Curable resin composition, cured product and three-dimensional object
By using a curable resin composition containing a (meth)acryloyl group-containing urethane resin and an acrylate compound, the problems of insufficient elastic modulus and impact resistance of the cured product in the prior art are solved, and low viscosity is achieved. and excellent mechanical properties.
Patent Information
- Application Number
- CN202080086868.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-12-10
AI Technical Summary
The curable resin composition used in the existing optical three-dimensional modeling method cannot meet the requirements of high elastic modulus and impact resistance, has low viscosity and poor mechanical properties.
A curable resin composition containing a (meth)acryloyl group-containing urethane resin, a monofunctional and a difunctional (meth)acrylate compound is used, and a polyester polyol, a polyisocyanate and a hydroxyl group and a (methyl) group are used. Acryloyl compounds are used as reaction raw materials to adjust their viscosity and mechanical properties.
It achieves low viscosity and excellent mechanical properties, is suitable for optical three-dimensional modeling methods, and improves the elastic modulus and impact resistance of the hardened product.
Smart Images

Figure GDA0003695024220000041 
Figure GDA0003695024220000191
Abstract
Description
Technical Field
[0001] The present invention relates to a curable resin composition, a cured product and a three-dimensional object. Background Art
[0002] In recent years, as a method for manufacturing resin molded products, the following optical stereolithography method (optical stereolithography method) has been used, that is, based on the three-dimensional shape data designed by a three-dimensional design system such as three-dimensional computer aided design (CAD), a curable resin composition is selectively polymerized and cured by active energy rays such as ultraviolet lasers, thereby producing a three-dimensional object. The optical stereolithography method can also handle complex shapes that are difficult to cut, the manufacturing time is short, and the operation is easy. Therefore, in addition to resin molded products, it is also widely used in the manufacture of prototypes of industrial products.
[0003] As a representative example of the optical three-dimensional formation method, there can be cited a method for obtaining a three-dimensional object by repeatedly performing the following operations, namely, irradiating a liquid photocurable resin placed in a container with a point-shaped ultraviolet laser controlled by a computer from above to harden a layer of a specified thickness, lowering the object only by one layer, supplying liquid resin to the layer, and irradiating and hardening it in the same manner as described by ultraviolet laser light and laminating it. In addition, recently, in addition to the point drawing method using the point-shaped ultraviolet laser, the following surface exposure method has also been added, that is, using a light source other than a laser such as a light emitting diode (LED), through a surface drawing mask called a digital micromirror device (DMD) in which a plurality of digital micromirror shutters (digital micromirror shutters) are arranged in a surface shape, irradiating ultraviolet light from below through a transparent container containing photocurable resin, hardening a layer of a specified cross-sectional shape pattern, pulling the object only by one layer upward, irradiating and hardening the next layer in the same manner as described, and laminating in sequence to obtain a three-dimensional object.
[0004] The required properties of the photocurable resin used in the optical stereolithography method include low viscosity, the ability to form a smooth liquid surface, and excellent curability. As such photocurable resins, resin compositions containing free radical polymerizable compounds as the main component are known (for example, see Patent Documents 1 and 2), but they cannot meet the increasingly high performance requirements of today in terms of elastic modulus, elongation, and impact resistance.
[0005] Therefore, a material having low viscosity and capable of forming a cured product having excellent mechanical properties is desired.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Laid-Open No. 7-228644
[0009] Patent Document 2: Japanese Patent Application Publication No. 2008-189782 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The problem to be solved by the present invention is to provide a curable resin composition having low viscosity and excellent mechanical properties in a cured product, a cured product, and a three-dimensional shaped object.
[0012] Technical means of solving problems
[0013] The present inventors have conducted intensive studies to solve the above problems and have found that the above problems can be solved by using a curable resin composition containing a specific urethane resin and a specific acrylate compound, thereby completing the present invention.
[0014] That is, the present invention relates to a curable resin composition, a cured product, and a three-dimensional shaped product, wherein the curable resin composition contains a urethane resin (A) having a (meth)acryloyl group, and a monofunctional (meth)acrylate compound (B1) and / or a difunctional (meth)acrylate compound (B2), wherein the urethane resin (A) contains a polyester polyol (a1), a polyisocyanate (a2), and a compound (a3) containing a hydroxyl group and a (meth)acryloyl group as essential reaction raw materials, and the polyester polyol (a1) contains a diol (a1-1) having a hydrocarbon group in a side chain, and a polycarboxylic acid (a1-2) as essential reaction raw materials.
[0015] Effects of the Invention
[0016] The curable resin composition of the present invention has low viscosity and can form a cured product with excellent mechanical properties, so it can be suitably used as a resin composition for optical three-dimensional molding. In addition, the so-called "excellent mechanical properties" in the present invention refers to excellent "elastic modulus" and "impact resistance". DETAILED DESCRIPTION
[0017] The curable resin composition of the present invention contains a urethane resin (A) having a (meth)acryloyl group, and a monofunctional (meth)acrylate compound (B1) and / or a bifunctional (meth)acrylate compound (B2).
[0018] In the present invention, "(meth)acrylate" refers to acrylate and / or methacrylate. In addition, "(meth)acryloyl" refers to acryloyl and / or methacryloyl. Furthermore, "(meth)acrylic" refers to acrylic and / or methacrylic.
[0019] The urethane resin (A) must have a (meth)acryloyl group.
[0020] As the urethane resin (A), polyester polyol (a1), polyisocyanate (a2) and a compound (a3) having a hydroxyl group and a (meth)acryloyl group are essential reaction raw materials, and the polyester polyol (a1) uses a polyester polyol having a diol (a1-1) having a hydrocarbon group in a side chain and a polycarboxylic acid (a1-2) as essential reaction raw materials.
