Composition for forming EUV resist underlayer film
By using the resist underlayer film composition of (meth)acrylic polymer in the EUV lithography process, the amino group is used to improve the adhesion and shape of the resist pattern by baking, and the uniformity of the resist underlayer film is solved. The problem of properties and pattern quality has significantly improved the fine machining effect of semiconductor devices.
Patent Information
- Application Number
- CN202180013074.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-07
- Filing Date
- 2021-02-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-02-05
AI Technical Summary
In the EUV lithography process, it is difficult to form a uniform film on the lower layer of the resist, resulting in pinholes and coagulation, and the line width, roughness and adhesion of the resist pattern are insufficient, affecting the fine machining effect of semiconductor devices.
The composition containing (meth)acrylic polymer is used as the EUV resist underlayer film formation. The side chain of the polymer has alkaline organic groups substituted with a protective group, and an amino group is generated during the baking process to increase the The adhesiveness of the resist and the film forms a good rectangular resist pattern.
The deterioration of line width and roughness of the resist pattern is effectively suppressed, the sensitivity and adhesion of the resist is improved, and the pattern quality in the EUV lithography process is significantly improved.
Smart Images

Figure CN115053184B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composition used in a photolithography process in semiconductor manufacturing, particularly a composition used in the most advanced photolithography processes (ArF, EUV, EB, etc.), and also relates to a method for manufacturing a substrate with a resist pattern to which the above-mentioned resist underlayer film is applied, and a method for manufacturing a semiconductor device. Background Art
[0002] All along, in the manufacture of semiconductor devices, micro-machining is performed by using the photolithography of a resist composition. The above-mentioned micro-machining is to form a thin film of a photoresist composition on a semiconductor substrate such as a silicon wafer, and to irradiate active light such as ultraviolet rays across a mask pattern depicting a device pattern, and to develop, and to etch the substrate with the obtained photoresist pattern as a protective film, so as to form a processing method of fine concave-convex corresponding to the above-mentioned pattern on the substrate surface. In recent years, the high integration of semiconductor devices has been continuously developed, and the active light used is in addition to the i-line (wavelength 365nm), KrF excimer laser (wavelength 248nm), ArF excimer laser (wavelength 193nm) used in the past, and in the most advanced micro-machining, the practicality of EUV light (wavelength 13.5nm) or EB (electron beam) has also been studied. Accompanied by this, the poor formation of the resist pattern caused by the influence of the semiconductor substrate, etc., becomes a big problem. Therefore, in order to solve this problem, a method of arranging a resist lower film between a resist and a semiconductor substrate has been widely studied. Therefore, in order to solve this problem, a method of providing a resist underlayer film between the resist and the semiconductor substrate has been widely studied.
[0003] Patent Document 1 discloses an additive for a resist underlayer film-forming composition for increasing the adhesion of a resist pattern formed on a resist underlayer film.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2013 / 058189 Summary of the invention
[0007] Problems to be solved by the invention
[0008] Examples of the properties required of the resist underlayer film include not being mixed with the resist film formed on the upper layer (not being dissolved in the resist solvent) and having a higher dry etching rate than the resist film.
[0009] In the case of photolithography with EUV exposure, the line width of the formed resist pattern is less than 32nm, and the resist underlayer film for EUV exposure is formed and used with a thinner film thickness than before. When forming such a thin film, pinholes and condensation are easily generated due to the influence of the substrate surface and the polymer used, making it difficult to form a uniform film without defects.
[0010] On the other hand, when forming a resist pattern, the following method is sometimes adopted: in the development process, a solvent capable of dissolving the resist film, usually an organic solvent, is used to remove the unexposed portion of the resist film, and the exposed portion of the resist film remains as the resist pattern. In such a negative-type development process, the improvement of the adhesion of the resist pattern becomes a major issue.
[0011] In addition, it is required to suppress deterioration of LWR (Line Width Roughness) when forming a resist pattern, form a resist pattern having a good rectangular shape, and improve resist sensitivity.
[0012] An object of the present invention is to provide a composition for forming a resist underlayer film capable of forming a desired resist pattern, which solves the above-mentioned problems, and a resist pattern forming method using the resist underlayer film forming composition.
[0013] Means of solving the problem
[0014] The present invention includes the following contents.
[0015] [1] A composition for forming an EUV resist underlayer film, comprising a (meth)acrylic polymer and an organic solvent, wherein the (meth)acrylic polymer has a basic organic group substituted with a protecting group in its side chain, and the composition for forming an EUV resist underlayer film does not contain a polymer other than the (meth)acrylic polymer.
