A preparation method of PLGA without monomer and solvent residues
By using a small amount of solvent low temperature co-precipitation method during the preparation of PLGA, the monomer and solvent residues were successfully reduced, the purity and application effect of PLGA were improved, the residual problems in the prior art were solved, and efficient material preparation was achieved.
Patent Information
- Application Number
- CN202210568051.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-05-24
AI Technical Summary
The prior art is difficult to effectively reduce monomer and solvent residues when preparing PLGA, which affects the purity and application effect of the material. In particular, lactide residues may lead to uneven red blood cell hemolysis and microsphere drug release, and the existing removal methods are inefficient or Solvent residue is produced.
The low-temperature co-precipitation method of a small amount of solvent is adopted to ensure that there is no monomer and solvent residue residue residue by polymerizing the crude PLGA product at anhydrous and oxygen-free conditions, and adding good solvents and poor solvents at low temperatures for multiple spraying and vacuum drying.
The high purity preparation of PLGA is achieved, which avoids red blood cell hemolysis and uneven release of microspheres, improves the application effect of materials, and simplifies the process, which is suitable for industrial production.
Smart Images

Figure CN114920919B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of biomedical polymer materials, and in particular relates to a method for preparing PLGA without monomer and solvent residues. Background Art
[0002] Poly(L-Glycol Glycol) (PLGA) is a biomedical color polymer material and a new biodegradable material that has been widely studied and applied at home and abroad. It can be used as clinical medical materials such as sutures, bone screws, bone plugs and various stents, and can also be used as a carrier for sustained-release drug delivery systems. It is degraded into lactic acid and glycolic acid through polyester hydrolysis in the body, and then finally degraded into carbon dioxide and water through the tricarboxylic acid cycle in the body. It has been approved by the FDA as a pharmaceutical excipient.
[0003] It can be obtained by ring-opening polymerization of glycolide and lactide monomers under anhydrous and oxygen-free conditions, so a small amount of monomers will remain in the polymer. A small amount of glycolide and lactide residues can change the chemical environment inside the PLGA microspheres and affect the burst release of the microspheres. Lactide can lower the pH value inside the microspheres, enhance the hydrophilicity inside the microspheres, and increase the water intake, thereby affecting the burst release. For glycolide-lactide copolymers, the 2015 edition of the "Chinese Pharmacopoeia Volume IV" monograph clearly stipulates that the glycolide residue shall not exceed 0.5% and the lactide residue shall not exceed 2.0%.
[0004] The triblock copolymer PLGA-PEG-PLGA has broad application prospects in the field of medical materials due to its good biocompatibility and biodegradability. Lactide is one of the monomers for synthesizing PLGA-PEG-PLGA. Its residue can dissolve in the blood, causing abnormal hemolysis of red blood cells. At the same time, solvent residues will also have an impact on it. Therefore, during the production process, it is very important to monitor the lactide and solvent residues in PLGA-PEG-PLGA for product safety.
[0005] In order to solve the above problems and reduce the residual monomers, vacuum heating is usually used to remove them, but the removal efficiency is low and the polymer color tends to deepen. The document "Removal of Residual Monomers in Lactide-Glycolide Copolymers" reports the dilute acid extraction method and ethanol precipitation method to remove glycolide and lactide residues.
[0006] The dilute acid extraction method mainly uses dilute acid to degrade the monomers into water-soluble lactic acid or glycolic acid to achieve the purpose of removing residual monomers. The residual monomers of unrefined PLGA (glycolide content 3.62%, lactide content 2.15%) can be reduced to 0.48% and 1.78% respectively, which meets the relevant regulations in the 2015 edition of the "Chinese Pharmacopoeia Volume IV".
[0007] Compared with the dilute acid extraction method, the ethanol precipitation method can avoid the use of acid to destroy the PLGA structure. It is also more efficient than the vacuum heating method and has a simple process. It can reduce the residual monomers of unrefined PLGA (glycolide content 3.62%, lactide content 2.15%) to 0.58% and 1.90%, respectively. The glycolide content exceeds the relevant provisions in the 2015 edition of the "Chinese Pharmacopoeia Volume IV".
