Reinforced materials and structures
By using a combination of thermosetting resin, tackifying resin and vulcanizing agent in the reinforcing material, combined with aliphatic aromatic copolymerized petroleum resin, the problem of improving the reinforcing performance of the existing reinforcing materials is solved, and the high strength of the resin layer is achieved. High adhesion significantly improves the fracture strength of the reinforcement member.
Patent Information
- Application Number
- CN202080090354.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-27
- Filing Date
- 2020-10-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-10-15
AI Technical Summary
There is room for improvement in the reinforcement properties of existing reinforcement materials, especially in terms of adhesion and curing strength of the resin layer.
Using a combination of a resin layer containing a thermosetting resin, a tackifying resin and a vulcanizing agent, the tackifying resin has a specific softening temperature and bromine value, and aliphatic aromatic copolymerized petroleum resin is used as a tackifying resin, and the binding layer is combined to improve the reinforcing layer. curing strength.
While ensuring the adhesion of the resin layer, the strength of the reinforcement material is improved, and the fracture strength and adhesion of the reinforcement member are significantly improved.
Smart Images

Figure CN114845869B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a reinforced material and a reinforced structure. Background Art
[0002] Conventionally, there is known a reinforcing material (reinforcing sheet) having a constraining layer and a reinforcing layer. The reinforcing layer contains at least styrene-butadiene rubber, epoxy resin, and a foaming agent (for example, see Patent Document 1).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2005-41210 Summary of the invention
[0006] Problems to be solved by the invention
[0007] In the reinforcing material described in Patent Document 1, further improvement in reinforcing performance is required.
[0008] Therefore, an object of the present invention is to provide a reinforcing material and a reinforcing structure capable of achieving improved reinforcement performance.
[0009] Means for solving problems
[0010] The present invention [1] includes a reinforcing material comprising: a resin layer comprising a thermosetting resin, a diene rubber, a tackifier resin and a vulcanizing agent; and a constraining layer disposed on the resin layer, wherein the thermosetting resin comprises a flexible epoxy resin, the tackifier resin has a softening temperature of 75° C. or higher and 100° C. or lower, the bromine value of the tackifier resin is 30 gBr2 / 100 g or higher, and the vulcanizing agent is contained in an amount of 20 parts by mass or less relative to a total of 100 parts by mass of the diene rubber and the tackifier resin.
[0011] The present invention [2] comprises the reinforcing material of the above-mentioned [1], wherein the tackifier resin is an aliphatic-aromatic copolymer petroleum resin containing a structural unit derived from an aliphatic monomer and a structural unit derived from an aromatic monomer.
[0012] The present invention [3] includes the reinforcing material of the above [2], wherein the ratio of the structural unit derived from the aliphatic monomer to the total of the structural unit derived from the aliphatic monomer and the structural unit derived from the aromatic monomer is higher than 50% by mass.
[0013] The present invention [4] includes a reinforcement structure, which includes a reinforcement object and a reinforcement component for reinforcing the above-mentioned reinforcement object, and the above-mentioned reinforcement component includes: a reinforcement layer, which is formed by a cured product of the above-mentioned resin layer of the above-mentioned [1], and the above-mentioned reinforcement layer is arranged on the above-mentioned reinforcement object, and the above-mentioned constraint layer of the above-mentioned [1] is arranged on the above-mentioned reinforcement layer.
[0014] Effects of the Invention
[0015] According to the reinforcing material and the reinforced structure of the present invention, the resin layer contains the tackifying resin having a specific softening temperature and a specific bromine value.
[0016] Therefore, the strength of the reinforcing material formed by curing the resin layer can be improved while ensuring the adhesive force of the resin layer.
[0017] As a result, the reinforcement performance of the reinforcing material can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a cross-sectional view of a reinforcing material as one embodiment of the present invention.
