Epoxy resin composition for prepreg and prepreg

By mixing a curing agent, silica particles and core-shell rubber particles into the epoxy resin and adjusting their ratio, the problem of resin fluidity and molding workability during heat curing of the epoxy resin composition for prepregs was solved. , achieving the elimination of resin defects and thickness uniformity, and improving the mechanical strength of fiber-reinforced composite materials.

CN115003752BActive Publication Date: 2024-10-01THE YOKOHAMA RUBBER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180011021.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2021-01-05
Publication Date
2024-10-01
Estimated Expiration
2041-01-05

AI Technical Summary

Technical Problem

Existing epoxy resin compositions for prepregs have strong resin fluidity when heated and cured, resulting in resin defects and uneven thickness, and the high room temperature viscosity worsens the molding workability.

Method used

A curing agent or curing accelerator, silica particles, and core-shell rubber particles are mixed with the epoxy resin, and the mixing ratio is specified to suppress the flow of the resin and increase the viscosity.

Benefits of technology

Effectively suppresses resin flow during heating and curing, eliminates resin defects and uneven thickness, and improves the workability and mechanical strength of prepregs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003764630360000101
    Figure BDA0003764630360000101
Patent Text Reader

Abstract

The epoxy resin composition for prepreg of the present invention contains (A) an epoxy resin, (B) a curing agent or a curing accelerator, (C) silica fine particles, and (D) core-shell rubber particles. The composition contains 1 to 5 parts by mass of the silica fine particles (C) and 2 to 10 parts by mass of the core-shell rubber particles (D) relative to 100 parts by mass of the epoxy resin (A), and the mass ratio of the silica fine particles (C) to the core-shell rubber particles (D) is 1 / 1 to 1 / 5 in terms of (C) / (D).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an epoxy resin composition for prepreg and a prepreg. Background Art

[0002] Fiber-reinforced composite materials using thermosetting resins represented by epoxy resins as a matrix are known. For example, Patent Document 1 discloses an epoxy resin composition containing an epoxy resin as a matrix, a thermoplastic resin for viscosity adjustment, a filler, and a curing agent, and also discloses a prepreg obtained by compounding the composition with reinforcing fibers.

[0003] However, conventional epoxy resin compositions for prepregs have problems such as difficulty in adjusting viscosity, and low viscosity when heated for curing although having high viscosity at room temperature. Due to this problem, when the prepreg is heated and cured, the resin composition flows out from the reinforcing fibers, and the resulting fiber-reinforced composite material suffers from resin defects, and the thickness becomes uneven. In order to suppress the flow of resin during curing, it is necessary to make the viscosity of the resin composition higher, but in this case, since the viscosity of the resin composition at room temperature becomes too high, the workability during prepreg molding deteriorates.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2011-99094 Summary of the invention

[0007] Problems to be solved by the invention

[0008] Therefore, an object of the present invention is to provide an epoxy resin composition for prepreg which can suppress resin flow during heat curing, eliminate resin defects and uneven thickness, and has excellent workability, and a prepreg using the epoxy resin composition for prepreg.

[0009] Methods for solving problems

[0010] The inventors of the present invention have repeatedly conducted in-depth research and found that the above-mentioned problems can be solved by mixing a curing agent or a curing accelerator, silica particles and core-shell rubber particles into an epoxy resin, and specifying the mixing amount of the above-mentioned silica particles and core-shell rubber particles and the mixing ratio of the two, thereby completing the present invention.

[0011] The present invention provides an epoxy resin composition for prepreg, characterized in that it contains

[0012] (A) Epoxy resin,

[0013] (B) curing agent or curing accelerator,

[0014] (C) silica particles, and

[0015] (D) core-shell rubber particles,

[0016] The above-mentioned (C) silica fine particles 1 to 5 parts by mass and the above-mentioned (D) core-shell rubber particles 2 to 10 parts by mass are contained with respect to 100 parts by mass of the above-mentioned (A) epoxy resin,

[0017] The mass ratio of the (C) silica fine particles to the (D) core-shell rubber particles is (C) / (D) 1 / 1 to 1 / 5.