[0008] Patent CN 105026458 B introduces that impurities in polyester, especially residual monomers, can weaken the stability of the polymer, reduce the mechanical properties of the polymer, especially the elastic strength, and further affect the application of polyester. Patent EP2221333 introduces the use of dry airflow to clean molten polyester, which can reduce the residual lactide in the polyester, but the final test result shows that the lactide content is still greater than 0.2%, which cannot meet special application requirements.
[0009] Patent WO 2007 / 088135 introduces that the monomer residue can be eliminated by first dissolving the polymer in a solvent and then precipitating it with a large amount of poor solvent. This method can achieve undetectable monomer. However, this method uses a large amount of solvent and will cause solvent residue, affecting the final use. Summary of the invention
[0010] The main purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing PLGA without monomer and solvent residues. The present invention reduces the residual amount of monomers in the glycolide-lactide polymer and reduces the solvent residue by using a small amount of solvent for low-temperature coprecipitation, while ensuring the product yield and improving the effect of PLGA in practical applications.
[0011] The purpose of the present invention and the solution to the technical problem are achieved by adopting the following technical solutions.
[0012] The present invention provides a method for preparing PLGA without monomer and solvent residues, the method comprising the following steps:
[0013] S1. Using glycolide and lactide as raw materials, adding a catalyst and an initiator, and polymerizing at high temperature under anhydrous and oxygen-free conditions to obtain a crude PLGA product;
[0014] S2. Add a good solvent to the PLGA crude product obtained above to completely dissolve the polymer, then filter, and drop the filtrate into a low-temperature poor solvent, centrifuge and dry under vacuum, spraying the poor solvent several times during the process, and finally obtain dry PLGA without monomer and solvent residue.
[0015] Preferably, in step S1, the catalyst is selected from stannous isooctanoate, and the initiator is selected from lactic acid, purified water, methanol, dodecanol, and hexanol.
[0016] Preferably, the high temperature polymerization condition in step S1 is a reaction temperature of 120-190°C.
[0017] Preferably, the good solvent in step S2 includes chloroform, acetone or dichloromethane.
[0018] More preferably, the good solvent in step S2 is acetone or dichloromethane.
[0019] Preferably, the poor solvent in step S2 is selected from methanol, ethanol or diethyl ether.
[0020] More preferably, the poor solvent in step S2 is ethanol.
[0021] Preferably, the pore size of the filter membrane used in the filter press in step S2 is 0.10-0.45 μm.
[0022] More preferably, the pore size of the filter membrane used in the filter press in step S2 is 0.22 μm.
[0023] Preferably, in step S2, the mass ratio of the good solvent to the polymer is 15-4:1.
[0024] Preferably, in step S2, the mass ratio of the poor solvent to the polymer is 30-15:1.
[0025] Preferably, the amount of the poor solvent sprayed once in step S2 is 1-10% of the dry polymer.
[0026] More preferably, the amount of the poor solvent sprayed once in step S2 is 1-2% of the dry polymer.
[0027] Preferably, the coprecipitation temperature in step S2 is between -10 and -30°C.
[0028] More preferably, the coprecipitation temperature in step S2 is between -15 and -25°C.
[0029] By means of the above technical solution, the present invention has at least the following advantages:
[0030] The refining process used in the present invention can well solve the problem of monomer glycolide-lactide residue and solvent residue in the process of preparing glycolide-lactide copolymer (PLGA), so that there is no monomer residue and no solvent residue. It effectively solves the problem that the PLGA purity is not high due to monomer and solvent residue, which affects the practical application. At the same time, it solves the hemolysis of red blood cells and the release of microsphere drugs in the body. The obtained glycolide-lactide copolymer has high purity, and the polymer is in the form of fine particles, and no secondary molding is required. The equipment and process required by the present invention are relatively simple, the operability is strong, the selected refined reagents are economical and safe, and the prepared PLGA has high purity, which is conducive to the industrial production of glycolide-lactide copolymer, and is widely used in microspheres and other fields.
[0031] In summary, the preparation method of the present invention has the above-mentioned advantages and practical values, and is truly innovative because no similar design has been publicly published or used in similar products. It has great improvements in both product components and functions, great technical progress, and produces good and practical effects. It has multiple enhanced functions compared to existing methods, making it more suitable for practical use and has wide industrial utilization value. It is truly a novel, progressive and practical new design.