[0016] [2] The EUV resist underlayer film forming composition described in [1], wherein the organic group is an acyloxy group having an amino group substituted with a protecting group or an acyloxy group having a nitrogen-containing heterocyclic ring substituted with a protecting group.
[0017] [3] The EUV resist underlayer film-forming composition according to any one of [1] or [2], wherein the protecting group is selected from a tert-butoxycarbonyl group, a benzyloxycarbonyl group, a 9-fluorenylmethoxycarbonyl group, a 2,2,2-trichloroethoxycarbonyl group, and an allyloxycarbonyl group.
[0018] [4] The EUV resist underlayer film-forming composition according to any one of [1] to [3], wherein the (meth)acrylic polymer is a polymer having a unit structure represented by the following formula (1):
[0019]
[0020] In formula (1), R1 represents a hydrogen atom or a methyl group, L represents a divalent linking group, and X represents an acyloxy group having an amino group substituted with a protecting group or an acyloxy group having a nitrogen-containing heterocyclic ring substituted with a protecting group.
[0021] [5] The EUV resist underlayer film forming composition according to any one of [1] to [4], further comprising a cross-linking catalyst.
[0022] [6] The EUV resist underlayer film forming composition according to any one of [1] to [5], further comprising a crosslinking agent.
[0023] [7] An EUV resist underlayer film, characterized in that it is a fired product of a coating film formed from the EUV resist underlayer film forming composition according to any one of [1] to [6].
[0024] [8] A method for manufacturing a patterned substrate, comprising: a step of coating the EUV resist underlayer film forming composition described in any one of [1] to [6] on a semiconductor substrate and baking the coating to form an EUV resist underlayer film; a step of coating an EUV resist on the EUV resist underlayer film and baking the coating to form an EUV resist film; a step of exposing the semiconductor substrate coated with the EUV resist underlayer film and the EUV resist; and a step of developing and patterning the exposed EUV resist film.
[0025] [9] A method for manufacturing a semiconductor device, comprising:
[0026] A step of forming an EUV resist underlayer film formed from the EUV resist underlayer film-forming composition according to any one of [1] to [6] on a semiconductor substrate,
[0027] forming an EUV resist film on the EUV resist underlayer film,
[0028] A process of forming an EUV resist pattern by irradiating an EUV resist film with light or electron beams and then developing the film.
[0029] a step of etching the EUV resist underlayer film through the formed EUV resist pattern to form a patterned EUV resist underlayer film, and
[0030] A step of processing a semiconductor substrate using the patterned EUV resist underlayer film.
[0031] Effects of the Invention
[0032] The composition for forming an EUV resist underlayer film of the present invention contains a (meth)acrylic polymer and an organic solvent. The (meth)acrylic polymer has a basic organic group substituted with a protecting group in its side chain. It is characterized in that the composition for forming an EUV resist underlayer film does not contain polymers other than the (meth)acrylic polymer. By having a basic organic group substituted with a protecting group in the side chain of the (meth)acrylic polymer, the resist underlayer film manufactured using the composition of the present application generates an amino group on the film surface by baking after coating the composition to form a film. The adhesion to the resist is improved by this amino group. As a result, there is no so-called edge pulling or undercut in the resist shape, and a good rectangular resist pattern can be formed. By setting the composition for forming an EUV resist underlayer film for lithography to such a configuration, it is possible to suppress the deterioration of LWR and improve the sensitivity during the formation of a resist pattern. In particular, the composition for forming an EUV resist underlayer film of the present application shows a more remarkable effect when using an EUV exposure resist. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a scanning microscope photograph observed from above the EUV positive resist pattern of Example 1.
[0034] Figure 2 It is a scanning microscope photograph observed from above the EUV positive resist pattern of Comparative Example 1.
[0035] Figure 3 It is a scanning microscope photograph observed from above the EUV negative resist pattern of Example 1.
[0036] Figure 4 It is a scanning microscope photograph observed from above the EUV negative resist pattern of Comparative Example 1. DETAILED DESCRIPTION OF THE INVENTION
[0037] <Composition for Forming EUV Resist Underlayer Film>
[0038] The EUV resist underlayer film forming composition of the present application contains a (meth) acrylic polymer and an organic solvent, wherein the (meth) acrylic polymer has a basic organic group substituted by a protective group in its side chain, and the EUV resist underlayer film forming composition does not contain polymers other than the (meth) acrylic polymer. That is, the EUV resist underlayer film forming composition of the present application only contains the polymer having a basic organic group substituted by a protective group in the side chain of the (meth) acrylic polymer, and does not contain other polymers. The polymer contained in the EUV resist underlayer film forming composition of the present application is composed only of the polymer having a basic organic group substituted by a protective group in the side chain of the (meth) acrylic polymer.
