A preparation process of nano-zirconia powder
By controlling the addition rate of zirconium ion and ammonium ion concentration in the liquid phase method, the problem of large particle size and many impurities of nano-zirconia powder is solved, the uniformity of nano-zirconia particle size and low impurities are achieved, and the calcination temperature is reduced. and energy consumption.
Patent Information
- Application Number
- CN202210313007.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-28
AI Technical Summary
When preparing nano-zirconia powder by the liquid phase method, agglomeration is easy to occur, the particle size is too large, and the impurity content is difficult to reduce.
By preparing the precipitant solution and zirconium salt solution and adding them to the mother liquor at the same time, heating and stirring, the concentration of zirconium ions, ammonium ions and ammonia water, as well as the addition rate, are controlled to avoid agglomeration and control the particle size of nano-zirconium oxide at 33-48nm. .
It effectively avoids the problems of unstable nano-zirconia particle size and high impurity content, achieves uniformity of nano-zirconia particle size and low impurities, and reduces the calcination temperature and energy consumption.
Abstract
Description
Technical Field
[0001] The invention relates to a process for preparing nano-level zirconium oxide powder, and belongs to the field of zirconium oxide powder preparation. Background Art
[0002] Nano-zirconia powder has the characteristics of large specific surface area, high surface energy, low sintering temperature, and excellent mechanical, thermal, electrical and optical properties. Therefore, it is widely used in high-temperature structural materials, high-temperature optical components, oxygen sensors, fuel cells, etc.
[0003] The preparation methods of zirconia ultrafine powder include wet chemical method, hydrothermal method, sol-gel method, etc. The main method for preparing nano zirconia powder is liquid phase method. The liquid phase method has a simple preparation process and small equipment investment. However, agglomeration is prone to occur during the preparation process using the liquid phase method, and the particle size of the obtained nano zirconia powder is relatively large. In addition, the content of ionic impurities in the nano zirconia powder is not easy to reduce.
[0004] Therefore, how to reduce the particle size and impurities of nano zirconium oxide powder prepared by liquid phase method has become a technical problem in this field. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a process for preparing nano-scale zirconium oxide powder, comprising the following steps: preparing a precipitant solution, a zirconium salt solution, and a mother liquor; heating the mother liquor, and maintaining the mother liquor at a first temperature; adding the precipitant solution and the zirconium salt solution to the mother liquor at the same time, stirring during the adding process, during which the flow rate of the zirconium salt solution is v1, and the flow rate of the precipitant solution is v2; achieving a small particle size of nano-zirconium oxide prepared by a liquid phase method, with a particle size of 33-48nm.
[0006] According to one aspect of the present invention, a process for preparing nano-scale zirconium oxide powder comprises the following steps: preparing a precipitant solution, a zirconium salt solution, and a mother liquor; heating the mother liquor to a first temperature; adding the precipitant solution and the zirconium salt solution to the mother liquor at the same time, stirring during the adding process, and the flow rate of the zirconium salt solution during the process is v1 m 3 / h, the flow rate of the precipitant solution is v2 m 3 / h; continue to stir at a constant temperature after the addition is completed; then filter, wash, and dry; after drying, calcine to obtain the nano zirconium oxide particle size of 33-48nm;
[0007] The zirconium ion concentration in the zirconium salt solution is a mol / L, where a is 0.5-2.5;
[0008] The mother liquor includes ammonium ions and / or ammonia water, the sum of the concentrations of ammonium ions and ammonia water in the mother liquor is b mol / L, and b is 0.2-2; the sum of the concentrations of ammonium ions and ammonia water in the mother liquor is b, that is, when there are only ammonium ions or ammonia water in the mother liquor, b is the concentration of ammonium ions or ammonia water; when there are only ammonium ions and ammonia water in the mother liquor, b is the sum of the concentrations of ammonium ions and ammonia water.
