attenuation of electromagnetic waves and are unable to effectively resist and weaken electromagnetic wave radiation. Especially in specific industries, the demand for directed control of electromagnetic waves is urgent.

Method used

The preparation method of carbonyl iron powder modified electromagnetic wave absorption composite fiber material is adopted. The dissolution reaction of high-concentration alcohol diluted silica rheology control agent is added, modified sheet-like carbonyl iron powder and graphene oxide are added, and dried and vacuumed. The stirring treatment is combined with PV particles to form a multi-layer fiber composite film, and the fiber material is sprayed using spray plate technology to enhance the absorbance performance of the material.

Benefits of technology

The effective absorption and attenuation of electromagnetic waves is achieved, and the maximum absorption effect of electromagnetic waves exceeds -8dB to -16dB, which improves the high-temperature protection and construction properties of the material, reduces its own density, and breaks through the bottleneck of weight reduction and efficiency enhancement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114786458B_ABST
    Figure CN114786458B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of composite fiber materials, specifically to a method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material, the preparation steps comprising: S1: first dilute a silica rheology control agent with high concentration alcohol to carry out a dissolution reaction; S2: add the modified flaky carbonyl iron powder, put it into a reactor and mix and stir for 2 hours, add a protective gas during stirring, and control it at a corresponding temperature. The present invention uses carbonyl flaky iron powder to synthesize ferrite based on the existing basic material carbonyl flaky iron powder as the main absorbing material, and forms a silicon composite surface film on its surface through a surface coating process of the flaky carbonyl iron powder, thereby enhancing its surface high temperature protection and oxidation resistance, solving the high temperature failure barrier of the carbonyl iron powder, and mixing and adding the resin PV, utilizing its high temperature thermoforming characteristics, spraying the absorbing composite material into a fiberized silk board fabric, breaking through the bottleneck of product weight reduction and efficiency improvement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite fiber materials, and in particular to a method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material. Background Art

[0002] With the development of modern science and technology, the impact of electromagnetic radiation on the environment is increasing. Flights at airports cannot take off due to electromagnetic interference. In hospitals, mobile communications will interfere with the normal operation of various electronic diagnostic instruments. The guided control application of electromagnetic waves is even more important in special industries. Finding an absorbing material that can resist, weaken and eliminate electromagnetic radiation has become a major topic in materials science. Traditional fiber materials cannot absorb and attenuate the electromagnetic wave energy projected onto the surface of objects due to their own performance, and need to be improved.

[0003] Chinese patent number CN101203315B discloses fiber materials and composite materials, the method comprising: shearing a fiber source to provide a first fiber material; and passing the first fiber material through a first screen with an average opening size of 1.59 mm or less to provide a second fiber material, wherein the second fiber material has a BET surface area greater than 0.5 m2 / g, an average length of the second fiber material of 0.5-2.5 mm, a standard deviation of the length of the second fiber material of less than 60% of the average length of the second fiber material, and the fiber material has excellent mechanical properties, which are improved compared with the past, but does not play a corresponding role in the absorption and attenuation of electromagnetic waves, and needs to be improved.

[0004] Chinese patent number CN214193581U discloses an anti-fouling composite fiber material, which is woven from anti-fouling multifunctional yarns. The anti-fouling multifunctional yarns are composed of a core layer, an antistatic layer, an antibacterial thermal insulation layer, and an anti-fouling layer from the inside to the outside. The anti-fouling layer is woven from a mixed yarn twisted and formed by nitrile rubber fiber filaments and spandex fiber filaments. The core layer is composed of polyester fibers. The method provides an anti-fouling composite fiber material, which is a fiber material with anti-fouling and antistatic properties and is not easily deformed by washing. The material can be used to prepare clothing fabrics, especially sweater materials. This material cannot absorb and attenuate electromagnetic waves and needs to be improved. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme: a method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material, the preparation steps are as follows:

[0007] S1: First, use high concentration alcohol to dilute the silica rheology control agent to perform a dissolution reaction;

[0008] S2: Add the modified flaky carbonyl iron powder and put it into a reactor for mixing and stirring for 2 hours, add protective gas during stirring, and control at a corresponding temperature;