[0021] As the polyester polyol (a1), as described above, a polyester polyol having a diol (a1-1) having a hydrocarbon group in a side chain and a polycarboxylic acid (a1-2) as essential reaction raw materials is used.
[0022] The diol (a1-1) having a hydrocarbon group on a side chain is not particularly limited in the number of branches and the molecular weight, and may be any compound. Specific examples thereof include 2-methyl-1,3-propanediol, neopentyl glycol, 2-ethyl-1,3-propanediol, 2-methyl-1,4-butanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-ethylbutane-14-butanediol, 2,3-dimethyl-1,4-butanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 3,3-dimethylpentane-1,5-diol, 2,2-diethyl-1,3-propanediol, 3-propylpentane-1,5-diol, 2,2-diethyl-1,4-butanediol, 2,4-diethyl-1,5-pentanediol, 2,2-dipropyl-1,3-propanediol, 2-ethyl-2-butyl-1,3-propanediol, and 2,5-diethyl-1,6-hexanediol. The diols (a1-1) having a hydrocarbon group in a side chain in the molecular structure may be used alone or in combination of two or more. Among these, 3-methylpentanediol is preferred in terms of obtaining a curable resin composition having a low viscosity and being able to form a cured product having excellent mechanical properties.
[0023] As the polycarboxylic acid (a1-2), for example, aliphatic polycarboxylic acids such as succinic acid, adipic acid, azelaic acid, sebacic acid, glutaric acid, pimelic acid, suberic acid, dodecanedicarboxylic acid, maleic acid, and fumaric acid can be listed; alicyclic polycarboxylic acids such as 1,3-cyclopentanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; aromatic polycarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, biphenyl dicarboxylic acid, and 1,2-bis(phenoxy)ethane-p,p′-dicarboxylic acid. These polycarboxylic acids can be used alone or in combination of two or more. Among these, aliphatic polycarboxylic acids are preferred in terms of obtaining a curable resin composition having a low viscosity and being able to form a cured product having excellent mechanical properties.
[0024] In order to obtain a curable resin composition having low viscosity and capable of forming a cured product having excellent mechanical properties, the number average molecular weight (Mn) of the polyester polyol (a1) is preferably in the range of 1,000 to 10,000, and more preferably in the range of 1,500 to 8,000. In the present invention, the "number average molecular weight (Mn)" is a value measured using a gel permeation chromatograph (GPC).
[0025] The polyester polyol (a1) can be produced by any method without any particular limitation, for example, a method in which the diol (a1-1) having a hydrocarbon group in a side chain and the polycarboxylic acid (a1-2) are subjected to a dehydration condensation reaction at a temperature range of 200° C. to 280° C. until the acid value is 5 mg / KOH or less.
[0026] Examples of the polyisocyanate (a2) include aliphatic diisocyanate compounds such as butane diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate; alicyclic diisocyanate compounds such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylene diisocyanate, and hydrogenated diphenylmethane diisocyanate; toluene diisocyanate, xylene diisocyanate, and diisocyanate; Aromatic diisocyanate compounds such as isocyanate, tetramethylxylene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, 4,4′-diisocyanato-3,3′-dimethylbiphenyl, and o-tolidine diisocyanate; polymethylene polyphenyl polyisocyanate having a repeating structure represented by the following structural formula (1); isocyanurate-modified products, biuret-modified products, and allophanate-modified products thereof. In addition, these polyisocyanates may be used alone or in combination of two or more.
[0027] [Chemistry 1]
[0028]
[0029] [Where R 1 R are each independently any one of a hydrogen atom and a hydrocarbon group having 1 to 6 carbon atoms. 2 Each independently represents an alkyl group having 1 to 4 carbon atoms, or any of the bonding points connected to the structural part represented by the structural formula (1) via a methylene group marked with an *. l represents 0 or an integer of 1 to 3, and m represents an integer of 1 to 15.]
[0030] Examples of the compound (a3) having a hydroxyl group and a (meth)acryloyl group include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, trimethylolpropane (meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol (meth)acrylate, dipentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, di-trimethylolpropane (meth)acrylate, di-trimethylolpropane di(meth)acrylate, and di-trimethylolpropane tri(meth)acrylate. In addition, (poly)oxyalkylene modified products in which (poly)oxyethylene chains, (poly)oxypropylene chains, (poly)oxytetramethylene chains, etc. are introduced into the molecular structure of the above-mentioned various compounds having hydroxyl groups and (meth)acryloyl groups; or lactone modified products in which (poly)lactone structures are introduced into the molecular structure of the above-mentioned various compounds having hydroxyl groups and (meth)acryloyl groups, etc. can also be used. These compounds having hydroxyl groups and (meth)acryloyl groups can be used alone or in combination of two or more.
[0031] In order to obtain a curable resin composition having low viscosity and capable of forming a cured product having excellent mechanical properties, the content of the urethane resin (A) is preferably in the range of 3% by mass to 50% by mass, and more preferably in the range of 20% by mass to 40% by mass, based on the solid content of the curable resin composition of the present invention.