[0009] The beneficial effects of the present invention over the prior art are that, by adding the precipitant solution and the zirconium salt solution to the mother liquor at the same time, zirconium ions can react slowly to generate zirconium hydroxide without generating zirconium hydroxide gel or agglomeration, and the obtained zirconium hydroxide powder has small particles; by including ammonium ions and / or ammonia water in the mother liquor, the rate of the reaction of zirconium ions to generate zirconium hydroxide can be effectively controlled;
[0010] By controlling the zirconium ion concentration in the zirconium salt solution, the concentration of ammonium ions and ammonia water in the mother liquor, and the rate of zirconium ion addition, the ratio of the added zirconium ions to the ammonium ions and ammonia water in the mother liquor can be stably controlled within a certain range during the reaction time when the zirconium ions are added to the mother liquor, thereby achieving continuous and stable generation of nano-scale zirconium hydroxide with small particles, avoiding the instability of the nano zirconium hydroxide particle size, and achieving the nano zirconium oxide particle size of 33-48nm; and after the zirconium hydroxide is generated, the ion concentration in the solution is low, which is conducive to achieving less impurities in the obtained nano zirconium oxide.
[0011] Furthermore, the precipitant solution includes one or more of ammonia water and urea, the concentration of the solute in the precipitant solution is c mol / L, and c is 0.3-1.5.
[0012] The beneficial effect of adopting the technical solution in the previous step is that the precipitant solution includes one or more of ammonia water, urea, and ammonia gas, so as to supplement the ammonium ions and / or ammonia water in the mother liquor, control the supplement rate of the ammonium ions and / or ammonia water, and achieve the concentration and stability of the ammonium ions and ammonia water in the mother liquor within a certain range with small fluctuations; the precipitant concentration c is 0.3-1.5 mol / L, which can achieve stable supplementation of the concentration of ammonium ions and ammonia water in the mother liquor, which is beneficial to achieve the concentration and stability of ammonium ions and ammonia water in the mother liquor, and is also beneficial to avoid the problem of high ion concentration in the solution after the zirconium hydroxide is generated.
[0013] Furthermore, the v1 m 3 / h is 0.5-2; and / or v2 m 3 / h is 0.1-1.2;
[0014] Furthermore, the first temperature is 60-80°C.
[0015] The beneficial effect of adopting the above technical solution is that it is conducive to achieving continuous generation of zirconium hydroxide precipitation in the mother liquor.
[0016] Furthermore, the calcination temperature is 450-540° C., and the calcination time is 3-5 hours.
[0017] The beneficial effect of adopting the technical solution in the previous step is that since the zirconium hydroxide particles obtained by the reaction are small and dispersed, agglomeration is avoided. Therefore, the calcination temperature is 450-540°C, which not only achieves the purpose of obtaining zirconium oxide, but also reduces energy consumption and avoids the phenomenon of increasing adhesion of some zirconium oxide particles after sintering due to uneven zirconium hydroxide particle size at high temperature.
[0018] Furthermore, the process for preparing nano-scale zirconium oxide powder includes controlling a process parameter x, wherein x=a﹒v1 / b.
[0019] The beneficial effect of adopting the technical solution in the previous step is that by controlling the process parameter x, a continuous and stable reaction in the mother liquor is achieved to generate small nano zirconium hydroxide particles, and the obtained nano zirconium hydroxide particles are uniform in size; thereby finally obtaining small and uniform nano zirconium oxide particles.
[0020] Furthermore, the process parameter x is 0.25-0.35.
[0021] The beneficial effect of adopting the technical solution in the previous step is that the parameter x is in the range of 0.25-0.35, which not only avoids the occurrence of zirconium hydroxide gel phenomenon or low output efficiency of nano zirconium hydroxide when zirconium ions enter the mother liquor for reaction, but also avoids the large particles of nano zirconium hydroxide precipitate produced by the reaction or the agglomeration phenomenon, and more effectively controls and realizes the continuous and stable reaction in the mother liquor to generate small nano zirconium hydroxide particles, so that the final nano zirconium hydroxide particles are small and uniform in size.
[0022] Further, it includes controlling the process parameter y, wherein = a / c.