[0018] Effects of the Invention

[0019] According to the present invention, the following epoxy resin composition for prepreg and the prepreg using the epoxy resin composition for prepreg can be provided: wherein, since (B) a curing agent or a curing accelerator, (C) silica particles, and (D) core-shell rubber particles are mixed with (A) epoxy resin, and the mixing amounts of the above-mentioned silica particles and core-shell rubber particles and the mixing ratio of the two are specified, the resin flow during heat curing can be suppressed, resin defects and thickness unevenness can be eliminated, and excellent workability can be achieved. DETAILED DESCRIPTION

[0020] Hereinafter, embodiments of the present invention will be described in further detail.

[0021] (A) Epoxy resin

[0022] Examples of the epoxy resin (A) used in the present invention include epoxy compounds having biphenyl groups such as bisphenol A type, bisphenol F type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol S type, bisphenol AF type, biphenyl type, epoxy compounds having bisphenyl groups, polyalkylene glycol type, epoxy compounds having alkylene glycol type, epoxy compounds having naphthalene rings, epoxy compounds having fluorene groups, bifunctional glycidyl ether type epoxy resins such as phenol novolac type, o-cresol novolac type, trihydroxyphenylmethane type, trifunctional type, and tetraphenolylethane type, glycidyl ester type epoxy resins of synthetic fatty acids such as dimer acid, glycidyl amine type epoxy resins, etc. Among them, by using an epoxy resin that does not contain a nitrogen atom, the effect of the present invention can be further improved, although the reason is unclear.

[0023] (B) Curing agent or curing accelerator

[0024] The (B) curing agent or curing accelerator used in the present invention is not particularly limited, and examples thereof include amines, acid anhydrides, novolac resins, phenols, thiols, Lewis acid amine complexes, Salt, and imidazole, etc.

[0025] (C) Silica particles

[0026] The (C) silica fine particles used in the present invention are preferably hydrophilic silica fine particles, and examples thereof include amorphous synthetic silica such as precipitated silica, gel silica, fumed silica, and fused silica; crystalline synthetic silica; and natural silica.

[0027] The shape of the silica particles is not particularly limited. For example, spherical, granular, irregularly shaped (irregularly shaped, amorphous) materials can be cited. From the viewpoint of satisfying heat resistance, toughness and the above-mentioned viscosity characteristics at the same time, spherical, granular and irregular shapes are preferred.

[0028] (C) Silica fine particles can be appropriately selected from commercially available ones, and examples thereof include CAB-O-SIL M5 (hydrophilic fumed silica) manufactured by CABOT Co., Ltd. and AEROSIL 200 (average particle size 12 nm) manufactured by Nippon Aerosil Co., Ltd.

[0029] The average particle size of the silica fine particles (C) is preferably 5 to 100 nm, more preferably 50 nm or less.

[0030] (D) Core-shell rubber particles

[0031] The (D) core-shell rubber particles used in the present invention are well known and may be particles obtained by graft-polymerizing a shell component polymer of a different type from the core component onto the surface of a particulate core component mainly composed of a crosslinked rubber polymer.

[0032] Examples of the core component include butadiene rubber, acrylic rubber, silicone rubber, butyl rubber, NBR, SBR, IR, and EPR.

[0033] Examples of the shell component include polymers obtained by polymerizing monomers selected from acrylic acid ester monomers, methacrylic acid ester monomers, aromatic vinyl monomers, and the like.

[0034] The average particle diameter of the core-shell rubber particles (D) is, for example, 10 nm to 10 μm, or preferably 100 nm to 500 nm.