[0032] There is no particular limitation on the method for producing the carbamate resin (A), and the carbamate resin can be produced by any method. For example, the carbamate resin can be produced by reacting all the reaction raw materials containing the polyester polyol (a1), the polyisocyanate (a2), and the compound (a3) having a hydroxyl group and a (meth) acryloyl group, or by reacting the reaction raw materials in sequence. Furthermore, in terms of a curable resin composition having a low viscosity and capable of forming a cured product with excellent mechanical properties, the total of the hydroxyl group (OH) possessed by the polyester polyol (a1) and the compound (a3) having a hydroxyl group and a (meth) acryloyl group, and the equivalent ratio (OH / NCO) of the isocyanate group (NCO) possessed by the polyisocyanate (a2) is preferably in the range of 0.9 / 1 to 1 / 0.9, more preferably 1 / 1.
[0033] In the production of the urethane resin (A), dibutyltin laurate, dibutyltin acetate, etc. can be used as a catalyst, and the urethane resin (A) can be produced under the conditions of a commonly performed urethane reaction. In addition, as necessary, a solvent such as ethyl acetate, butyl acetate, methyl isobutyl ketone, toluene, xylene, or a free radical polymerizable monomer that does not contain a site reactive with isocyanate and does not contain a hydroxyl group or an amino group can be used as a solvent.
[0034] Examples of the monofunctional (meth)acrylate compound (B1) include phenoxyethyl (meth)acrylate, phenoxybenzyl (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, cyclohexylmethyl (meth)acrylate, cyclohexylethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dipropylene glycol mono(meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, isononyl (meth)acrylate, benzyl (meth)acrylate, phenylbenzyl (meth)acrylate, lauryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and (meth)acrylate. ethoxyethoxyethyl methacrylate, 2-(meth)acryloyloxyethyl succinate, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylmethoxy (meth)acrylate, 2-ethylethoxy (meth)acrylate, 2-ethylbutoxy (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, butoxydiethylene glycol (meth)acrylate, Butoxytriethylene glycol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, (meth)acryloylmorpholine, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl hexahydrophthalate, glycidyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate ) acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, pentamethylpiperidinyl (meth)acrylate, tetramethylpiperidinyl (meth)acrylate, (meth)acrylate (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl ester, 3,4-epoxycyclohexylmethyl methacrylate, cyclic trimethylolpropane formal (meth)acrylate, 1-adamantyl (meth)acrylate, 2-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, etc. These monofunctional (meth)acrylate compounds can be used alone or in combination of two or more. In addition, among these, in terms of the curable resin composition that can obtain a low viscosity and can form a cured product with excellent mechanical properties, it is preferably a compound whose glass transition temperature (hereinafter referred to as "Tg") of the polymer of the monofunctional (meth)acrylate compound is above 80°C.Among them, preferred are (meth)acrylate compounds having cyclic structures such as condensed polycyclic structures and heterocyclic structures, and further preferred are acryloylmorpholine (Tg: 145°C), isobornyl acrylate (Tg: 94°C), isobornyl methacrylate (Tg: 180°C), dicyclopentenyl acrylate (Tg: 120°C), dicyclopentanyl acrylate (Tg: 120°C), and dicyclopentanyl methacrylate (Tg: 175°C), and particularly preferred is acryloylmorpholine.
[0035] Furthermore, when two or more monofunctional (meth)acrylate compounds (B1) are used in combination, it is preferred that the Tg of the copolymer of the two or more monofunctional (meth)acrylate compounds is 80° C. or higher.
[0036] Examples of the difunctional (meth)acrylate compound (B2) include 1,6-hexanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide-modified 1,6-hexanediol di(meth)acrylate, hydroxytrimethylol neopentyl glycol di(meth)acrylate, propylene oxide-modified Neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, ethylene oxide-modified di(meth)acrylate of bisphenol A, propylene oxide-modified di(meth)acrylate of bisphenol A, ethylene oxide-modified di(meth)acrylate of bisphenol F, tricyclodecane dimethanol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, glycerol Propylene oxide modified tri(meth)acrylate, 2-hydroxy-3-acryloxypropyl (meth)acrylate, ethylene oxide modified di(meth)acrylate of bisphenoxyethanol fluorene, polytetramethylene glycol di(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, phenoxyethylene glycol (meth)acrylate, stearyl (meth)acrylate, 2-(meth)acryloxyethyl succinate, trifluoroethyl (meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 2 , 3-[(meth)acryloyloxymethyl]norbornane, 2,5-[(meth)acryloyloxymethyl]norbornane, 2,6-[(meth)acryloyloxymethyl]norbornane, 1,3-adamantyl di(meth)acrylate, 1,3-bis[(meth)acryloyloxymethyl]adamantane, tris(hydroxyethyl)isocyanuric acid di(meth)acrylate, 3,9-bis[1,1-dimethyl-2-(meth)acryloyloxyethyl]-2,4,8,10-tetra-side oxygen spiro[5.5]undecane, etc. These difunctional (meth)acrylate compounds can be used alone or in combination of two or more. In addition, among these, in terms of a curable resin composition that can obtain a low viscosity and can form a cured product with excellent mechanical properties, a compound whose Tg of a polymer of a difunctional (meth)acrylate compound is above 80°C is preferred. Among them, dipropylene glycol diacrylate (Tg: 102°C) and tricyclodecane dimethanol diacrylate (Tg: 110°C) are more preferred.
[0037] Furthermore, when two or more difunctional (meth)acrylate compounds (B2) are used in combination, it is preferred that the Tg of the copolymer of the two or more difunctional (meth)acrylate compounds is 80° C. or higher.
[0038] The monofunctional (meth)acrylate compound (B1) and the difunctional (meth)acrylate compound (B2) may be used in combination. In such a case, the Tg of the copolymer of the (meth)acrylate compound used in combination is preferably 80° C. or higher.