[0019] FIG. 2 is used to illustrate the use of Figure 1 FIG. 1 is an explanatory diagram of a method of reinforcing an object to be reinforced by a reinforcing material shown in FIG. Figure 2A It refers to the process of attaching the reinforcement material to the reinforcement object. Figure 2B This refers to a curing step of foaming and curing the reinforcement object to which the reinforcement material is attached. DETAILED DESCRIPTION
[0020] 1. Reinforcement material 1
[0021] Figure 1 The reinforcing material 1 shown is used to reinforce the object P (refer to Figure 2B ) is a member to be reinforced. As the reinforcement object P, for example, metal plates such as aluminum plates, stainless steel plates, iron plates, copper plates, zinc plates, and brass plates can be cited. It should be noted that the metal plate can be used for transportation equipment such as automobiles, railway vehicles, ships, and aircraft, such as buildings. Preferably, the reinforcement material 1 is a reinforcement sheet. The reinforcement material 1 has a resin layer 2 and a constraint layer 3. The reinforcement material 1 has a release sheet 4 as needed.
[0022] (1) Resin layer 2
[0023] The resin layer 2 has a predetermined thickness and has a first surface S1 and a second surface S2 in the thickness direction of the resin layer 2 .
[0024] The thickness of the resin layer 2 is, for example, 0.1 mm or more, preferably 0.2 mm or more, and for example, 10 mm or less, preferably 5 mm or less.
[0025] The resin layer 2 is formed by a resin composition containing a thermosetting resin, a diene rubber, a tackifying resin and a vulcanizing agent. The resin composition preferably contains a vulcanization accelerator, a thermosetting resin curing agent and a foaming agent in addition to the above components. It should be noted that the resin composition may also contain additives such as fillers, pigments, and thixotropic materials in addition to the above components.
[0026] (1-1) Thermosetting resin
[0027] The thermosetting resin contains a flexible epoxy resin. The flexible epoxy resin has higher flexibility than bisphenol A epoxy resin. Preferably, the flexible epoxy resin has higher flexibility than the aromatic epoxy resin described below. More preferably, the flexible epoxy resin has higher flexibility than other epoxy resins described below.
[0028] The flexible epoxy resin does not contain a cyclic structure (e.g., an aromatic ring, an aliphatic hydrocarbon ring, a nitrogen-containing ring, etc.) in the main chain, or contains less cyclic structures than other epoxy resins described later. Preferably, the flexible epoxy resin has a soft component in the main chain instead of a cyclic structure. Examples of the soft component include a non-cyclic aliphatic hydrocarbon component, a rubber component, a polyol component, and the like.
[0029] The epoxy equivalent of the flexible epoxy resin is, for example, 220 g / eq or more, preferably 300 g / eq or more, and more preferably 500 g / eq or more. If the epoxy equivalent is above the lower limit, the reinforcing member 11 (see Figure 2B It should be noted that the reinforcing member 11 includes a reinforcing layer 5 which is a cured product of the resin layer 2 and a constraining layer 3.
[0030] The epoxy equivalent of the flexible epoxy resin is, for example, 2000 g / eq or less, or preferably 1200 g / eq or less. When the epoxy equivalent is equal to or less than the above upper limit, the strength of the reinforcing member 11 described below can be ensured.
[0031] Specifically, as flexible epoxy resin, for example, aliphatic modified epoxy resin, butadiene epoxy resin, ε-caprolactone modified epoxy resin, thiol epoxy resin, rubber (for example NBR, carboxyl terminal NBR, amino terminal NBR, etc.) modified epoxy resin, dimer acid modified epoxy resin, carbamate modified epoxy resin, polyol modified epoxy resin, amine modified epoxy resin, etc. can be enumerated. As flexible epoxy resin, from the viewpoint of compatibility with rubber, the adhesion of resin layer 2, preferably aliphatic modified epoxy resin, rubber modified epoxy resin, dimer acid modified epoxy resin can be enumerated, and more preferably dimer acid modified epoxy resin can be enumerated. Flexible epoxy resin can be used in combination with multiple.
[0032] Examples of commercially available flexible epoxy resins include jER (registered trademark) series (manufactured by Mitsubishi Chemical Corporation), such as jER871, jER872, and jER872X75.
[0033] The thermosetting resin may contain epoxy resins other than the flexible epoxy resin.
[0034] As other epoxy resins, for example, there can be mentioned bisphenol epoxy resins (for example, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, etc.), novolac epoxy resins (for example, phenol novolac epoxy resin, cresol novolac epoxy resin, etc.), naphthalene epoxy resins, biphenyl epoxy resins and other aromatic epoxy resins, for example, bicyclic epoxy resins, hydrogenated bisphenol A epoxy resins and other alicyclic epoxy resins, for example, triglycidyl isocyanurate, hydantoin epoxy resin, triglycidyl isocyanurate resin and other nitrogen-containing epoxy resins, and the like.