[0035] (D) The core-shell rubber particles can be appropriately selected from commercially available materials, and examples thereof include MX-153 (epoxy resin (bisphenol A type diglycidyl ether) / core-shell rubber particle masterbatch; containing 33% by mass of butadiene-based core-shell rubber particles; average particle size = 100 to 200 nm) and MX-154 (epoxy resin (bisphenol A type diglycidyl ether) / core-shell rubber particle masterbatch; containing 40% by mass of butadiene-based core-shell rubber particles; average particle size = 200 to 300 nm) manufactured by Kaneka Co., Ltd. =100~200nm), MX-257 (epoxy resin (bisphenol A type diglycidyl ether) / core-shell rubber particle masterbatch; containing 37% by mass of butadiene-based core-shell rubber particles; average particle size = 100~200nm), MX-125 manufactured by Kanekaka Co., Ltd. (epoxy resin (bisphenol A type diglycidyl ether) / core-shell rubber particle masterbatch; containing 25% by mass of SBR-based core-shell rubber particles; average particle size = 100~200nm), etc.

[0036] When the master batch is used, the epoxy resin contained therein is included in the amount of the epoxy resin (A).

[0037] In addition, the so-called average particle size in the present invention refers to the average value of the equivalent circle diameter measured using an electron microscope, a laser microscope, etc., and can be measured, for example, using a laser diffraction and scattering particle size distribution measuring device LA-300 (manufactured by Horiba, Ltd.), a laser microscope VK-8710 (manufactured by Keyence Corporation), etc.

[0038] In the present invention, a thermoplastic resin may be blended as necessary.

[0039] Examples of the thermoplastic resin include polyethersulfone (PES), polyimide, polyetherimide (PEI), polyamideimide, polysulfone, polycarbonate, polyetheretherketone, polyamides such as nylon 6, nylon 12, and amorphous nylon, aromatic polyamides, aromatic esters, polyester carbonates, and phenoxy resins.

[0040] Among them, phenoxy resins are preferred from the viewpoint of being able to further improve the above-mentioned viscosity characteristics.

[0041] (Mixing ratio)

[0042] The epoxy resin composition for prepreg of the present invention comprises 1 to 5 parts by mass of (C) silica fine particles and 2 to 10 parts by mass of (D) core-shell rubber particles relative to 100 parts by mass of (A) epoxy resin, wherein the mass ratio of the (C) silica fine particles to the (D) core-shell rubber particles is 1 / 1 to 1 / 5 as expressed in terms of (C) / (D).

[0043] If the blending ratio of (C) the silica fine particles is less than 1 part by mass or the blending ratio of (D) the core-shell rubber particles is less than 2 parts by mass, the flow of the resin during heat curing is insufficiently suppressed and the effects of the present invention cannot be achieved.

[0044] When the mixing ratio of the (C) silica fine particles exceeds 5 parts by mass, the viscosity of the resin composition at room temperature becomes too high, and workability during prepreg molding deteriorates.

[0045] If the content of the core-shell rubber particles (D) exceeds 10 parts by mass, the flow of the resin during heat curing is insufficiently suppressed, and the mechanical strength of the molded prepreg becomes insufficient.

[0046] When the mass ratio of (C) silica fine particles to (D) core-shell rubber particles exceeds 1 / 1 in terms of (C) / (D), that is, when the blending amount of component (D) is small relative to component (C), the flow of the resin during heat curing is insufficiently suppressed and the effect of the present invention cannot be exerted.

[0047] When the mass ratio of (C) silica fine particles to (D) core-shell rubber particles is less than 1 / 5 in terms of (C) / (D), that is, when the compounding amount of the (D) component is too large relative to the (C) component, the viscosity of the resin composition at room temperature becomes too high, and the workability during prepreg molding deteriorates.

[0048] The (B) curing agent or curing accelerator may be mixed in an appropriate amount depending on the type of the curing agent, and determination of the amount is easy for those skilled in the art.

[0049] In the present invention, the blending amount of the (C) silica fine particles is more preferably 2 to 4 parts by mass, the blending amount of the (D) core-shell rubber particles is more preferably 4 to 8 parts by mass, and the mass ratio of the (C) silica fine particles to the (D) core-shell rubber particles is more preferably 1 / 1.5 to 1 / 4 in terms of (C) / (D), relative to 100 parts by mass of the (A) epoxy resin.

[0050] When a thermoplastic resin is used, the amount thereof blended is preferably 5 to 50 parts by mass, more preferably 10 to 30 parts by mass, based on 100 parts by mass of the (A) epoxy resin.