[0039] Furthermore, the monofunctional (meth)acrylate compound (B1) and / or the difunctional (meth)acrylate compound (B2) and a trifunctional or higher (meth)acrylate compound may be used in combination as needed within the range not hindering the effects of the present invention. In such a case, it is also preferred that the Tg of the copolymer of the (meth)acrylate compound used in combination is 80° C. or higher.
[0040] Examples of the trifunctional or higher (meth)acrylate compound include: trifunctional (meth)acrylates such as ethylene oxide (EO)-modified glycerol acrylate, propylene oxide (PO)-modified glycerol triacrylate, pentaerythritol triacrylate, EO-modified phosphoric acid triacrylate, trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, hydroxypropyl acrylate (HPA)-modified trimethylolpropane triacrylate, (EO)- or (PO)-modified trimethylolpropane triacrylate, alkyl-modified dipentaerythritol triacrylate, and tri(acryloyloxyethyl) isocyanurate.
[0041] Tetrafunctional (meth)acrylates such as di-trimethylolpropane tetraacrylate, pentaerythritol ethoxy tetraacrylate, and pentaerythritol tetraacrylate;
[0042] Pentafunctional (meth)acrylates such as dipentaerythritol hydroxy pentaacrylate and alkyl-modified dipentaerythritol pentaacrylate;
[0043] Hexafunctional (meth)acrylates such as dipentaerythritol hexaacrylate. These trifunctional or higher functional (meth)acrylates may be used alone or in combination of two or more.
[0044] The curable resin composition of the present invention further contains a photopolymerization initiator. Examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propane-1-one, thioxanthone and thioxanthone derivatives, 2,2′-dimethoxy-1,2-diphenylethane-1-one, diphenyl(2,4,6-trimethoxybenzoyl)phosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phosphine oxide, and bis(2,4,6-trimethylbenzoyl)phosphine oxide. phenylphosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, ethyl phenyl(2,4,6-trimethylbenzoyl)phosphonate, ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate (TPO-L), etc.
[0045] Examples of commercially available photopolymerization initiators include: "Omnirad-1173", "Omnirad-184", "Omnirad-127", "Omnirad-2959", "Omnirad-369", "Omnirad-379", "Omnirad-907", "Omnirad-4265", and "Omnirad- -1000", "Omnirad-651", "Omnirad-TPO", "Omnirad-819", "Omnirad-2022", "Omnirad-2100", "Omnirad-754", "Omnirad-784", "Omnirad-500", "Omnirad-81 ... "Kayacure-DETX", "Kayacure-MBP", "Kayacure-DMBI", "Kayacure-EPA", "Kayacure-OA" (manufactured by Nippon Kayaku Co., Ltd.); "Vicure-10", "Vicure-55" (manufactured by Stoff Chemical Co., Ltd.); "Trigonal P1" (manufactured by Akzo); "Sandoray 1000" (manufactured by SANDOZ); "Deap" (manufactured by APJOHN); "Quantacure-PDO", "Quantacure-ITX", "Quantacure-EPD" (manufactured by Ward Blenkinsop); "Runtecure-1104" (manufactured by Runtec), etc.
[0046] In the curable resin composition, the photopolymerization initiator is preferably used in an amount within a range of, for example, 1% by mass to 20% by mass.
[0047] Furthermore, a photosensitizer may be added to the curable resin composition as necessary to improve the curability.
[0048] Examples of the photosensitizer include amine compounds such as aliphatic amines and aromatic amines, urea compounds such as o-tolylthiourea, and sulfur compounds such as sodium diethyldithiophosphate and s-benzylisothiouronium-p-toluenesulfonate.
[0049] The curable resin composition of the present invention may contain various additives such as ultraviolet absorbers, antioxidants, polymerization inhibitors, silicon-based additives, fluorine-based additives, silane coupling agents, phosphate compounds, organic beads, inorganic fine particles, organic fillers, inorganic fillers, rheology control agents, degassing agents, and colorants as needed.
[0050] Examples of the ultraviolet absorber include triazine derivatives such as 2-[4-{(2-hydroxy-3-dodecyloxypropyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and 2-[4-{(2-hydroxy-3-tridecyloxypropyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine; 2-(2′-xanthenecarboxyl-5′-methylphenyl)benzotriazole, 2-(2′-o-nitrobenzyloxy-5′-methylphenyl)benzotriazole, 2-xanthenecarboxyl-4-dodecyloxybenzophenone, and 2-o-nitrobenzyloxy-4-dodecyloxybenzophenone. These ultraviolet absorbers may be used alone or in combination of two or more.
[0051] Examples of the antioxidant include hindered phenol antioxidants, hindered amine antioxidants, organic sulfur antioxidants, phosphate antioxidants, etc. These antioxidants may be used alone or in combination of two or more.
[0052] Examples of the polymerization inhibitor include hydroquinone, quinone, di-tert-butylhydroquinone, p-methoxyphenol, butylhydroxytoluene, and nitrosamine salts.
[0053] Examples of the silicon-based additive include dimethylpolysiloxane, methylphenylpolysiloxane, cyclic dimethylpolysiloxane, methylhydrogenpolysiloxane, polyether-modified dimethylpolysiloxane copolymers, polyester-modified dimethylpolysiloxane copolymers, fluorine-modified dimethylpolysiloxane copolymers, amino-modified dimethylpolysiloxane copolymers, and other polyorganosiloxanes having an alkyl group or a phenyl group, polyether-modified polydimethylsiloxane having an acrylic group, polyester-modified polydimethylsiloxane having an acrylic group, etc. These silicon-based additives may be used alone or in combination of two or more.