[0035] The thermosetting resin is contained in the resin layer 2 (resin composition) in an amount of, for example, 30% by mass or more, preferably 35% by mass or more, for example, 50% by mass or less, preferably 40% by mass or less.
[0036] The flexible epoxy resin is contained in 100 parts by mass of the thermosetting resin in an amount of, for example, 50 parts by mass or more, preferably 60 parts by mass or more, for example, 100 parts by mass or less.
[0037] (1-2) Diene rubber
[0038] Examples of the diene rubber include styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), isoprene rubber, butadiene rubber, etc. Preferably, NBR and polybutadiene rubber are used in combination.
[0039] The proportion of the diene rubber relative to 100 parts by mass of the thermosetting resin is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and, for example, 500 parts by mass or less, preferably 300 parts by mass or less, more preferably 100 parts by mass or less.
[0040] (1-3) Tackifying resin
[0041] The tackifier resin imparts adhesiveness to the resin layer 2 .
[0042] The tackifier resin has a specific softening temperature and a specific bromine value. It should be noted that the bromine value is determined by the amount of unsaturated bonds in the tackifier resin. Therefore, "having a specific bromine value" means having a specific amount of unsaturated bonds.
[0043] The softening temperature of the tackifier resin is, for example, 75° C. or higher, preferably 80° C. or higher, and more preferably 85° C. or higher. When the softening temperature of the tackifier resin is at least the lower limit value described above, the strength of the reinforcing member 11 described below can be ensured.
[0044] The softening temperature of the tackifier resin is, for example, 100° C. or less, or preferably 96° C. or less. When the softening temperature of the tackifier resin is equal to or less than the above upper limit, the adhesiveness of the resin layer 2 to the reinforcement object P can be ensured.
[0045] The softening temperature is measured by the method specified in JIS K 5601-2-2:1999.
[0046] The strength of the reinforcing member 11 is evaluated by the breaking strength of the reinforcing member 11. The breaking strength of the reinforcing member 11 is measured by the method described in Examples described later.
[0047] The breaking strength of the reinforcing member 11 is, for example, 250 N / cm or more, preferably 260 N / cm or more. If the breaking strength of the reinforcing layer 5 is equal to or greater than the above lower limit, the reinforcement object P can be reliably reinforced. It should be noted that the upper limit of the breaking strength of the reinforcing member 11 is not limited.
[0048] The adhesive force of the resin layer 2 was evaluated as the adhesive force of the resin layer 2 at 5° C. The adhesive force of the resin layer 2 at 5° C. was measured by the method described in Examples described later.
[0049] The adhesive force of the resin layer 2 at 5°C is, for example, 5 N / 10 mm or more, preferably 10 N / 10 mm or more, and more preferably 30 N / 10 mm or more. If the adhesive force of the resin layer 2 at 5°C is greater than or equal to the above lower limit, it is possible to suppress the reinforcing material 1 attached to the reinforcement object P from falling off. It should be noted that the upper limit of the adhesive force of the resin layer 2 at 5°C is not limited.
[0050] The bromine value of the tackifier resin is, for example, 30 gBr2 / 100 g or more, preferably 35 gBr2 / 100 g or more, and more preferably 40 gBr2 / 100 g or more. If the bromine value of the tackifier resin is equal to or greater than the above lower limit, the strength of the reinforcing member 11 described below can be improved.
[0051] It should be noted that the upper limit of the bromine value of the tackifier resin is not limited. The bromine value of the tackifier resin is, for example, 100 gBr2 / 100 g or less.
[0052] The bromine value is measured by the method described in the examples described later.
[0053] The weight average molecular weight of the tackifier resin is, for example, 1000 or more, preferably 2000 or more, and more preferably 3000 or more. When the weight average molecular weight of the tackifier resin is equal to or more than the above lower limit, the strength of the reinforcing member 11 described below can be ensured.
[0054] The weight average molecular weight of the tackifier resin is, for example, 5000 or less, preferably 4000 or less. When the weight average molecular weight of the tackifier resin is below the upper limit, the tackifier resin can be easily compatible with the diene rubber and the thermosetting resin, and the adhesion of the resin layer 2 to the reinforcement object P can be ensured.
[0055] The weight average molecular weight is measured by gel permeation chromatography (GPC) as a standard polystyrene conversion value.
