A method for manufacturing 2GPa ultra-high strength martensitic die steel
By optimizing process parameters through laser selective melting and heat treatment technology, the problems of difficult processing and insufficient performance of ultra-high-strength martensitic mold steel have been solved, and the manufacturing of 2GPa-grade mold steel has been achieved, significantly improving the mechanical properties and hardness.
Patent Information
- Application Number
- CN202210606837.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When manufacturing molds using traditional methods, ultra-high-strength martensitic steel has poor quenching permeability and is difficult to process. Existing additive manufacturing processes cannot effectively improve mold performance to 2 GPa.
Ultra-high-strength martensitic mold steel is prepared using laser selective melting method, combined with solution treatment and aging heat treatment, and process parameters such as scanning spacing, laser power and heat treatment temperature are optimized to form a fine full martensitic lath structure.
The mechanical properties of mold steel are significantly improved, the yield strength and tensile strength are significantly improved, and the hardness value is increased by more than 82%, achieving the manufacturing of 2GPa-level ultra-high-strength martensitic mold steel.
Smart Images

Figure CN114918429B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of additive manufacturing engineering, and relates to a method for manufacturing 2GPa-level ultra-high-strength martensitic die steel. Background Art
[0002] Ultra-high strength martensitic steel, with its structure as high-strength martensitic laths, has ultra-high strength, hardness and wear resistance. This makes ultra-high strength martensitic steel have significant advantages in the production and application of conformal cooling water channels, precision injection molds and die-casting molds.
[0003] Moulds are the main processing tools in the fields of machinery manufacturing, aerospace and automobile manufacturing. The quality and performance of moulds directly determine the quality of processed products and production costs. During service, moulds are subjected to great compressive stress, impact force and friction force. Correspondingly, moulds require high strength and hardness to ensure the smooth progress of the production process and the quality of processed products. However, the traditional method of manufacturing moulds requires quenching and tempering heat treatment. The hardenability of the mould is poor and it is easy to crack during the quenching process. During the tempering process, the second strengthening phases such as Ni3(Mo,Ti) and Fe2Mo produced by ultra-high strength martensitic steel lead to ultra-high strength and strength, which increases the difficulty of processing.
[0004] Selective laser melting (SLM), as an advanced manufacturing technology with the characteristics of layer-by-layer accumulation and high cooling rate, has advantages in mold forming. Based on the characteristics of "bottom-up" point-by-point and layer-by-layer production, SLM technology is suitable for the production of molds with complex structures, and can achieve near-net forming of molds, thereby reducing material waste and reducing production costs. In addition, SLM can also achieve rapid molding of molds, thereby shortening the production cycle. Importantly, the SLM printing process has a very high cooling rate, so that the alloy elements of the mold steel are dissolved in large quantities inside, forming a supersaturated solid solubility structure and refining the steel grains. These unique structures are beneficial to improving the strength of the material and can enable the mold to achieve higher performance.
[0005] Although the existing additive manufacturing process methods can complete the rapid prototyping of molds, their performance has not achieved a major breakthrough and has not reached 2GPa. Summary of the invention
[0006] The purpose of the present invention is to solve the problems of difficult processing and insufficient performance of martensitic die steel, and to provide a method for manufacturing 2GPa-level ultra-high-strength martensitic die steel. By optimizing the process parameters to form MS1 ultra-high-strength martensitic die steel, its mechanical properties are greatly improved, and 2GPa-level ultra-high-strength martensitic die steel is obtained.
[0007] The present invention provides a method for manufacturing 2GPa-level ultra-high-strength martensitic die steel, the method comprising the following steps:
[0008] Step 1) preparing an ultra-high strength martensitic die steel workpiece by a laser selective melting method, wherein the scanning interval is 0.07 mm-0.13 mm;
[0009] Step 2) The martensitic die steel workpiece prepared in step 1) is subjected to solution treatment and aging heat treatment in sequence.