[0054] Examples of the fluorine-based additive include "Megaface" series manufactured by DIC Corporation. These fluorine-based additives may be used alone or in combination of two or more.
[0055] Examples of the silane coupling agent include vinyl trichlorosilane, vinyl trimethoxysilane, vinyl triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, 3-glycidyloxypropyl trimethoxysilane, 3-glycidyloxypropyl methyl diethoxysilane, 3-glycidyloxypropyl triethoxysilane, p-phenylene trimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-acryloxypropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2-(aminoethyl)-3-aminopropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl trimethoxysilane, Vinyl silane coupling agents such as 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride, special aminosilane, 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, allyltrichlorosilane, allyltriethoxysilane, allyltrimethoxysilane, diethoxymethylvinylsilane, and vinyltri(2-methoxyethoxy)silane;
[0056] Epoxy silane coupling agents such as diethoxy(glycidoxypropyl)methylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane;
[0057] Styrene-based silane coupling agents such as p-styryltrimethoxysilane;
[0058] (Meth)acryloxy-based silane coupling agents such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane;
[0059] Amino silane coupling agents such as N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane;
[0060] Urea-based silane coupling agents such as 3-ureidopropyltriethoxysilane;
[0061] Chloropropyl silane coupling agents such as 3-chloropropyltrimethoxysilane;
[0062] Mercapto-based silane coupling agents such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane;
[0063] Sulfide silane coupling agents such as bis(triethoxysilylpropyl)tetrasulfide;
[0064] Isocyanate-based silane coupling agents such as 3-isocyanatepropyltriethoxysilane, etc. These silane coupling agents may be used alone or in combination of two or more.
[0065] Examples of the phosphate compound include compounds having a (meth)acryloyl group in the molecular structure, and examples of commercially available products include "Kayamer PM-2" and "Kayamer PM-21" manufactured by Nippon Kayaku Co., Ltd., "Light Ester P-1M", "Light Ester P-2M", and "Light Acrylate P-1A (N)" manufactured by Kyoeisha Chemical Co., Ltd., "SIPOMER PAM 100", "SIPOMER PAM 200", "SIPOMER PAM 300", and "SIPOMER PAM 4000" manufactured by Solvay, "Viscoat #3PA" and "Viscoat #3PMA" manufactured by Osaka Organic Chemical Industry Co., Ltd., and "New Frontier" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. "Frontier S-23A"; "SIPOMER PAM 5000" manufactured by SOLVAY, which is a phosphate ester compound having an allyl ether group in its molecular structure.
[0066] Examples of the organic beads include polymethyl methacrylate beads, polycarbonate beads, polystyrene beads, polyacrylic styrene beads, silicone beads, glass beads, acrylic beads, benzoguanamine resin beads, melamine resin beads, polyolefin resin beads, polyester resin beads, polyamide resin beads, polyimide resin beads, polyvinyl fluoride resin beads, polyethylene resin beads, etc. These organic beads may be used alone or in combination of two or more. In addition, the average particle size of these organic beads is preferably in the range of 1 μm to 10 μm.
[0067] The inorganic particles include, for example, particles of silicon dioxide, aluminum oxide, zirconium oxide, titanium dioxide, barium titanate, antimony trioxide, etc. These inorganic particles can be used alone or in combination of two or more. In addition, the average particle size of these inorganic particles is preferably in the range of 95nm to 250nm, and more preferably in the range of 100nm to 180nm.
[0068] In the case of containing the inorganic particles, a dispersing aid can be used. As the dispersing aid, for example, phosphate compounds such as isopropyl acid phosphate, triisodecyl phosphite, and ethylene oxide modified phosphoric acid dimethyl acrylate can be listed. These dispersing aids can be used alone or in combination of two or more. In addition, as commercial products of the dispersing aid, for example, "Kayamer PM-21" and "Kayamer PM-2" manufactured by Nippon Kayaku Co., Ltd., "Light Ester P-2M" manufactured by Kyoeisha Chemical Co., Ltd. can be listed.
[0069] Examples of the organic filler include plant-derived solvent-insoluble substances such as cellulose, lignin, and cellulose nanofibers.
[0070] Examples of the inorganic filler include glass (particles), silica (particles), alumina-silicate, talc, mica, aluminum hydroxide, aluminum oxide, calcium carbonate, and carbon nanotubes.
[0071] Examples of the rheology control agent include amide waxes such as "Disparlon 6900" manufactured by Kusumoto Chemicals Co., Ltd.; urea rheology control agents such as "BYK410" manufactured by BYK-Chemie; polyethylene waxes such as "Disparlon 4200" manufactured by Kusumoto Chemicals Co., Ltd.; and cellulose acetate butyrates such as "CAB-381-2" and "CAB 32101" manufactured by Eastman Chemical Products.
[0072] Examples of the defoaming agent include oligomers containing fluorine or silicon atoms, oligomers such as higher fatty acids and acrylic acid polymers, and the like.
[0073] Examples of the colorant include pigments and dyes.
[0074] As the pigment, known and commonly used inorganic pigments or organic pigments can be used.
[0075] Examples of the inorganic pigment include titanium oxide, antimony red, red iron, cadmium red, cadmium yellow, cobalt blue, Prussian blue, ultramarine blue, carbon black, and graphite.
[0076] Examples of the organic pigment include quinacridone pigments, quinacridonequinone pigments, dioxazine pigments, phthalocyanine pigments, anthraquinone pigments, anthraquinone pigments, indanthrone pigments, flavanthrone pigments, perylene pigments, diketopyrrolopyrrole pigments, perinone pigments, quinonaphthalone pigments, anthraquinone pigments, thioindigo pigments, benzimidazolone pigments, and azo pigments. These pigments may be used alone or in combination of two or more.