[0056] Examples of the tackifier resin include natural resin-based tackifier resins and synthetic resin-based tackifier resins.
[0057] Examples of the natural resin tackifier resin include rosin resins such as rosin esters, and terpene resins such as aromatic modified terpene resins and terpene phenolic resins.
[0058] Examples of the synthetic resin tackifier resin include aliphatic (C5) petroleum resins, aromatic (C9) petroleum resins, and aliphatic-aromatic copolymer (C5 / C9) petroleum resins.
[0059] Aliphatic (C5) petroleum resins mainly contain structural units derived from aliphatic monomers having 5 carbon atoms, such as isoprene and piperylene. Aliphatic (C5) petroleum resins are produced by polymerizing a mixture (C5 fraction) of aliphatic hydrocarbons having 5 carbon atoms (such as isoprene and piperylene) produced as by-products by thermal decomposition of naphtha.
[0060] Aromatic (C9) petroleum resins mainly contain structural units derived from aromatic monomers having a carbon number of 9, such as styrene, vinyltoluene, and indene. Aromatic (C9) petroleum resins are produced by polymerizing a mixture (C9 fraction) of aromatic hydrocarbons having a carbon number of 9 (such as styrene, vinyltoluene, indene, etc.) produced as by-products by thermal decomposition of naphtha.
[0061] Aliphatic aromatic copolymer (C5 / C9) petroleum resin mainly contains structural units derived from the above-mentioned aliphatic monomers and structural units derived from the above-mentioned aromatic monomers. Aliphatic aromatic copolymer (C5 / C9) petroleum resin is produced by polymerizing C5 fraction and C9 fraction.
[0062] The tackifier resin is preferably a synthetic resin-based tackifier resin, and more preferably an aliphatic aromatic copolymer-based petroleum resin.
[0063] When the tackifying resin is an aliphatic-aromatic copolymer petroleum resin, the ratio of the structural units derived from the aliphatic monomer to the total of the structural units derived from the aliphatic monomer and the structural units derived from the aromatic monomer (C5 ratio) is, for example, higher than 50% by mass, preferably higher than 60% by mass, for example, lower than 80% by mass, preferably lower than 70% by mass.
[0064] When the C5 ratio is greater than the lower limit, it is possible to ensure adhesion of the resin layer 2 to the reinforcement object P. When the C5 ratio is less than or equal to the upper limit, it is possible to ensure strength of the reinforcing member 11 described later.
[0065] The C5 ratio can be measured by nuclear magnetic resonance spectroscopy ( 1 H-NMR) was used for determination.
[0066] The mixing ratio of the tackifier resin relative to 100 parts by mass of the thermosetting resin is, for example, 20 parts by mass or more, preferably 40 parts by mass or more, for example, 70 parts by mass or less, preferably 60 parts by mass or less.
[0067] The blending ratio of the tackifier resin is, for example, 50 parts by mass or more, preferably 80 parts by mass or more, and for example, 200 parts by mass or less, preferably 150 parts by mass or less, based on 100 parts by mass of the diene rubber.
[0068] (1-4) Vulcanizing agent
[0069] The vulcanizing agent crosslinks (vulcanizes) the diene rubber by heating.
[0070] Examples of the vulcanizing agent include sulfur, sulfur compounds, and organic peroxides. Preferably, the vulcanizing agent is sulfur.
[0071] The mixing ratio of the vulcanizing agent relative to 100 parts by mass of the thermosetting resin is, for example, 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and for example, 20 parts by mass or less, preferably 15 parts by mass or less.
[0072] The mixing ratio of the vulcanizing agent is, for example, 2 parts by mass or more, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and for example, 80 parts by mass or less, preferably 70 parts by mass or less, more preferably 50 parts by mass or less, based on 100 parts by mass of the diene rubber.
[0073] The blending ratio of the vulcanizing agent is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and more preferably 10 parts by mass or more, relative to 100 parts by mass of the total of the diene rubber and the tackifier resin.
[0074] When the mixing ratio of the vulcanizing agent is not less than the above lower limit, the double bonds of the tackifier can be crosslinked by vulcanization of the diene rubber, and the strength of the reinforcing member 11 can be improved.