[0051] When the epoxy resin composition for prepreg of the present invention was subjected to viscoelasticity measurement at a temperature of 70 °C and a frequency of 1 Hz using parallel plates, the tanδ at a strain of 1% was less than 1, and the tanδ at a strain of 100% was greater than 1. As a result, the resin flow during heat curing was suppressed, resin defects and thickness non-uniformity were less likely to occur, and the workability was particularly excellent. In addition, the viscoelasticity measurement can be performed using, for example, ARES manufactured by TA Instruments. Furthermore, this viscoelasticity can be achieved by appropriately setting the blending amounts of (C) silica fine particles and (D) core-shell rubber particles relative to (A) epoxy resin within the above ranges.

[0052] The epoxy resin composition for prepreg of the present invention may contain other additives as needed. Examples of the additives include fillers, anti-aging agents, solvents, flame retardants, reaction retardants, antioxidants, pigments (dyes), plasticizers, thixotropy imparting agents, ultraviolet absorbers, surfactants (including leveling agents), dispersants, dehydrating agents, tackifiers, antistatic agents, and the like.

[0053] The prepreg of the present invention is made of the above-mentioned epoxy resin composition for prepreg of the present invention and reinforcing fibers. Since the prepreg of the present invention is made of the above-mentioned epoxy resin composition for prepreg of the present invention and reinforcing fibers, resin defects and thickness non-uniformity are also suppressed, and thus the mechanical strength is excellent.

[0054] Specifically, the prepreg of the present invention is obtained by impregnating the reinforcing fibers with the epoxy resin composition for prepreg of the present invention.

[0055] There is no particular limitation on the reinforcing fibers used in the prepreg of the present invention, and examples thereof include conventionally known substances. Among them, from the viewpoint of strength, at least one selected from carbon fibers, glass fibers, and aramid fibers is preferred.

[0056] Regarding the fibers, there is no particular limitation on their form, and examples include rovings, substances obtained by aligning rovings unidirectionally, woven fabrics, non-woven fabrics, knitted fabrics, and gauzes.

[0057] There is no particular limitation on the manufacturing method of the prepreg of the present invention. Examples include the wet method using a solvent and the hot melt method as a solvent-free method. From the viewpoint of being able to shorten the drying time, the amount of the solvent used is preferably 80 to 200 parts by mass relative to 100 parts by mass of the solid content of the epoxy resin composition for prepreg.

[0058] In the prepreg of the present invention, from the viewpoint of the mechanical properties of the resulting fiber-reinforced composite material, the content of the epoxy resin composition for prepreg is preferably 30 to 60% by mass in the prepreg.

[0059] There is no particular limitation on the use of the prepreg of the present invention. By curing the prepreg of the present invention, for example, a fiber-reinforced composite material known in the past can be obtained. Specifically, for example, aircraft parts such as fairings, flaps, leading edges, floors, propellers, and fuselages; two-wheeled vehicle parts such as motorcycle frames, front cowls, and mudguards; automobile parts such as doors, hoods, tailgates, side fenders, side panels, fenders, energy absorbing components, trunk lids, hardtops, exterior mirror covers, spoilers, diffusers, ski racks, engine cylinder heads, engine hoods, chassis, air spoilers, and drive shafts; vehicle noses, roofs, side panels, doors, hoods, side skirts, and other vehicle parts. Vehicle outer panels; railway vehicle parts such as luggage racks and seats; interior decoration, wing inner panels, outer panels, roofs, floors, etc. in wing cars, streamlined parts such as side skirts installed on cars and bicycles; shell applications for notebook personal computers, mobile phones, etc.; medical applications such as X-ray cassettes and top panels; applications in audio products such as flat speaker panels and speaker cones; applications in sports goods such as golf club heads, panels, snowboards, surfboards, and protective gear; general industrial applications such as leaf springs, windmill blades, and elevators (box panels, doors).

[0060] In addition, the prepreg of the present invention can be laminated with other members (for example, honeycomb core) to produce a fiber-reinforced composite material. Examples of fiber-reinforced composite materials that can be laminated with the prepreg of the present invention and other members include honeycomb sandwich panels.