[0010] Preferably, in step 1), MS1 ultra-high strength martensitic die steel powder is used as raw material.
[0011] Preferably, the scanning interval in step 1) is 0.07 mm.
[0012] Preferably, the laser power of the laser selective melting method in step 1) is 175W.
[0013] Preferably, the scanning speed of the laser selective melting method in step 1) is 1000 mm / s.
[0014] Preferably, the treatment temperature of the solution treatment in step 2) is 850°C;
[0015] Preferably, the treatment time of the solution treatment in step 2) is 1 h.
[0016] Preferably, the treatment temperature of the aging heat treatment in step 2) is 550°C.
[0017] Preferably, the treatment time of the aging heat treatment in step 2) is 4 hours.
[0018] The present invention has the following beneficial effects:
[0019] The manufacturing method of the 2GPa-level ultra-high-strength martensitic die steel provided by the present invention is suitable for ultra-high-strength martensitic die steel formed by laser selective melting. The present invention preferably combines the optimal process parameters of scanning spacing of 0.07mm-0.13mm, line scanning speed of 1000mm / s, and laser power of 175W and prepares a martensitic die steel workpiece with an ideal macroscopic morphology; after solution and aging heat treatment, the microstructure of the martensitic die steel becomes fine full martensitic laths, and the martensitic laths of different orientations form a certain angle, at this time, the tiny pore defects disappear, and the organization is uniform and dense; the yield strength is increased from 913MPa to 1982MPa, an increase of more than 1 times; the tensile strength is increased from 1186MPa to 2017MPa, an increase of more than 70%; the average Vickers hardness value is increased from 312HV0.3 to 569HV0.3, and the hardness value is increased by more than 82%.
[0020] The present invention achieves the elimination of microscopic defects in SLM forming die steel and uniform and dense structure through optimized SLM process parameters and a suitable heat treatment system, and obtains MS1 ultra-high strength martensitic die steel with excellent performance, laying an important foundation for the subsequent production and use of ultra-high strength martensitic steel die. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The specific embodiments of the present invention can be more fully understood in conjunction with the following drawings, in which:
[0022] Figure 1 It is a cladding morphology image of MS1 ultra-high strength martensitic die steel formed by using different scanning intervals in Examples 1-3 of the present invention;
[0023] Figure 2 is the JMatPro phase diagram of the MS1 ultra-high strength martensitic die steel formed in Example 1 of the present invention;
[0024] Figure 3 This is a SEM image of the MS1 ultra-high strength martensitic die steel formed in Example 1 of the present invention in the printing and heat treatment state. DETAILED DESCRIPTION
[0025] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0026] Embodiment one:
[0027] (1) The material is MS1 ultra-high strength martensitic die steel powder, which is loaded into the powder feeding chamber of the German SLM Solutions 280 3D metal printer.
[0028] (2) The test set the laser power to 175 W, the scanning speed to 1000 mm / s, and the scanning interval to 0.07 mm.
[0029] (3) Two sets of φ30mm×400mm specimens printed on the substrate.
[0030] (4) The sample with the best cladding quality in step (3) is heat treated in a SG-XQL1800 vacuum heat treatment furnace by solution treatment at 850°C for 1 h and aging treatment at 550°C for 4 h.
[0031] Embodiment 2:
[0032] The present embodiment is different from the first embodiment in that the process parameter of the scanning pitch in the laser forming process is changed, specifically, the scanning pitch is set to 0.10 mm, and the rest is the same as the first embodiment.
[0033] Embodiment three:
[0034] The difference between this embodiment and the first embodiment is that the process parameter of the scanning pitch in the laser forming process is changed, specifically: the scanning pitch is set to 0.13 mm, and the rest is the same as the first embodiment.