[0009] S3: adding carbonyl iron powder and graphene oxide, and continuing stirring. The stirring is carried out under the protection of inert gas and controlled at a specified temperature;

[0010] S4: vacuum pressure drying, the temperature is controlled at 80-110 degrees Celsius, the heating process adopts a step-by-step heating method, the temperature is kept constant for 2 hours, then the temperature is lowered to 80 degrees, and the temperature is kept constant for 5 hours;

[0011] S5: Add special PV particles to the processed powder, vacuum stir to a specified form, and then stir and mature;

[0012] S6: pouring the mixed liquid melted and stirred at high temperature into a solution into a pressure spray wet machine, and spraying it into a modified carbonyl iron powder composite electromagnetic absorbing fiber material or fiber cloth material of a desired thickness through nozzles of different calibers;

[0013] S7: After cooling and forming, a multi-layer fiber composite film is formed.

[0014] In order to ensure the effectiveness of the dissolution reaction of high-concentration alcohol, the present invention has an improvement that in S1, the concentration of the high-concentration alcohol is 99%.

[0015] In order to ensure that the processed material can be fully dissolved, the present invention has the following improvements: in S1, the temperature during the dissolution reaction is 20 to 25 degrees Celsius, and the reaction time is 60 minutes.

[0016] In order to avoid damage to the material during the stirring process, the present invention has an improvement that in S2, the protective gas is an inert gas and the corresponding temperature is 30 to 40 degrees Celsius.

[0017] In order to limit the stirring time and stirring temperature, the present invention has the following improvements: in S3, the stirring time is 30 to 60 minutes, and the specified temperature is 30 to 40 degrees Celsius.

[0018] In order to limit the temperature of vacuum stirring, the present invention has the following improvements: in S5, the temperature of vacuum stirring is 300 degrees Celsius, and the specified form is molten.

[0019] In order to ensure the perfection of material preparation, the present invention has an improvement that the stirring and aging time in S5 is 2 hours.

[0020] In order to realize the fiber discharging function of the nozzle, the present invention has the following improvements: in S6, the nozzle is a wire plate nozzle.

[0021] In order to ensure the quality of the multi-layer fiber composite film, the present invention has the following improvements: in S7, when the thickness of the multi-layer fiber composite film is 0.2 to 0.5 mm, the maximum electromagnetic wave absorption exceeds -8 dB to -16 dB.

[0022] Compared with the prior art, the advantages and positive effects of the present invention are:

[0023] The present invention adopts carbonyl flaky iron powder as the main wave absorbing material based on the carbonyl flaky iron powder as the basic material of the prior art, and the maximum electromagnetic wave absorption is -16dB. The surface coating process of the flaky carbonyl iron powder is used to generate a silicon composite surface film on the surface to repair the structural defects generated in the production process of the flaky iron powder, enhance the high temperature protection and oxidation resistance of the surface, improve the construction performance and physical and chemical properties of the subsequent processes, solve the high temperature failure barrier of the carbonyl iron powder, and mix the resin PV and utilize its high temperature thermoforming characteristics to spray the wave absorbing composite material into a fiberized silk board fabric, so that the new material formed has continuous loss and multi-directional loss, improves its wave absorbing performance and reduces its own density, and breaks through the bottleneck of product weight reduction and efficiency improvement. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The overall structural schematic diagram of a method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material proposed by the present invention;

[0025] Figure 2 The present invention provides a preparation flow chart of a method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material;

[0026] Figure 3 The present invention provides a schematic diagram of the test results of various embodiments of the method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material.

[0027] Legend:

[0028] 1. High and low temperature protection layer; 2. Guide layer; 3. Impedance matching layer; 4. Loss layer; 5. Reflection layer. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0030] In the description of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, in the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined.

[0031] See also Figure 1-3 The present invention provides a technical solution: a method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material, the preparation steps are as follows:

[0032] S1: First, use 99% alcohol to dilute the silica rheology control agent and perform a dissolution reaction. The temperature during the dissolution reaction is 22 degrees Celsius and the reaction time is 60 minutes.