[0061] Example

[0062] Hereinafter, the present invention will be further described by way of Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0063] In the examples described below, the following materials were used.

[0064] (A) Epoxy resin 1: Nippon Steel & Sumitomo Metal Chemical Corporation YD-128 (bisphenol A diglycidyl ether (DEGBA). Viscosity at 25° C. = 10,000 to 15,000 mPa·s);

[0065] (A) Epoxy resin 2: Nippon Steel & Sumitomo Metal Chemical Corporation YD-014 (bisphenol A type diglycidyl ether (DEGBA). Softening point: 100° C.)

[0066] (B) Curing agent: DICY-15 (dicyandiamide) manufactured by Mitsubishi Chemical Corporation

[0067] (B) Curing accelerator: OMICURE 24 (urea) manufactured by CVC Thermoset Specialties

[0068] (C) Silica fine particles: CAB-O-SIL M5 (hydrophilic fumed silica) manufactured by CABOT Co., Ltd.

[0069] (C) Silica particles: AEROSIL 200 (hydrophilic fumed silica) manufactured by Japan Aerosil Corporation

[0070] (D) Core-shell rubber particles: MX-153 manufactured by Kaneka Co., Ltd. (bisphenol A diglycidyl ether (DEGBA) / core-shell rubber particle masterbatch; containing 33% by mass of butadiene-based core-shell rubber particles)

[0071] (D) MX-154 manufactured by Kaneka Co., Ltd. (bisphenol A diglycidyl ether (DEGBA) / core-shell rubber particle masterbatch; containing 40% by mass of butadiene core-shell rubber particles; average particle size = 100 to 200 nm)

[0072] (D) MX-257 manufactured by Kaneka Co., Ltd. (epoxy resin (bisphenol A type diglycidyl ether) / core-shell rubber particle masterbatch; containing 37% by mass of butadiene-based core-shell rubber particles; average particle size = 100 to 200 nm)

[0073] (D) MX-125 manufactured by Kaneka Co., Ltd. (bisphenol A diglycidyl ether (DEGBA) / core-shell rubber particle masterbatch; containing 25% by mass of SBR core-shell rubber particles; average particle size = 100 to 200 nm)

[0074] Thermoplastic resin: YP-75 (phenoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.

[0075] The respective materials were kneaded at 70° C. using a kneader according to the blending ratios (parts by mass) shown in the following Table 1 to prepare various epoxy resin compositions for prepreg.

[0076] The following measurements were performed on the various epoxy resin compositions for prepregs obtained.

[0077] Viscoelasticity: Using ARES manufactured by Thermo Instruments, tan δ was measured at a strain of 1% or 100% with parallel plates at a temperature of 70° C. and a frequency of 1 Hz.

[0078] Prepreg molding

[0079] The epoxy resin composition film for prepreg (resin weight 104g / m 2 ) impregnated in glass fiber fabric (fiber basis weight 156g / m 2 ) to form a prepreg. The epoxy resin composition for prepreg in the formed prepreg is 40% by mass.

[0080] Workability: The workability during the preparation of the epoxy resin composition film for prepreg and during the impregnation into the glass fiber fabric was evaluated according to the following evaluation criteria.

[0081] ○: The film was well produced and the impregnation into the glass fiber fabric was good

[0082] ×: Since film production is difficult, prepreg molding is not possible

[0083] Dimensional stability: Ten prepregs cut into 300 mm×300 mm were stacked and cured in an autoclave at 120° C. for 2 hours, and the thickness of the obtained fiber-reinforced composite material was measured.

[0084] Evaluation was performed according to the following evaluation criteria.

[0085] ○: The difference between the maximum thickness and the minimum thickness is 5% or less of the maximum thickness, and the moldability (dimensional stability) is good.

[0086] ×: The difference between the maximum thickness and the minimum thickness exceeds 5% of the maximum thickness, and the moldability (dimensional stability) is poor.