[0075] The mixing ratio of the vulcanizing agent is, for example, 40 parts by mass or less, or preferably 30 parts by mass or less, relative to 100 parts by mass of the total of the diene rubber and the tackifier resin.
[0076] When the mixing ratio of the vulcanizing agent is equal to or less than the above upper limit, the strength of the reinforcing member 11 can be improved with a small amount of the vulcanizing agent.
[0077] (1-5) Vulcanization accelerator
[0078] Vulcanization accelerators accelerate vulcanization based on vulcanizing agents.
[0079] Examples of the vulcanization accelerator include thiazole vulcanization accelerators, thiourea vulcanization accelerators, thiuram vulcanization accelerators, dithiocarbamate vulcanization accelerators, guanidine vulcanization accelerators, aldehyde-ammonia vulcanization accelerators, and sulfenamide vulcanization accelerators. Preferred examples of the vulcanization accelerator include thiazole vulcanization accelerators.
[0080] The mixing ratio of the vulcanization accelerator is, for example, 1 part by mass or more, preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and for example, 10 parts by mass or less, preferably 8 parts by mass or less, based on 100 parts by mass of the thermosetting resin.
[0081] The mixing ratio of the vulcanization accelerator is, for example, 10 parts by mass or more, preferably 30 parts by mass or more, and for example, 100 parts by mass or less, preferably 70 parts by mass or less, based on 100 parts by mass of the vulcanizing agent.
[0082] (1-6) Thermosetting resin curing agent
[0083] Thermosetting resin curing agents accelerate the curing of thermosetting resins.
[0084] Examples of the thermosetting resin curing agent include cyanamide, amine, acid anhydride, amide, hydrazide, imidazole, and imidazoline.
[0085] Examples of cyanamide include dicyandiamide.
[0086] Examples of the amine include ethylenediamine, propylenediamine, diethylenetriamine, triethylenetetramine, amine adducts thereof, metaphenylenediamine, diaminodiphenylmethane, and diaminodiphenyl sulfone.
[0087] Examples of the acid anhydride include phthalic anhydride, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylnadic anhydride, pyromellitic anhydride, dodecenylsuccinic anhydride, dichlorosuccinic anhydride, benzophenonetetracarboxylic anhydride, and chlorendic anhydride.
[0088] Examples of the amide include polyamide and the like.
[0089] Examples of the hydrazide include dihydrazide and the like.
[0090] Examples of the imidazole include methylimidazole, 2-ethyl-4-methylimidazole, ethylimidazole, isopropylimidazole, 2,4-dimethylimidazole, phenylimidazole, undecylimidazole, heptadecylimidazole, and 2-phenyl-4-methylimidazole.
[0091] Examples of the imidazoline include methylimidazoline, 2-ethyl-4-methylimidazoline, ethylimidazoline, isopropylimidazoline, 2,4-dimethylimidazoline, phenylimidazoline, undecylimidazoline, heptadecylimidazoline, and 2-phenyl-4-methylimidazoline.
[0092] The mixing ratio of the thermosetting resin curing agent is, for example, 1 part by mass or more, preferably 2 parts by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, based on 100 parts by mass of the thermosetting resin.
[0093] (1-7) Foaming agent
[0094] The foaming agent foams by heating. When the resin layer 2 contains the foaming agent, the thickness of the reinforcing layer 5 described later can be increased, and the strength of the reinforcing member 11 can be improved.
[0095] Examples of the foaming agent include inorganic foaming agents and organic foaming agents.
[0096] Examples of the inorganic foaming agent include ammonium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and azides.
[0097] Examples of the organic foaming agent include N-nitroso compounds such as N,N'-dinitrosopentamethylenetetramine, azo compounds such as azobisisobutyronitrile, fluorinated alkanes such as trichloromonofluoromethane, hydrazine compounds such as 4,4'-oxybis(benzenesulfonylhydrazide) and allylbis(sulfonylhydrazide), semicarbazide compounds such as p-toluenesulfonylsemicarbazide, triazole compounds such as 5-morpholinyl-1,2,3,4-thiatriazole, etc. Preferably, 4,4'-oxybis(benzenesulfonylhydrazide) (OBSH) is used.
[0098] The mixing ratio of the foaming agent is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and for example, 20 parts by mass or less, preferably 5 parts by mass or less, based on 100 parts by mass of the thermosetting resin.