[0033] S2: Add the modified flaky carbonyl iron powder and put it into a reactor for mixing and stirring for 2 hours, add inert gas during stirring, and control the temperature at 35 degrees Celsius;

[0034] S3: Add carbonyl iron powder and graphene oxide, continue stirring, the stirring is carried out under the protection of inert gas and controlled at 35 degrees Celsius, and the stirring time is 50 minutes;

[0035] S4: vacuum pressure drying, the temperature is controlled at 100 degrees Celsius, the temperature rise process adopts a step-by-step heating method, the temperature is kept constant for 2 hours, then the temperature is lowered to 80 degrees, and the temperature is kept constant for 5 hours;

[0036] S5: Add special PV particles to the processed powder, vacuum stir until molten, the vacuum stirring temperature is 300 degrees Celsius, and then stir and mature for 2 hours;

[0037] S6: pouring the mixed liquid melted and stirred at high temperature into a solution into a pressure wet spraying machine, and spraying it into a modified carbonyl iron powder composite electromagnetic absorbing fiber material or fiber cloth material of a desired thickness through a wire plate nozzle with different calibers;

[0038] S7: After cooling and molding, a multi-layer fiber composite film is formed. When the thickness of the multi-layer fiber composite film is 0.35 mm, the maximum electromagnetic wave absorption exceeds -12dB.

[0039] Embodiment 2

[0040] The preparation steps of the method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material are as follows:

[0041] S1: First, use 99% alcohol to dilute the silica rheology control agent and perform a dissolution reaction. The temperature during the dissolution reaction is 20 degrees Celsius and the reaction time is 60 minutes.

[0042] S2: Add the modified flaky carbonyl iron powder and put it into a reactor for mixing and stirring for 2 hours, add inert gas during stirring, and control the temperature at 30 degrees Celsius;

[0043] S3: Add carbonyl iron powder and graphene oxide, continue stirring, the stirring is carried out under the protection of inert gas and controlled at 30 degrees Celsius, and the stirring time is 30 minutes;

[0044] S4: vacuum pressure drying, the temperature is controlled at 80 degrees Celsius, the temperature rise process adopts a step-by-step heating method, the temperature is kept constant for 2 hours, then the temperature is lowered to 80 degrees, and the temperature is kept constant for 5 hours;

[0045] S5: Add special PV particles to the processed powder, vacuum stir until molten, the vacuum stirring temperature is 300 degrees Celsius, and then stir and mature for 2 hours;

[0046] S6: pouring the mixed liquid melted and stirred at high temperature into a solution into a pressure wet spraying machine, and spraying it into a modified carbonyl iron powder composite electromagnetic absorbing fiber material or fiber cloth material of a desired thickness through a wire plate nozzle with different calibers;

[0047] S7: After cooling and molding, a multi-layer fiber composite film is formed. When the thickness of the multi-layer fiber composite film is 0.2 mm, the maximum electromagnetic wave absorption exceeds -8dB.

[0048] Embodiment 3

[0049] The preparation steps of the method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material are as follows:

[0050] S1: First, use 99% alcohol to dilute the silica rheology control agent and perform a dissolution reaction. The temperature during the dissolution reaction is 25 degrees Celsius and the reaction time is 60 minutes.

[0051] S2: Add the modified flaky carbonyl iron powder and put it into a reactor for mixing and stirring for 2 hours, add inert gas during stirring, and control the temperature at 40 degrees Celsius;

[0052] S3: Add carbonyl iron powder and graphene oxide, continue stirring, the stirring is carried out under the protection of inert gas and controlled at 40 degrees Celsius, and the stirring time is 60 minutes;

[0053] S4: vacuum pressure drying, the temperature is controlled at 110 degrees Celsius, the temperature rise process adopts a step-by-step heating method, the temperature is lowered to 80 degrees after 2 hours of constant temperature, and the temperature is kept constant for 5 hours;

[0054] S5: Add special PV particles to the processed powder, vacuum stir until molten, the vacuum stirring temperature is 300 degrees Celsius, and then stir and mature for 2 hours;

[0055] S6: pouring the mixed liquid melted and stirred at high temperature into a solution into a pressure wet spraying machine, and spraying it into a modified carbonyl iron powder composite electromagnetic absorbing fiber material or fiber cloth material of a desired thickness through a wire plate nozzle with different calibers;

[0056] S7: After cooling and molding, a multi-layer fiber composite film is formed. When the thickness of the multi-layer fiber composite film is 0.5 mm, the maximum electromagnetic wave absorption exceeds -16dB.