[0077] As the dye, for example, azo dyes such as monoazo-disazo, metal complex dyes, naphthol dyes, anthraquinone dyes, indigo dyes, carbonium dyes, quinoneimine dyes, cyanine dyes, quinoline dyes, nitro dyes, nitroso dyes, benzoquinone dyes, naphthoquinone dyes, naphthalimide dyes, perinone dyes, phthalocyanine dyes, triallyl methane dyes, etc. can be listed. These dyes can be used alone or in combination of two or more.
[0078] The cured product of the present invention can be obtained by irradiating the curable resin composition with active energy rays. Examples of the active energy rays include ultraviolet rays, electron beams, ionizing radiation such as α rays, β rays, and γ rays. In addition, when ultraviolet rays are used as the active energy rays, the irradiation may be performed in an inert gas environment such as nitrogen or in an air environment in order to efficiently perform the curing reaction using ultraviolet rays.
[0079] As the ultraviolet light source, ultraviolet lamps are generally used from the viewpoint of practicality and economy, and specific examples thereof include low-pressure mercury lamps, high-pressure mercury lamps, ultrahigh-pressure mercury lamps, xenon lamps, gallium lamps, metal halide lamps, sunlight, and LEDs.
[0080] The cumulative light intensity of the active energy rays is not particularly limited, but is preferably 50 mJ / cm 2 ~5,000mJ / cm 2 , more preferably 300 mJ / cm 2~1,000mJ / cm 2 When the integrated light amount is within the above range, the generation of uncured portions can be prevented or suppressed, which is preferred.
[0081] The three-dimensional structure of the present invention can be produced by a known optical three-dimensional structure method.
[0082] Examples of the optical three-dimensional forming method include a stereolithography apparatus (SLA) method, a digital light processing (DLP) method, and an inkjet method.
[0083] The so-called stereolithography (SLA) method is a method of irradiating active energy rays such as laser beams in the form of points on grooves of a liquid curable resin composition, and curing them layer by layer while moving a molding table to form a three-dimensional shape.
[0084] The digital light processing (DLP) method is a method of irradiating a groove of a liquid curable resin composition with active energy rays such as LEDs in a planar manner, and curing the composition layer by layer while moving a molding table to perform three-dimensional molding.
[0085] The inkjet photolithography method is a method in which minute droplets of a curable resin composition for photolithography are ejected from a nozzle to draw a predetermined shape pattern, and then irradiated with ultraviolet rays to form a cured film.
[0086] Among these optical three-dimensional forming methods, the DLP method is preferable because it can perform high-speed forming based on a surface.
[0087] The DLP method is not particularly limited as long as it is a method using a DLP method optical forming system. As the forming conditions, in order to improve the forming accuracy of the three-dimensional object, it is necessary that the stacking pitch of the optical forming is in the range of 0.01 mm to 0.2 mm, the irradiation wavelength is in the range of 350 nm to 410 nm, and the light intensity is 0.5 mW / cm 2 ~50mW / cm 2 The accumulated light intensity of each layer is 1mJ / cm 2 ~100mJ / cm 2 In terms of the further improvement of the shaping accuracy of the three-dimensional object, it is preferred that the stacking spacing of the optical shaping is in the range of 0.02 mm to 0.1 mm, the irradiation wavelength is in the range of 380 nm to 410 nm, and the light intensity is 5 mW / cm 2 ~15mW / cm 2 The cumulative amount of light per layer is 5mJ / cm 2 ~15mJ / cm 2range.
[0088] The three-dimensional structure of the present invention has a high elastic modulus and excellent impact resistance, and therefore can be suitably used in, for example, automobile parts, aerospace-related parts, electrical and electronic parts, home appliances, building materials, interior decoration, jewelry, medical materials, etc.
[0089] Example
[0090] Hereinafter, the present invention will be specifically described by way of Examples and Comparative Examples.
[0091] In addition, in this Example, the number average molecular weight (Mn) and the weight average molecular weight (Mw) are values measured using gel permeation chromatography (GPC) under the following conditions.
[0092] Measuring device: HLC-8220 manufactured by Tosoh Corporation
[0093] Column: Guard column H manufactured by Tosoh Corporation XL -H
[0094] +TSKgel G5000HXL manufactured by Tosoh Corporation
[0095] +TSKgel G4000HXL manufactured by Tosoh Corporation
[0096] +TSKgel G3000HXL manufactured by Tosoh Corporation
[0097] +TSKgel G2000HXL manufactured by Tosoh Corporation
[0098] Detector: RI (differential refractometer)
[0099] Data processing: SC-8010 manufactured by Tosoh Corporation
[0100] Measurement conditions: column temperature 40°C
[0101] Solvent tetrahydrofuran
[0102] Flow rate 1.0ml / min
[0103] Standard: Polystyrene
[0104] Sample: A tetrahydrofuran solution having a resin solid content of 0.4% by mass was filtered through a microfilter (100 μl)
[0105] (Synthesis Example 1: Synthesis of polyester polyol (1))
[0106] 448 parts by mass of 3-methyl-1,5-pentanediol and 352 parts by mass of adipic acid were added to a reaction vessel including a stirrer, a condenser and a thermometer. The mixture was stirred under a nitrogen gas stream and reacted at 200°C to 250°C for 18 hours to obtain a polyester polyol (1). The polyester polyol (1) had a number average molecular weight (Mn) of 500, a weight average molecular weight (Mw) of 1,100, an acid value of 2.4 mgKOH / g and a hydroxyl value of 220 mgKOH / g. The hydroxyl value and the acid value were values measured by a neutralization titration method according to Japanese Industrial Standards (JIS) K 0070 (1992).