[0032] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows.
[0033] The specific embodiments of the present invention are given in detail by the following examples. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 A GPC spectrum for detecting the residual solvent of PLGA obtained according to the preparation method of the present invention;
[0035] Figure 2 This is a GPC spectrum for detecting monomer residues of PLGA obtained according to the preparation method of the present invention. DETAILED DESCRIPTION
[0036] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation method, method and effects of the technical solution proposed by the present invention are described in detail below in combination with the preferred embodiments and the accompanying drawings.
[0037] The mass ratio of the good solvent to the polymer described in this embodiment needs to be determined according to the molecular weight of the polymer. The larger the molecular weight, the more solvent is added, and it is controlled within 15-4:1; the mass ratio of the poor solvent to the polymer needs to be determined according to the molecular weight of the polymer. The larger the molecular weight, the more solvent is added, and it is controlled within 30-15:1. Among them, the polymer molecular weight is measured by GPC (gel permeation chromatography) using tetrahydrofuran as the solvent.
[0038] The determination of glycolide and lactide residues described in this embodiment is determined by molecular exclusion chromatography (General Rule 0514), using a gel chromatography column, tetrahydrofuran as the mobile phase, and a differential refractive index detector; the detector temperature is 35°C. Take 20μL of each of the above-mentioned reference solution, inject it into the liquid chromatograph, record the chromatogram, and calculate the regression equation by GPC software. Take 20μL of the test solution, determine it in the same way, and use GPC software to calculate the weight average molecular weight, number average molecular weight and molecular weight distribution of the test sample.
[0039] Example 1
[0040] Weigh 50g lactide, 13.43g glycolide, 0.019g stannous isooctanoate and 0.19g purified water, add to a 250mL three-necked flask, turn on the stirring to 100rpm, vacuum for 15min, then flush with nitrogen to normal pressure, and repeatedly replace nitrogen 3 times. After glycolide and lactide are completely melted, adjust the speed to 300rpm, heat to 140℃ for 6h, and continue to heat to 160℃ for 4h. Stop the reaction, take samples and send them for molecular weight and viscosity. Using chloroform as solvent, the viscosity of the copolymer was measured with an Ubbelohde viscometer at 25℃; using tetrahydrofuran as solvent, GPC measured the molecular weight of the copolymer, and the weight average molecular weight was 11001 and the molecular weight distribution was 1.40.
[0041] Add 4 times the mass of acetone to the copolymer and slowly dissolve it at room temperature. After it is completely dissolved, use a 0.1 micron filter membrane for filter pressing. Slowly add the filtrate to a 15 times the mass of methanol solution at -10°C. White floccules are produced. After the addition is completed, stir for another 1h, and the stirring rate is maintained at 100 rpm / min. After the reaction is completed, centrifuge to obtain a filter cake, place it in a vacuum drying oven, dry it at 45°C and -0.1MPa for 12h, and take a sample for inspection of glycolide and lactide residues (detection method: according to molecular exclusion chromatography (General Rule 0514), gel chromatography column, tetrahydrofuran as mobile phase, differential refractive index detector; detector temperature 35°C. Take 20µL of each of the above reference solution, inject it into the liquid chromatograph, record the chromatogram, and calculate the regression equation by GPC software. Take 20µL of the test solution, determine it in the same way, and use GPC software to calculate the weight average molecular weight, number average molecular weight and molecular weight distribution of the test product). Repeat the above refining process twice, and in the last drying process, spray methanol twice, the spraying mass is 0.5% of the polymer mass, dry for 12 hours, and the test shows that no glycolide residue is detected, no lactide residue is detected, and no solvent residue is detected. (See the attached for specific results) Figure 1 )
[0042] Example 2
[0043] Weigh 50g lactide, 13.43g glycolide, 0.019g stannous isooctanoate and 0.34g methanol, add to a 250mL three-necked flask, turn on the stirring to 100rpm, vacuum for 15min, then flush with nitrogen to normal pressure, and repeatedly replace nitrogen 3 times. After glycolide and lactide are completely melted, adjust the speed to 300rpm, heat to 140℃ for 6h, and continue to heat to 160℃ for 4h. Stop the reaction, take samples and send them for inspection of molecular weight and viscosity. Using chloroform as solvent, the viscosity of the copolymer was measured with an Ubbelohde viscometer at 25℃; using tetrahydrofuran as solvent, GPC measured the molecular weight of the copolymer, and the weight average molecular weight was 11861, and the molecular weight distribution was 1.41.