[0039] The so-called (meth)acrylic polymer generally refers to a polymer having a unit structure derived from one or more monomers selected from (meth)acrylic acid, (meth)acrylic esters, and their derivatives. (Meth)acrylic polymers are particularly preferably vinyl polymers formed by reacting olefins or (meth)acrylic polymers formed by polymerizing (meth)acrylic ester compounds. It should be noted that in the present invention, (meth)acrylic ester compounds refer to both acrylic ester compounds and methacrylic ester compounds. For example, (meth)acrylic acid refers to acrylic acid and methacrylic acid. The above polymers can be manufactured by known methods. The above polymers can be chain-like or cross-linked, preferably chain-like.
[0040] Examples of the organic solvent contained in the EUV resist underlayer film-forming composition of the present invention include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, 4-methyl-2-pentanol, 2-hydroxyisobutyric acid methyl ester, 2-hydroxyisobutyric acid ethyl ester, ethoxyethyl acetate, 2-hydroxyethyl acetate, 3-methoxypropionic acid methyl ester, 3-methoxypropionic acid ethyl ester, 3-ethoxypropionic acid ethyl ester, 3-ethoxypropionic acid methyl ester, methyl pyruvic acid, ethyl pyruvic acid, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents can be used alone or in combination of two or more.
[0041] Among these solvents, preferred are propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, and cyclohexanone, etc. Propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate are particularly preferred.
[0042] The basic organic group mentioned in the present invention refers to a saturated or unsaturated group of a univalent group that contains carbon atoms, hydrogen atoms and heteroatoms (for example, at least one selected from the group consisting of oxygen atoms, sulfur atoms and nitrogen atoms), and shows basicity through the uneven electrons in the molecular structure caused by the heteroatoms. Preferably, the heteroatom is at least two selected from the group consisting of oxygen atoms, sulfur atoms and nitrogen atoms, or at least one selected from the group consisting of oxygen atoms and nitrogen atoms, more preferably oxygen atoms and nitrogen atoms. The organic group is preferably an acyloxy group having an amino group substituted by a protecting group or an acyloxy group having a nitrogen-containing heterocyclic ring substituted by a protecting group.
[0043] The protecting group mentioned here refers to a group that bonds to the above-mentioned amino group or nitrogen-containing heterocyclic ring to inhibit the change in the prescribed chemical reaction, but then detaches by prescribed means to play a role in restoring the original amino group or nitrogen-containing heterocyclic ring. Preferred protecting groups include carbamate protecting groups such as tert-butoxycarbonyl, benzyloxycarbonyl, 9-fluorenylmethoxycarbonyl, 2,2,2-trichloroethoxycarbonyl, and allyloxycarbonyl, sulfonamide protecting groups such as tosyl and nonylsulfonyl, imide protecting groups such as phthaloyl, and trifluoroacetyl. For example, when the above-mentioned protecting group is tert-butoxycarbonyl, an acyloxy group having an amino group protected by tert-butoxycarbonyl or an acyloxy group having a nitrogen-containing heterocyclic ring protected by tert-butoxycarbonyl is represented by the following formulas (a) to (j). Here, the acyloxy group is represented by "-OC(=O)-R" (R represents an organic group having an amino group protected by a tert-butoxycarbonyl group or an organic group having a nitrogen-containing heterocyclic ring protected by a tert-butoxycarbonyl group), and the tert-butoxycarbonyl group is sometimes abbreviated as "t-Boc" or "Boc".
[0044]
[0045] The protecting group is preferably selected from tert-butoxycarbonyl, benzyloxycarbonyl, 9-fluorenylmethoxycarbonyl, 2,2,2-trichloroethoxycarbonyl and allyloxycarbonyl, and among them, tert-butoxycarbonyl is preferred.
[0046] The (meth)acrylic polymer is preferably a polymer having a unit structure represented by the following formula (1).
[0047]
[0048] In formula (1), R1 represents a hydrogen atom or a methyl group, L represents a divalent linking group, and X represents an acyloxy group having an amino group substituted with a protecting group or an acyloxy group having a nitrogen-containing heterocyclic ring substituted with a protecting group.
[0049] The (meth)acrylic polymer of the present invention preferably has a structural unit represented by the above formula (1). The above (meth)acrylic polymer may be a homopolymer obtained by polymerizing one monomer component or a copolymer obtained by polymerizing two or more monomer components, and is preferably a homopolymer.