[0107] (Synthesis Example 2: Synthesis of polyester polyol (2))
[0108] 378 parts by mass of 3-methyl-1,5-pentanediol and 422 parts by mass of adipic acid were added to a reaction vessel including a stirrer, a condenser and a thermometer. The mixture was stirred under a nitrogen gas flow and reacted at 200°C to 250°C for 18 hours to obtain a polyester polyol (2). The polyester polyol (2) had a number average molecular weight (Mn) of 2,100, a weight average molecular weight (Mw) of 3,800, an acid value of 3.0 mgKOH / g and a hydroxyl value of 56 mgKOH / g.
[0109] (Synthesis Example 3: Synthesis of polyester polyol (3))
[0110] 359 parts by mass of 3-methyl-1,5-pentanediol and 441 parts by mass of adipic acid were added to a reaction vessel including a stirrer, a condenser and a thermometer. The mixture was stirred under a nitrogen gas flow and reacted at 200° C. to 250° C. for 18 hours to obtain a polyester polyol (3). The polyester polyol (3) had a number average molecular weight (Mn) of 9,800, a weight average molecular weight (Mw) of 19,400, an acid value of 3.2 mgKOH / g and a hydroxyl value of 9 mgKOH / g.
[0111] (Synthesis Example 4: Synthesis of polyester polyol (4))
[0112] 353 parts by mass of neopentyl glycol and 450 parts by mass of adipic acid were added to a reaction vessel including a stirrer, a condenser and a thermometer. The mixture was stirred under a nitrogen gas flow and reacted at 200° C. to 250° C. for 18 hours to obtain a polyester polyol (4). The polyester polyol (4) had a number average molecular weight (Mn) of 2,000, a weight average molecular weight (Mw) of 4,200, an acid value of 3.0 mgKOH / g and a hydroxyl value of 53 mgKOH / g.
[0113] (Synthesis Example 5: Synthesis of polyester polyol (5))
[0114] 262 parts by mass of ethylene glycol and 571 parts by mass of adipic acid were added to a reaction vessel including a stirrer, a condenser and a thermometer. The mixture was stirred under a nitrogen gas flow and reacted at 200°C to 250°C for 18 hours to obtain a polyester polyol (5). The polyester polyol (5) had a number average molecular weight (Mn) of 2,300, a weight average molecular weight (Mw) of 4,800, an acid value of 2.0 mgKOH / g and a hydroxyl value of 49 mgKOH / g.
[0115] (Synthesis Example 6: Synthesis of Urethane Resin (A-1) Having Acryloyl Group)
[0116] In a 1-liter flask equipped with a stirrer, a gas introduction tube, a condenser, and a thermometer, 297 parts by mass of isophorone diisocyanate, 1.6 parts by mass of tert-butylhydroxytoluene, 0.2 parts by mass of methoxyhydroquinone, and 0.2 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C, and 347 parts by mass of the polyester polyol (1) obtained in Synthesis Example 1 was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C for 3 hours, and then 155 parts by mass of hydroxyethyl acrylate was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C until 2250 cm-1 of the isocyanate group was obtained. -1 The infrared absorption spectrum of disappeared, and a urethane resin (A-1) having an acryloyl group was obtained.
[0117] (Synthesis Example 7: Synthesis of Urethane Resin (A-2) Having Acryloyl Group)
[0118] In a 1-liter flask equipped with a stirrer, a gas introduction tube, a condenser, and a thermometer, 131 parts by mass of isophorone diisocyanate, 1.6 parts by mass of tert-butylhydroxytoluene, 0.2 parts by mass of methoxyhydroquinone, and 0.2 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C. 600 parts by mass of the polyester polyol (2) obtained in Synthesis Example 2 was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C for 3 hours, and then 68 parts by mass of hydroxyethyl acrylate was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C until 2250 cm-1 of the isocyanate group was reached. -1 The infrared absorption spectrum of disappeared, and a urethane resin (A-2) having an acryloyl group was obtained.
[0119] (Synthesis Example 8: Synthesis of Urethane Resin (A-3) Having Acryloyl Group)
[0120] In a 1-liter flask equipped with a stirrer, a gas introduction tube, a condenser, and a thermometer, 27 parts by mass of isophorone diisocyanate, 1.6 parts by mass of tert-butylhydroxytoluene, 0.2 parts by mass of methoxyhydroquinone, and 0.2 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C, and 760 parts by mass of the polyester polyol (3) obtained in Synthesis Example 3 was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C for 3 hours, and then 14 parts by mass of hydroxyethyl acrylate was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C until 2250 cm-1 of the isocyanate group was obtained. -1 The infrared absorption spectrum of disappeared, and a urethane resin (A-3) having an acryloyl group was obtained.
[0121] (Synthesis Example 9: Synthesis of Urethane Resin (A-4) Having Acryloyl Group)
[0122] In a 1-liter flask equipped with a stirrer, a gas introduction tube, a condenser, and a thermometer, 125 parts by mass of isophorone diisocyanate, 1.6 parts by mass of tert-butylhydroxytoluene, 0.2 parts by mass of methoxyhydroquinone, and 0.2 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C. 609 parts by mass of the polyester polyol (4) obtained in Synthesis Example 4 was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C for 3 hours, and then 65 parts by mass of hydroxyethyl acrylate was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C until 2250 cm-1 of the isocyanate group was obtained. -1 The infrared absorption spectrum of disappeared, and a urethane resin (A-4) having an acryloyl group was obtained.