[0044] Add 15 times the mass of dichloromethane to the copolymer and slowly dissolve it at room temperature. After it is completely dissolved, use a 0.22 micron filter membrane for filter pressing, and slowly add the filtrate to a 25 times mass ethanol solution at -15°C. White floccules are produced. After the addition is completed, stir for another 1h, and the stirring rate is maintained at 100 rpm / min. After the reaction is completed, centrifuge to obtain a filter cake, which is placed in a vacuum drying oven and dried at 45°C and -0.1MPa for 12h. Samples are taken for inspection of glycolide and lactide residues (the detection method is as described in Example 1). Repeat the above refining process 3 times. In the last drying process, spray methanol 3 times, and the spraying mass is 1% of the polymer mass. Dry for 12h, and obtain a glycolide residue that is not detected, a lactide residue that is not detected, and a solvent residue that is not detected.
[0045] Example 3
[0046] Weigh 30g lactide, 8.06g glycolide, 0.019g stannous isooctanoate and 0.038g lactic acid, add to a 250mL three-necked flask, turn on the stirring to 100rpm, vacuum for 15min, then flush with nitrogen to normal pressure, and repeatedly replace nitrogen 3 times. After glycolide and lactide are completely melted, adjust the speed to 300rpm, continue to heat to 140℃ for 6h, and continue to heat to 160℃ for 4h. Stop the reaction, take samples and send them for inspection of molecular weight and viscosity. Using chloroform as solvent, the viscosity of the copolymer was measured with an Ubbelohde viscometer at 25℃; using tetrahydrofuran as solvent, GPC measured the molecular weight of the copolymer, and the weight average molecular weight was 45262, and the molecular weight distribution was 1.82.
[0047] Add 6 times the mass of chloroform to the copolymer and slowly dissolve it at room temperature. After it is completely dissolved, use a 0.45 micron filter membrane for filter pressing, and slowly add the filtrate to a 20 times mass ethanol solution at -30°C. White floccules are produced. After the addition is completed, stir for another 1h, and the stirring rate is maintained at 100 rpm / min. After the reaction is completed, centrifuge to obtain a filter cake, which is placed in a vacuum drying oven at 45°C and -0.1MPa for 12h. Samples are taken for inspection of glycolide and lactide residues (the detection method is as described in Example 1). Repeat the above refining process 3 times. In the last drying process, spray methanol 3 times, and the spraying mass is 10% of the polymer mass. Dry for 12h, and obtain a glycolide residue that is not detected, a lactide residue that is not detected, and a solvent residue that is not detected.
[0048] Example 4
[0049] Weigh 30g lactide, 8.06g glycolide, 0.0114g stannous isooctanoate and 0.0079g dodecanol, add to a 250mL three-necked flask, turn on the stirring to 100rpm, vacuum for 15min, then flush with nitrogen to normal pressure, and repeatedly replace nitrogen 3 times. After glycolide and lactide are completely melted, adjust the speed to 300rpm, continue to heat to 140℃ for 6h, and continue to heat to 160℃ for 4h. Stop the reaction, take samples and send them for inspection of molecular weight and viscosity. Using chloroform as solvent, the viscosity of the copolymer was measured with an Ubbelohde viscometer at 25℃; using tetrahydrofuran as solvent, GPC measured the molecular weight of the copolymer, and the weight average molecular weight was 111522, and the molecular weight distribution was 2.10.
[0050] Add 10 times the mass of dichloromethane to the copolymer and slowly dissolve it at room temperature. After it is completely dissolved, use a 0.30 micron filter membrane for filter pressing, and slowly add the filtrate to a 30 times mass ether solution at -25°C. White floccules are produced. After the addition is completed, stir for another 1h, and the stirring rate is maintained at 100 rpm / min. After the reaction is completed, centrifuge to obtain a filter cake, which is placed in a vacuum drying oven and dried at 45°C and -0.1MPa for 12h. Samples are taken for inspection of glycolide and lactide residues (the detection method is as described in Example 1). Repeat the above refining process twice. In the last drying process, spray methanol twice, and the spraying mass is 2% of the polymer mass. Dry for 12h, and the glycolide residue is not detected, the lactide residue is not detected, and the solvent residue is not detected.