[0023] The beneficial effect of adopting the technical solution in the previous step is that, by controlling the process parameter y, the ratio of the zirconium ion concentration a in the zirconium salt solution to the solute concentration c in the precipitant solution can be achieved, which is beneficial to achieving the concentration and stability of ammonium ions and ammonia water in the mother liquor during the reaction, and avoiding the occurrence of zirconium hydroxide precipitation or zirconium hydroxide gel when zirconium ions continuously react to generate zirconium hydroxide, and is also beneficial to reducing the ion concentration in the solution after the generation of zirconium hydroxide.
[0024] Furthermore, the process parameter y is 1-1.5.
[0025] The beneficial effect of adopting the technical solution in the previous step is that the process parameter y is controlled to be 1-1.5, which avoids the problem that the nano zirconium hydroxide precipitate particles produced by the reaction are large and agglomerate when y is less than 1, and avoids the problem of high ion content in the solution after the zirconium hydroxide is generated; it also avoids the problem of zirconium hydroxide gel phenomenon or low production efficiency when y is greater than 1; thereby effectively achieving high efficiency in generating nano zirconium hydroxide by reaction, without large nano zirconium hydroxide precipitate particles or agglomeration, and without high ion concentration in the solution during the reaction, and finally achieving small nano zirconium oxide particles, less impurities, and high production efficiency.
[0026] Furthermore, the precipitant solution and the zirconium salt solution are added to the mother liquor at the same time, the intersection point of the extended line of the liquid outlet of the precipitant solution adding device and the mother liquor surface is point e, and the intersection point of the extended line of the liquid outlet of the zirconium salt solution adding device and the mother liquor surface is point f; the horizontal distance between point e and point f is L, and L is 0-1.5m, preferably L is 0-1m.
[0027] The beneficial effect of adopting the above technical solution is that by controlling L to be 0-1.5 m, when the process parameters x and y are within the above range, the concentration of ammonium ions and ammonia water in the mother liquor can be further effectively stabilized, thereby achieving the stability of the size of the nano zirconium hydroxide particles generated in the reaction. DETAILED DESCRIPTION
[0028] In order to better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments.
[0029] Embodiment 1:
[0030] This embodiment provides a process for preparing nano-scale zirconium oxide powder, comprising the following steps: preparing a precipitant solution, a zirconium salt solution, and a mother solution;
[0031] The mother liquid is heated to maintain a temperature of the mother liquid at a first temperature, wherein the first temperature is specifically 70° C.;
[0032] Add a certain amount of mother liquid to the container, the specific amount is 2m 3 ;
[0033] Adding the precipitant solution and the zirconium salt solution to the mother liquor simultaneously, stirring during the adding process, wherein the flow rate of the zirconium salt solution is v1, and the flow rate of the precipitant solution is v2;
[0034] After the addition is completed, the stirring is continued at a constant temperature, and specifically, the stirring is continued at a constant temperature for 1 hour after the addition is completed; then, the process is filtered, washed, and dried; after drying, the process is calcined to obtain the nano zirconium oxide with a particle size of 35 nm; specifically, the washed zirconium hydroxide slurry is spray dried to obtain zirconium hydroxide powder; specifically, the calcination temperature is 480°C, and the calcination time is 4 hours.