[0099] The blending ratio of the foaming agent is, for example, 0.2 parts by mass or more, preferably 1 part by mass or more, and for example, 40 parts by mass or less, preferably 10 parts by mass or less, based on 100 parts by mass of the total of the thermosetting resin, the diene rubber and the tackifier resin.
[0100] (2) Constraint layer 3
[0101] The constraining layer 3 is disposed on the first surface S1 of the resin layer 2. The constraining layer 3 constrains the reinforcing layer 5 described later. The constraining layer 3 constrains the reinforcing layer 5, thereby improving the toughness of the reinforcing layer 5. The constraining layer 3 has a predetermined thickness in the thickness direction of the resin layer 2.
[0102] The thickness of the constrained layer 3 is, for example, not less than 0.01 mm, preferably not less than 0.05 mm, and for example, not more than 3 mm, preferably not more than 1 mm.
[0103] As a material of the constraining layer 3, metal, glass fiber, etc. can be cited, for example. As a metal, aluminum, copper, etc. can be cited, as a metal, aluminum can be cited preferably, and as a glass fiber, resin-impregnated glass fiber cloth can be cited preferably.
[0104] (3) Release sheet 4
[0105] The release sheet 4 is disposed on the second surface S2 of the resin layer 2. The release sheet 4 protects the resin layer 2 while being disposed on the second surface S2 of the resin layer 2. The release sheet 4 can be peeled from the resin layer 2. As the release sheet 4, for example, a known release paper or the like can be used.
[0106] 2. Enhancement Methods
[0107] Next, a method of reinforcing the reinforcement object P using the reinforcing material 1 will be described.
[0108] like Figure 2A and Figure 2B As shown, the reinforcement method includes a step of attaching the reinforcement material 1 to the reinforcement object P (see Figure 2A ), and a curing step of thermally curing the resin layer 2 while the reinforcing material 1 is attached to the reinforcement object P (see Figure 2B ).
[0109] like Figure 2A As shown, in the attaching step, the operator peels the release sheet 4 from the resin layer 2 to bring the second surface S2 of the resin layer 2 into contact with the reinforcement object P. The reinforcing material 1 is attached to the reinforcement object P by the adhesive force of the resin layer 2 .
[0110] Next, in the curing step, the operator heats the reinforcement object P to which the reinforcing material 1 is attached.
[0111] The heating temperature is, for example, 140° C. or higher, preferably 160° C. or higher, and, for example, 220° C. or lower, preferably 200° C. or lower.
[0112] The heating time is, for example, 5 minutes or more, preferably 10 minutes or more, and, for example, 60 minutes or less, preferably 30 minutes or less.
[0113] During the curing process, Figure 2A and Figure 2B As shown, the resin layer 2 is cured. It should be noted that, when the resin layer 2 contains a foaming agent, the resin layer 2 is foamed and cured. The reinforcing layer 5 is formed by curing the resin layer 2. That is, the reinforcing layer 5 is composed of the cured product of the resin layer 2. The reinforcing layer 5 is fixed to the reinforcement object P.
[0114] When the resin layer 2 contains a foaming agent, the foaming ratio (thickness of the reinforcing layer 5 / thickness of the resin layer 2 ) is, for example, 2 times or more, preferably 3 times or more, for example, 10 times or less.
[0115] The curing process is completed, so that Figure 2B As shown, a reinforcement structure 10 including a reinforcement object P and a reinforcement member 11 is formed. The reinforcement member 11 includes a reinforcement layer 5 and a constraining layer 3. The reinforcement member 11 reinforces the reinforcement object P. The reinforcement layer 5 is arranged on the reinforcement object P. The constraining layer 3 is arranged on the reinforcement layer 5. The constraining layer 3 is arranged on the opposite side of the reinforcement object P relative to the reinforcement layer 5 in the thickness direction of the reinforcement layer 5.
[0116] 3. Effect
[0117] According to the reinforcing material 1, Figure 1 The resin layer 2 shown contains a tackifying resin having a specific softening temperature and a specific bromine value.
[0118] Therefore, the adhesive force of the resin layer 2 can be ensured while improving the strength of the reinforcing member 11 (the reinforcing material 1 in which the resin layer 2 is cured, see Figure 2B This is believed to be because the unsaturated bonds in the tackifying resin react during the curing process to form a cross-linked structure.
[0119] As a result, the reinforcement performance of the reinforcing material 1 can be improved.