[0051] Example 5
[0052] Weigh 30g lactide, 8.06g glycolide, 0.0114g stannous isooctanoate and 0.0043g hexanol, add to a 250mL three-necked flask, turn on the stirring to 100rpm, vacuum for 15min, then flush with nitrogen to normal pressure, and repeatedly replace nitrogen 3 times. After glycolide and lactide are completely melted, adjust the speed to 300rpm, continue to heat to 140℃ for 6h, and continue to heat to 160℃ for 4h. Stop the reaction, take samples and send them for inspection of molecular weight and viscosity. Using chloroform as solvent, the viscosity of the copolymer is measured with an Ubbelohde viscometer at 25℃; using tetrahydrofuran as solvent, GPC measures the molecular weight of the copolymer, and the weight average molecular weight is 120011, and the molecular weight distribution is 2.23.
[0053] Add 15 times the mass of dichloromethane to the copolymer and slowly dissolve it at room temperature. After it is completely dissolved, use a 0.30 micron filter membrane for filter pressing, and slowly add the filtrate to a 25 times the mass of methanol solution at -25°C. White floccules are produced. After the addition is completed, stir for another 1h, and the stirring rate is maintained at 100 rpm / min. After the reaction is completed, centrifuge to obtain a filter cake, which is placed in a vacuum drying oven and dried at 45°C and -0.1MPa for 12h. Samples are taken for inspection of glycolide and lactide residues (the detection method is as described in Example 1). Repeat the above refining process twice. In the last drying process, methanol is sprayed twice, and the spraying mass is 1% of the polymer mass. Dry for 12h, and the glycolide residue is not detected, the lactide residue is not detected, and the solvent residue is not detected.
[0054] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A method for preparing PLGA without monomer and solvent residues, characterized in that: The method comprises the following steps: S1. Using glycolide and lactide as raw materials, adding a catalyst and an initiator, and polymerizing at high temperature under anhydrous and oxygen-free conditions to obtain a crude PLGA product; the high-temperature polymerization condition is a reaction temperature of 120-190°C; S2. Add a good solvent to the PLGA crude product obtained above to completely dissolve the polymer, then filter press, and dropwise add the filtrate into a low-temperature poor solvent for co-precipitation, centrifuge and dry, vacuum dry, sample and send for inspection of glycolide and lactide residues, repeat the above refining process two or three times, and during the last drying process, spray the poor solvent several times to finally obtain dry PLGA without monomer and solvent residues; the multiple times are two or three times; In step S2, the good solvent is chloroform, acetone or dichloromethane; the mass ratio of the good solvent to the polymer is 15-4:1; In step S2, the poor solvent is methanol, ethanol or diethyl ether; the mass ratio of the poor solvent to the polymer is 30-15:1; The amount of the poor solvent sprayed once in step S2 is 0.5-10% of the dry polymer; The coprecipitation temperature in step S2 is between -10 and -30°C.
2. The method for preparing PLGA without monomer and solvent residue according to claim 1, characterized in that: In step S1, the catalyst is selected from stannous isooctanoate, and the initiator is selected from lactic acid, purified water, methanol, dodecanol or hexanol.
3. The method for preparing PLGA without monomer and solvent residue according to claim 1, characterized in that: The pore size of the filter membrane used in the filter press in step S2 is 0.10-0.45 μm.
Citation Information
Patent Citations
Method for Purifying Polyester
CN105026458B
Method for the purification of resorbable polymers from residual monomers
WO2007088135A1
Method for the purification of resorbable polymers from residual monomers
CN101400708A
Method for measuring glycolide and D, L-lactide copolymer monomer conversion rate
CN105301029A
Technology for preparing high-molecular-weight MPLGA by directly grafting maleic anhydride onto PLGA
CN105315412A
Cited By
Novel preparation method of high molecular weight and high conversion rate PLGA (poly (lactic-co-glycolic acid))
CN122037147A