[0035] The zirconium ion concentration in the zirconium salt solution is a mol / L, where a is 0.5-2.5; the specific zirconium salt solution is a zirconium nitrate solution, where the zirconium ion concentration a in the zirconium nitrate solution is 1 mol / L;
[0036] The mother liquor includes ammonium ions, the ammonium ions in the mother liquor are b mol / L, and b is 0.2-2; the specific mother liquor is ammonium nitrate solution, and the ammonium ion concentration b in the mother liquor is 1.9375 mol / L;
[0037] The precipitant solution includes ammonia water, the concentration of the solute in the precipitant solution is c mol / L, and c is 0.5-1.5; specifically, the precipitant solution is ammonia water, and the concentration c of the ammonia water in the precipitant solution is 0.8 mol / L;
[0038] The v1 m 3 / h is 0.5-2, and the specific flow rate of the zirconium nitrate solution is 0.6m 3 / h;
[0039] The v2 m 3 / h is 0.1-1.2, and the specific flow rate of the precipitant ammonia water is 0.318m 3 / h;
[0040] The nano-scale zirconium oxide powder preparation process also includes controlling a process parameter x, wherein x=a﹒v1 / b; the process parameter x is specifically 0.31; this not only avoids the occurrence of zirconium hydroxide gel phenomenon or low nano zirconium hydroxide output efficiency when zirconium ions enter the mother liquor for reaction, but also avoids the large particles of nano zirconium hydroxide precipitates or agglomeration phenomenon produced by the reaction, and more effectively controls and realizes the continuous and stable reaction in the mother liquor to generate nano zirconium hydroxide particles with small particles, thereby achieving the final nano zirconium hydroxide particles with small size and uniform size;
[0041] The nano-scale zirconium oxide powder preparation process also includes controlling a process parameter y, wherein y=a / c; the process parameter y is specifically 1.25; it can achieve the ratio of the zirconium ion concentration a in the zirconium salt solution to the solute concentration c in the precipitant solution, which is beneficial to achieving the stability of the concentration of ammonium ions and ammonia water in the mother liquor during the reaction, and avoids the phenomenon of zirconium hydroxide precipitation or zirconium hydroxide gel when zirconium ions react continuously to generate zirconium hydroxide, and is also beneficial to reducing the ion concentration in the solution after the zirconium hydroxide is generated;
[0042] The ammonia solution and zirconium nitrate solution are added to the mother liquor at the same time, the intersection point between the extended line of the ammonia solution adding device outlet and the mother liquor surface is point e, and the intersection point between the extended line of the zirconium nitrate solution adding device outlet and the mother liquor surface is point f;
[0043] The horizontal distance between point e and point f is L, and L is 0.5 m. When the process parameters x and y are within the range, the concentration of ammonium ions and ammonia water in the mother liquor can be further effectively stabilized, thereby achieving a stable size of the nano zirconium hydroxide particles generated in the reaction.
[0044] Embodiment 2:
[0045] The same parts as those of the first embodiment are not described in detail. The present embodiment provides a process for preparing nano-scale zirconium oxide powder, comprising the following steps: preparing a precipitant solution, a zirconium salt solution, and a mother liquor;
[0046] The mother liquid is heated to maintain a temperature of the mother liquid at a first temperature, wherein the first temperature is specifically 75° C.;
[0047] Add a certain amount of mother liquid to the container, the specific amount is 0.7m 3 ;
[0048] Specifically, the calcination temperature is 500° C. and the calcination time is 3.8 h.
[0049] The specific zirconium salt solution is a zirconium chloride solution, wherein the zirconium ion concentration a in the zirconium chloride solution is 0.77 mol / L;
[0050] The specific mother liquor is an ammonium nitrate solution, and the ammonium ion concentration b in the mother liquor is 1.3 mol / L;
[0051] Specifically, the precipitant solution includes ammonia water and urea, and the concentration of ammonia water and urea in the precipitant solution is 0.55 mol / L;
[0052] Specifically, the flow rate v1 of the zirconium nitrate solution is 0.55 m 3 / h;
[0053] Specifically, the precipitant ammonia water flow rate v2 is 0.297m 3 / h;
[0054] The process parameter x is specifically 0.33;
[0055] The process parameter y is specifically 1.4;
[0056] The ammonia solution and zirconium nitrate solution are added to the mother liquor at the same time, the intersection point between the extended line of the ammonia solution adding device outlet and the mother liquor surface is point e, and the intersection point between the extended line of the zirconium nitrate solution adding device outlet and the mother liquor surface is point f;
[0057] The horizontal distance between point e and point f is L, and L is 0.3 m;
[0058] The final particle size of the nano zirconium oxide is 40 nm.