[0057] Working principle: First, use 99% alcohol to dilute the silica rheology control agent for dissolution reaction. The temperature of the dissolution reaction is 25 degrees Celsius and the reaction time is 60 minutes. Add the modified flaky carbonyl iron powder and put it into the reactor for mixing and stirring for 2 hours. Add inert gas during stirring and control it at 40 degrees Celsius. Then add carbonyl iron powder and graphene oxide and continue stirring. Stirring is carried out under the protection of inert gas and controlled at 40 degrees Celsius. The stirring time is 60 minutes. Vacuum pressure drying, the temperature is controlled at 110 degrees Celsius, and the heating process adopts a step-by-step heating method. After 2 hours of constant temperature, the temperature is lowered to 80 degrees and kept at a constant temperature for 5 hours. Special PV particles are added to the processed powder and vacuum stirred until molten. The vacuum stirring temperature is 300 degrees Celsius, and then stirred and matured for 2 hours. The mixed liquid that is melted and stirred into a solution at high temperature is poured into a pressure spray machine and sprayed into a modified carbonyl iron powder composite electromagnetic absorbing fiber material or fiber cloth material of the required thickness through a wire plate nozzle with different calibers. After cooling and molding, a multi-layer fiber composite film is formed. When the thickness of the multi-layer fiber composite film is 0.5 mm, the maximum electromagnetic wave absorption exceeds -16dB.

[0058] The above are only preferred embodiments of the present invention and are not intended to limit the present invention in other forms. Any technician familiar with the profession may use the technical contents disclosed above to change or modify them into equivalent embodiments with equivalent changes and apply them to other fields. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a carbonyl iron powder modified electromagnetic wave absorbing composite fiber material, characterized in that: The preparation steps include: S1: First, use high concentration alcohol to dilute the silica rheology control agent to perform a dissolution reaction; S2: Add the modified flaky carbonyl iron powder and put it into a reactor for mixing and stirring for 2 hours, add protective gas during stirring, and control at a corresponding temperature; S3: adding carbonyl iron powder and graphene oxide, and continuing stirring. The stirring is carried out under the protection of inert gas and controlled at a specified temperature; S4: vacuum pressure drying, the temperature is controlled at 80-110 degrees Celsius, the heating process adopts a step-by-step heating method, the temperature is kept constant for 2 hours, then the temperature is lowered to 80 degrees, and the temperature is kept constant for 5 hours; S5: Add special PV particles to the processed powder, vacuum stir to a specified form, and then stir and mature; S6: pouring the mixed liquid melted and stirred at high temperature into a solution into a pressure spray wet machine, and spraying it into a modified carbonyl iron powder composite electromagnetic absorbing fiber material or fiber cloth material of a required thickness through nozzles of different calibers; S7: After cooling and forming, a multi-layer fiber composite film is formed.

2. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: In the S1, the concentration of the high-concentration alcohol is 99%.

3. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: In S1, the temperature during the dissolution reaction is 20 to 25 degrees Celsius, and the reaction time is 60 minutes.

4. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: In the S2, the protective gas is an inert gas, and the corresponding temperature is 30 to 40 degrees Celsius.

5. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: In S3, the stirring time is 30 to 60 minutes, and the specified temperature is 30 to 40 degrees Celsius.

6. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: In the above S5, the temperature of vacuum stirring is 300 degrees Celsius, and the specified state is molten.

7. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: The stirring and aging time in S5 is 2 hours.

8. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: In S6, the nozzle is a wire plate nozzle.

9. The method for preparing the carbonyl iron powder modified electromagnetic wave absorbing composite fiber material according to claim 1, characterized in that: In S7, when the thickness of the multi-layer fiber composite film is 0.2 to 0.5 mm, the maximum electromagnetic wave absorption exceeds -8 dB to -16 dB.