[0123] (Synthesis Example 10: Synthesis of Urethane Resin (A-5) Having Acryloyl Group)
[0124] In a 1-liter flask equipped with a stirrer, a gas introduction tube, a condenser, and a thermometer, 118 parts by mass of isophorone diisocyanate, 1.6 parts by mass of tert-butylhydroxytoluene, 0.2 parts by mass of methoxyhydroquinone, and 0.2 parts by mass of dibutyltin diacetate were added, and the temperature was raised to 70°C, and 620 parts by mass of the polyester polyol (5) obtained in Synthesis Example 5 was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C for 3 hours, and then 62 parts by mass of hydroxyethyl acrylate was added dropwise over 1 hour. After the addition, the reaction was allowed to proceed at 70°C until 2250 cm-1 of the isocyanate group was obtained. -1 The infrared absorption spectrum of disappeared, and a urethane resin (A-5) having an acryloyl group was obtained.
[0125] (Example 1: Preparation of curable resin composition (1))
[0126] Into a four-necked flask equipped with a stirrer, a thermometer and a cooling tube, 30 parts by mass of the urethane resin (A-1) having an acryloyl group obtained in Synthesis Example 6 and 70 parts by mass of acryloylmorpholine ("ACMO" manufactured by KJ Chemical Co., Ltd.) were placed, and stirred at 60° C. or less until uniformly dissolved, to obtain a curable resin composition (1).
[0127] (Example 2 to Example 9: Preparation of Curable Resin Compositions (2) to (9))
[0128] Except having changed the composition and the compounding amount of the urethane resin and the (meth)acrylate compound which have an acrylic group into the thing shown in Table 1, it carried out similarly to Example 1, and obtained the curable resin composition (2) - curable resin composition (9).
[0129] (Comparative Examples 1 to 3: Preparation of Curable Resin Compositions (C1) to (C3))
[0130] Curable resin compositions (C1) to (C3) were obtained by the same method as in Example 1 except that the urethane resin having an acrylic group and the (meth)acrylate compound used in Example 1 were changed to the compositions and blending amounts shown in Table 1.
[0131] The following evaluations were performed using the curable resin compositions obtained in Examples 1 to 9 and Comparative Examples 1 to 3.
[0132] [Viscosity measurement]
[0133] The viscosity at 25° C. of the curable resin composition obtained in each of Examples and Comparative Examples was measured using an E-type viscometer (“TV-22” manufactured by Toki Sangyo Co., Ltd.).
[0134] [Preparation of test pieces]
[0135] A photolithography 3D printer (ACCULAS BA-30S manufactured by D-MEC Co., Ltd.) was used to produce a dumbbell for tensile testing (based on American Society for Testing and Materials (ASTM) D638 TYPE1) and a specimen for Izod impact testing (based on ASTM D256). Next, the dumbbell for tensile testing and the specimen for Izod impact testing obtained by photolithography were cleaned with isopropyl alcohol, dried at room temperature for 1 hour, and then irradiated with ultraviolet (UV) light (10000 mJ / cm each) on both sides using a high-pressure mercury lamp as post-hardening.2 ), and obtained test piece 1 (dumbbell for tensile test) and test piece 2 (specimen for Izod impact test).
[0136] [Determination method of elastic modulus and elongation]
[0137] In accordance with ASTM D638, the test piece 1 was used to perform a tensile test with Autograph "AG-Xplus 100 kN" manufactured by Shimadzu Corporation (load cell 100 kN, head speed 5 mm / min, test piece width 10 mm) to measure the elastic modulus and elongation.
[0138] [Measurement method of Izod impact strength (impact resistance)]
[0139] The Izod impact strength was measured using the test piece 2 in accordance with ASTM D256 using a “universal impact tester” manufactured by Toyo Seiki Seisaku-sho, Ltd.
[0140] Table 1 shows the compositions and evaluation results of the curable resin compositions obtained in Examples 1 to 9 and Comparative Examples 1 to 3.
[0141]
Claims
1. A curable resin composition comprising: a urethane resin (A) having a (meth)acryloyl group, a monofunctional (meth)acrylate compound (B1) and a difunctional (meth)acrylate compound (B2), wherein: The urethane resin (A) has polyester polyol (a1), polyisocyanate (a2) and a compound (a3) having a hydroxyl group and a (meth)acryloyl group as essential reaction raw materials. The polyester polyol (a1) has a diol (a1-1) having a hydrocarbon group in a side chain and a polycarboxylic acid (a1-2) as essential reaction raw materials. The number average molecular weight of the polyester polyol (a1) is in the range of 2,000 to 2,100, and The glass transition temperature of the copolymer of the monofunctional (meth)acrylate compound (B1) and the difunctional (meth)acrylate compound (B2) is 80° C. or higher. 2 . The curable resin composition according to claim 1 , wherein the diol (a1-1) comprises 3-methylpentanediol. 3 . The curable resin composition according to claim 1 , wherein a content of the urethane resin (A) in a solid content of the curable resin composition is in a range of 3% by mass to 50% by mass.
4. The curable resin composition according to claim 1, wherein the monofunctional (meth)acrylate compound (B1) is one or more selected from the group consisting of (meth)acryloylmorpholine, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.
5. A hardened product, characterized in that: A hardening reaction product of the curable resin composition according to any one of claims 1 to 4. 6 . The cured product according to claim 5 , wherein the curing condition is irradiation with active energy rays.
7. A three-dimensional object, characterized in that: The hardener according to claim 5 or 6 is included.