[0087] Resin flow during curing: 6 prepregs cut into 100mm×100mm were stacked and sandwiched between metal plates with a 0.8mm thick metal spacer. 2 After pressing for 5 minutes, the weight of the cured resin protruding from the fibers was measured, and the resin flow was calculated by the following formula.

[0088] Resin flow (%)=(weight of exposed cured resin) / (weight of laminate before pressing)×100 was evaluated according to the following evaluation criteria.

[0089] ○: 6-10%

[0090] ×: Other than the above ○ (When the resin flow is small, the molded product does not have a chip, but the specified thickness cannot be obtained (it cannot be pressed to the thickness of the spacer). In addition, when the resin flow is large, the molded product has a chip and the thickness varies.)

[0091] Table 1 shows the results.

[0092] [Table 1]

[0093]

[0094] The results in Table 1 show that the epoxy resin compositions for prepregs of each embodiment in which (B) a curing agent or a curing accelerator, (C) silica particles and (D) core-shell rubber particles are added to (A) epoxy resin and the mixing ratio of (C) silica particles and (D) core-shell rubber particles to (A) epoxy resin is specified within the range specified in the present invention can suppress the flow of resin during heat curing, eliminate resin defects and uneven thickness, and have excellent workability. In addition, when the epoxy resin compositions for prepregs of each embodiment are subjected to viscoelasticity measurement using parallel plates at a temperature of 70°C and a frequency of 1 Hz, tan δ at a strain of 1% is less than 1, and tan δ at a strain of 100% is greater than 1, so that it is solid (tan δ < 1) at low strain, and the flow of resin during heat curing can be suppressed. In addition, it is liquid (tan δ ≥ 1) at high strain, and the workability during film coating and impregnation becomes good.

[0095] On the other hand, in Comparative Example 1, since (C) silica fine particles and (D) core-shell rubber particles were not added, the dimensional stability and the flow of the resin during curing were deteriorated.

[0096] In Comparative Example 2, since the amount of (C) silica fine particles added exceeded the upper limit specified in the present invention and (D) core-shell rubber particles were not added, workability, dimensional stability, and resin flow during curing were deteriorated.

[0097] In Comparative Example 3, since (C) silica fine particles were not added, the dimensional stability and the resin flow during curing were deteriorated.

[0098] In Comparative Example 4, since the above (C) / (D) was outside the range of the present invention, the result of resin flow during curing was deteriorated.

[0099] In Comparative Example 5, since the amount of the core-shell rubber particles (D) added exceeded the upper limit specified in the present invention, workability and resin flow during curing were deteriorated.

Claims

1. An epoxy resin composition for prepreg, characterized in that contain: (A) Epoxy resin, (B) curing agent or curing accelerator, (C) silica particles, and (D) core-shell rubber particles, The (C) silica fine particles are 1 to 5 parts by mass and the (D) core-shell rubber particles are 2 to 10 parts by mass relative to 100 parts by mass of the (A) epoxy resin. The mass ratio of the (C) silica fine particles to the (D) core-shell rubber particles is 1 / 1 to 1 / 5 (C) / (D). And the (A) epoxy resin does not contain nitrogen atoms.

2. The epoxy resin composition for prepreg according to claim 1, characterized in that When viscoelasticity is measured using parallel plates at a temperature of 70° C. and a frequency of 1 Hz, tan δ at a strain of 1% is less than 1, and tan δ at a strain of 100% is greater than 1.

3. The epoxy resin composition for prepreg according to claim 1, characterized in that The average particle size of the (C) silicon dioxide particles is 5 nm to 100 nm.

4. The epoxy resin composition for prepreg according to claim 1, characterized in that The average particle size of the (D) core-shell rubber particles is 10 nm to 10 μm.

5. The epoxy resin composition for prepreg according to claim 1, characterized in that 5 to 50 parts by mass of a thermoplastic resin is further mixed with 100 parts by mass of the (A) epoxy resin.

6. The epoxy resin composition for prepreg according to claim 5, characterized in that The thermoplastic resin is a phenoxy resin.

7. A prepreg, comprising the epoxy resin composition for prepreg according to claim 1 and reinforcing fibers.