[0120] Example
[0121] Next, the present invention is described based on examples and comparative examples. The present invention is not limited by the following examples. In addition, the specific numerical values of the physical property values, parameters, etc. used in the following descriptions can be replaced by the upper limit values (defined as the numerical value "below") or lower limit values (defined as the numerical value "above") of the physical property values, parameters, etc. corresponding to them recorded in the above-mentioned "Specific Implementation Methods".
[0122] 1. Preparation of resin layer
[0123] Example 1
[0124] The following materials (1) to (8) were mixed to prepare a resin composition.
[0125] The obtained resin composition was rolled into a thickness of 1.0 mm using a press forming machine to prepare a resin layer. A resin-impregnated glass fiber cloth with a thickness of 0.2 mm was pasted on one side of the obtained resin layer as a restraining layer, and a release paper was pasted on the other side of the resin layer (the surface opposite to the one side). Thus, a reinforcing material was obtained.
[0126] Table 1 shows the softening temperature, bromine value, weight average molecular weight, and C5 ratio of the tackifier resin.
[0127] The bromine value is determined by the following method. First, 10 ml of hexane is added to a specified amount of tackifying resin to prepare a hexane solution of the tackifying resin. Next, a certain excess of a potassium bromide-potassium bromate mixture is added to the solution under the acidity of acetic acid. Thus, bromine is added to the tackifying resin. Next, a potassium iodide solution is added. Next, the free iodine is titrated with sodium thiosulfate, and the mass of bromine added per 100 g of tackifying resin (bromine value) is calculated.
[0128] (1) Thermosetting resin
[0129] Flexible epoxy resin (dimer acid-modified epoxy resin, epoxy equivalent 600-700 g / eq, manufactured by Mitsubishi Chemical Corporation, "jER872") 70 parts by mass
[0130] 30 parts by mass of hydrogenated bisphenol A epoxy resin (epoxy equivalent 215 g / eq, manufactured by ADEKA Corporation, “EP-4080E”)
[0131] (2) Diene rubber
[0132] Polybutadiene diene rubber (manufactured by Asahi Kasei Chemicals Co., Ltd., "Tufden 2003") 40 parts by mass
[0133] Acrylonitrile butadiene diene rubber (Nipol 1052J, manufactured by Nippon Zeon Co., Ltd.) 10 parts by mass
[0134] (3) Tackifying resin
[0135] Aliphatic aromatic copolymer petroleum resin (manufactured by Tosoh Corporation, "PETROTAC 90HM") 50 parts by mass
[0136] In addition, "PETROTAC 90HM" is described as "90HM" in Table 1.
[0137] (4) Vulcanizing agent
[0138] Sulfur 12 parts by mass (manufactured by Tsurumi Chemical Industry Co., Ltd., "Kinhua Printing Micro Powder Sulfur")
[0139] (5) Vulcanization accelerator
[0140] Thiazole vulcanization accelerator 6 parts by mass ("NOCCELER DM" manufactured by Ouchi Shinko Chemical Co., Ltd.)
[0141] (6) Thermosetting resin curing agent
[0142] Dicyandiamide (manufactured by Nippon Carbon Industries) 3 parts by mass
[0143] (7) Foaming agent
[0144] 2.5 parts by mass of 4,4'-oxybis(benzenesulfonylhydrazide) (OBSH) (manufactured by Eiwa Chemical Industry Co., Ltd., "Neocellborn N#1000S")
[0145] (8) Filling materials
[0146] 50 parts by mass of heavy calcium carbonate (manufactured by Maruo Calcium Co., Ltd.)
[0147] Examples 2, 3, and Comparative Examples 1 to 3
[0148] A reinforcing material was obtained in the same manner as in Example 1 except that the tackifier resin was changed to the tackifier resin described in Table 1.
[0149] It should be noted that in Table 1, "100V" is PETROTAC 100V (aliphatic aromatic copolymer petroleum resin, manufactured by Tosoh Corporation), "90" is PETROTAC 90 (aliphatic aromatic copolymer petroleum resin, manufactured by Tosoh Corporation), "60" is PETROTAC 60 (aliphatic aromatic copolymer petroleum resin, manufactured by Tosoh Corporation), "T1080" is HIKOREZ T-1080 (aliphatic aromatic copolymer petroleum resin, manufactured by Kolon Corporation), and "G115" is Quintone G115 (aliphatic aromatic copolymer petroleum resin, manufactured by Nippon Zeon Co., Ltd.).