[0035] Figure 1 The cladding morphology of the MS1 ultra-high strength martensitic die steel formed by Examples 1-3;
[0036] The molded samples of different embodiments were observed and found to be Figure 1 As shown in part (a), when the scanning interval is 0.07 mm, the surface between two adjacent melt tracks is flat and the heights of the two melt tracks are the same;
[0037] like Figure 1 As shown in part (b), when the scanning interval is 0.10 mm, the depression between two adjacent melt paths leads to the formation of porosity defects between the two cladding layers;
[0038] like Figure 1 As shown in part (c), when the scanning spacing is 0.13 mm, the defects of the cladding layer are more obvious, and even large-area depressions appear. Therefore, the smaller the scanning spacing, the better the cladding quality, and the optimal value of the scanning spacing is 0.07 mm.
[0039] Figure 2 is the JMatPro phase diagram of the MS1 ultra-high strength martensitic die steel formed in Example 1, as shown in Figure 2 As shown in the figure, the complete austenitization temperature of MS1 ultra-high strength martensitic die steel is about 800℃, and precipitation phases such as M(C,N) can be efficiently precipitated and have the largest proportion at about 500℃. The main purpose of solid solution is to convert the matrix into austenite structure, but the temperature cannot be too high, otherwise the structure will coarsen. The role of aging is to efficiently generate more precipitation strengthening phases to obtain high strength. Considering the influence of the superheat of the metal material, the heat treatment method with an aging temperature of 850℃ and a solid solution temperature of 500℃ is selected, which can just achieve a finer fully austenitized structure and efficiently generate more precipitation strengthening phases.
[0040] The metallographic samples of the heat-treated and non-heat-treated MS1 ultra-high strength martensitic die steel formed in Example 1 were treated with a 10% nitric acid + 20% hydrochloric acid etchant, and then microstructures were analyzed using a FEI Nova Nano field emission scanning electron microscope (SEM). The SEM images obtained are as follows: Figure 3As shown; among them, Figure 3 As shown in part (a), the microstructure of the sample that has not been heat treated is mainly composed of lath-shaped martensite and austenite, and the grains are uniform and fine. There are no defects such as large macroscopic holes and cracks in the structure. However, the keyhole collapses during the SLM forming process, resulting in a small number of tiny pores in the structure; Figure 3 As shown in part (b), the sample structure after heat treatment is long strips, and the strips of different orientations intersect at a certain angle, and the width of the strips is slightly increased, but the internal structure is uniform and dense, and a small amount of pores are eliminated. It can be seen that the sequential 850℃×1h solution treatment and 550℃×4h aging heat treatment can significantly improve the printed structure of MS1 ultra-high strength martensitic die steel.
[0041] The heat-treated and unheat-treated MS1 ultra-high strength martensitic die steel samples were processed into standard tensile test bars and subjected to tensile tests on a WDW-100KN universal testing machine at a strain increment of 0.3% and a strain rate of 10-3s-1. The mechanical properties obtained are shown in Table 1:
[0042] Table 1 Mechanical properties comparison table
[0043]
[0044] It can be seen from the table that after heat treatment, the yield strength of MS1 ultra-high strength martensitic die steel increased from 913MPa to 1982MPa, an increase of more than 1 times; the tensile strength increased from 1186MPa to 2017MPa, an increase of more than 70%; the average Vickers hardness value increased from 312HV0.3 to 569HV0.3, and the hardness value increased by more than 82%.
[0045] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for manufacturing 2GPa grade ultra-high strength martensitic die steel, characterized in that: The steps include: Step 1) using a laser selective melting method to prepare an ultra-high strength martensitic die steel workpiece, wherein: Using MS1 ultra-high strength martensitic die steel powder as raw material; The laser power of the laser selective melting method is 175W, the scanning speed is 1000mm / s, and the scanning spacing is 0.07mm; Step 2) performing solution treatment and aging heat treatment on the martensitic die steel workpiece prepared in step 1); The treatment temperature of the solution treatment is 850 °C and the treatment time is 1 h; The treatment temperature of aging heat treatment is 550℃ and the treatment time is 4 h.