[0059] Embodiment three:
[0060] The same parts as those of the first embodiment are not described in detail. The present embodiment provides a process for preparing nano-scale zirconium oxide powder, comprising the following steps: preparing a precipitant solution, a zirconium salt solution, and a mother liquor;
[0061] The mother liquid is heated to maintain a temperature of the mother liquid at a first temperature, wherein the first temperature is specifically 65° C.;
[0062] Add a certain amount of mother liquid to the container, the specific amount is 1m 3 ;
[0063] Specifically, the calcination temperature is 460° C. and the calcination time is 4.5 h.
[0064] The specific zirconium salt solution is a zirconium chloride solution, wherein the zirconium ion concentration a in the zirconium chloride solution is 0.6 mol / L;
[0065] The specific mother liquor is an ammonium nitrate solution, and the ammonium ion concentration b in the mother liquor is 1.62 mol / L;
[0066] The precipitant solution includes aqueous ammonia,
[0067] Specifically, the precipitant solution includes ammonia water and urea, and the concentration c of ammonia water and urea in the precipitant solution is 0.414 mol / L;
[0068] Specifically, the flow rate v1 of the zirconium nitrate solution is 0.7 m 3 / h;
[0069] Specifically, the precipitant ammonia water flow rate v2 is 0.43m 3 / h;
[0070] The process parameter x is specifically 0.26;
[0071] The process parameter y is specifically 1.45;
[0072] The ammonia solution and zirconium nitrate solution are added to the mother liquor at the same time, the intersection point between the extended line of the ammonia solution adding device outlet and the mother liquor surface is point e, and the intersection point between the extended line of the zirconium nitrate solution adding device outlet and the mother liquor surface is point f;
[0073] The horizontal distance between point e and point f is L, and L is 0.25m;
[0074] Finally, the nano zirconium oxide particle size is 35nm. The above description is only a preferred embodiment of the present application and an explanation of the technical principle used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but also should cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features have similar functions to those disclosed in this application (but not limited to).
Claims
1. A process for preparing nano-scale zirconium oxide powder, characterized in that: The following steps are involved: Prepare precipitant solution, zirconium salt solution and mother liquor; Heating the mother liquor to a first temperature; Add the precipitant solution and the zirconium salt solution to the mother liquor simultaneously, stirring during the adding process, wherein the flow rate of the zirconium salt solution is v1 m³ / h, and the flow rate of the precipitant solution is v2 m³ / h; After the addition is complete, continue stirring at constant temperature; Then filter, wash and dry; After drying, calcination is performed to obtain the product; The zirconium ion concentration in the zirconium salt solution is a mol / L, where a is 0.5-2.5; The mother liquor comprises ammonium ions and / or ammonia water, the sum of the concentrations of ammonium ions and ammonia water in the mother liquor is b mol / L, and b is 0.2-2; Including controlling the process parameter x, wherein x=a﹒v1 / b; the process parameter x is 0.25-0.35; The precipitant solution and the zirconium salt solution are added to the mother liquor at the same time, the intersection point of the extended line of the liquid outlet of the precipitant solution adding device and the liquid surface of the mother liquor is point e, and the intersection point of the extended line of the liquid outlet of the zirconium salt solution adding device and the liquid surface of the mother liquor is point f; The horizontal distance between point e and point f is L, and L is 0-1.5 m.
2. A process for preparing nano-scale zirconium oxide powder according to claim 1, characterized in that: The precipitant solution includes one or more of ammonia water and urea, the concentration of the solute in the precipitant solution is c mol / L, and c is 0.3-1.
5.
3. A process for preparing nano-scale zirconium oxide powder according to claim 1, characterized in that: The v1 is 0.5-2; and / or The v2 is 0.1-1.
2.
4. A process for preparing nano-scale zirconium oxide powder according to claim 1, characterized in that: The first temperature is 60-80°C.
5. A process for preparing nano-scale zirconium oxide powder according to claim 1, characterized in that: The calcination temperature is 450-540° C., and the calcination time is 3-5 hours.
6. A process for preparing nano-scale zirconium oxide powder according to claim 2, characterized in that: Including controlling process parameter y, wherein y=a / c; The process parameter y is 1-1.5.