[0150] 2. Determination of the adhesion of the resin layer
[0151] A strip-shaped test piece was cut out from the reinforcing material of each embodiment and each comparative example. The width of the test piece (the length in the direction orthogonal to the length direction of the test piece) was 25 mm. The release paper was peeled off from the test piece and pressed onto the steel plate using a 2 kg roller at 5 ° C. After the test piece was pressed onto the steel plate for 30 minutes, the adhesion (N / 25 mm) was measured by a 90 ° peel test (tensile speed 300 mm / min) using a tensile compression tester TG-5KN (manufactured by Minebea Mitsumi) at 5 ° C. The results are shown in Table 1.
[0152] 3. Determination of the breaking strength of reinforced components
[0153] The reinforcing materials of each example and each comparative example were peeled off the release paper and attached to the entire surface of a cold-rolled steel plate (SPCC-SD manufactured by Nippon Testpanel Co., Ltd., width: 25 mm, length: 150 mm, thickness: 0.8 mm) to be reinforced in an atmosphere of 20°C.
[0154] Next, the steel plate with the reinforcement material attached was heated at 180° C. for 20 minutes. The resin layer was thereby foamed and cured, thereby obtaining a test piece having a steel plate and a reinforcement member (a reinforcement member having a reinforcement layer which is a cured product of the resin layer and a restraining layer).
[0155] Then, the fracture strength of the reinforcement member was measured using a tensile compression tester TG-5KN (manufactured by Minebea Mitsumi Co., Ltd.) Specifically, the test piece was supported on the tester at intervals of 100 mm with the steel plate facing upward, and a test rod was lowered from above at a speed of 1 mm / min relative to the center of the length direction of the test piece.
[0156] The bending strength (N) when the reinforcing member was broken after the test rod was in contact with the steel plate was the breaking strength.
[0157] [Table 1]
[0158] Table 1
[0159]
[0160] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but this is merely an illustration and is not to be construed as limiting. Modifications of the present invention that are obvious to those skilled in the art are included in the technical solutions described below.
[0161] Industrial Applicability
[0162] The reinforcing material and the reinforcing structure of the present invention are used, for example, to reinforce metal plates used in transportation equipment such as automobiles, railway vehicles, ships, and aircraft, and in buildings.
[0163] Description of Reference Numerals
[0164] 1: Reinforcement Materials
[0165] 2: Resin layer
[0166] 3: Constraint layer
[0167] 5: Enhancement layer
[0168] 10: Enhanced structure
[0169] 11: Enhanced components
[0170] P: Enhanced object
Claims
1. A reinforcing material, characterized in that: have: a resin layer comprising a thermosetting resin, a diene rubber, a tackifying resin and a vulcanizing agent; and a constraining layer disposed on the resin layer, The thermosetting resin contains a flexible epoxy resin having an epoxy equivalent of 300 g / eq or more and 1200 g / eq or less. The mixing ratio of the tackifier resin is 20 parts by weight or more and 60 parts by weight or less relative to 100 parts by weight of the thermosetting resin. The softening temperature of the tackifying resin is 75° C. or higher and 100° C. or lower. The bromine value of the tackifying resin is greater than 30 gBr2 / 100 g.
2. The reinforcing material according to claim 1, characterized in that The tackifying resin is an aliphatic-aromatic copolymer petroleum resin containing structural units derived from aliphatic monomers and structural units derived from aromatic monomers. The ratio of the structural unit derived from the aliphatic monomer to the total of the structural unit derived from the aliphatic monomer and the structural unit derived from the aromatic monomer is higher than 50% by mass.
3. The reinforcing material according to claim 1, characterized in that The thermosetting resin contains 60 parts by mass or more of the flexible epoxy resin in 100 parts by mass of the thermosetting resin.
4. A reinforcement structure, characterized in that: A reinforcement object and a reinforcement component for reinforcing the reinforcement object are provided. The reinforcing member comprises: a reinforcing layer formed of a cured product of the resin layer of the reinforcing material according to claim 1, wherein the reinforcing layer is arranged on the reinforcing object, The constrained layer of the reinforcing material according to claim 1, which is arranged on the reinforcing layer.