[0050] The (meth)acrylic polymer of the present invention may contain one or more polymers having a basic organic group substituted with a protecting group in a side chain of the (meth)acrylic polymer, preferably two or less, and most preferably only one.
[0051] In the above formula (1), the divalent linking group represented by L is not particularly limited, and examples thereof include -C(=O)OR2- group and phenylene group. R2 of the -C(=O)OR2- group represents an alkylene group having 1 to 10 carbon atoms, and a portion of the hydrogen atoms of the alkylene group may be substituted by hydroxyl groups or halogen atoms.
[0052] Examples of the alkylene group having 1 to 10 carbon atoms include methylene, ethylene, n-propylene, isopropylene, cyclopropylene, n-butylene, isobutylene, sec-butylene, tert-butylene, cyclobutylene, 1-methyl-cyclopropylene, 2-methyl-cyclopropylene, n-pentylene, 1-methyl-n-butylene, 2-methyl-n-butylene, 3-methyl-n-butylene, 1,1-dimethyl-n-propylene, 1,2-dimethyl-n-propylene, 2,2-dimethyl-n-propylene, 1-ethyl-n-propylene, cyclopentylene, 1-methyl-cyclobutylene, 2-methyl-cyclopropylene, Butyl, 3-methyl-cyclobutylene, 1,2-dimethyl-cyclopropylene, 2,3-dimethyl-cyclopropylene, 1-ethyl-cyclopropylene, 2-ethyl-cyclopropylene, n-hexylene, 1-methyl-n-pentylene, 2-methyl-n-pentylene, 3-methyl-n-pentylene, 4-methyl-n-pentylene, 1,1-dimethyl-n-butylene, 1,2-dimethyl-n-butylene, 1,3-dimethyl-n-butylene, 2,2-dimethyl-n-butylene, 2,3-dimethyl-n-butylene, 3,3-dimethyl-n-butylene, 1-ethyl-n-butylene 1-ethyl-1-methyl-n-propylene, 1-ethyl-2-methyl-n-propylene, cyclohexylene, 1-methyl-cyclopentylidene, 2-methyl-cyclopentylidene, 3-methyl-cyclopentylidene, 1-ethyl-cyclobutylene, 2-ethyl-cyclobutylene, 3-ethyl-cyclobutylene, 1,2-dimethyl-cyclobutylene, 1,3-dimethyl-cyclobutylene, 2,2-dimethyl-cyclobutylene, 2,3-dimethyl-cyclobutylene, 2,4-dimethyl ...pentylidene, 1-methyl-cyclopentylidene, 2-methyl-cyclopentylidene, 3-methyl-cyclopentylidene, 1-ethyl-cyclobutylene, 2-ethyl-cyclobutylene, 3-ethyl-cyclobutylene, 1,2-dimethyl-cyclobutylene, 1,3-dimethyl-cyclobutylene, 2,2-dimethyl-cyclobutylene, 2,3-dimethyl-cyclobutylene, 2,4-dimethyl- Methyl-cyclobutylene, 3,3-dimethyl-cyclobutylene, 1-n-propyl-cyclopropylene, 2-n-propyl-cyclopropylene, 1-isopropyl-cyclopropylene, 2-isopropyl-cyclopropylene, 1,2,2-trimethyl-cyclopropylene, 1,2,3-trimethyl-cyclopropylene, 2,2,3-trimethyl-cyclopropylene, 1-ethyl-2-methyl-cyclopropylene, 2-ethyl-1-methyl-cyclopropylene, 2-ethyl-2-methyl-cyclopropylene, 2-ethyl-3-methyl-cyclopropylene, n-heptylene, n-octylene, n-nonylene, or n-decylene.
[0053] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.
[0054] The meth(acrylic) polymer having the structural unit represented by the above formula (1) can be obtained, for example, by reacting a (meth)acrylic polymer having an epoxy group at the terminal with a monomer reactive with the epoxy group. Examples of such monomers include N-(tert-butoxycarbonyl)glycine, N-(tert-butoxycarbonyl)alanine, N-(tert-butoxycarbonyl)valine, N-(tert-butoxycarbonyl)leucine, N-(tert-butoxycarbonyl)isoleucine, N-(tert-butoxycarbonyl)methionine, N-(tert-butoxycarbonyl)serine, N-(tert-butoxycarbonyl)threonine, N-(tert-butoxycarbonyl)proline, N-(tert-butoxycarbonyl)histidine, N-(tert-butoxycarbonyl)phenylalanine, N-(tert-butoxycarbonyl)tyrosine, N-(tert-butoxycarbonyl)tryptophan, O-benzyl-N-(tert-butoxycarbonyl)serine, 4-benzyl N-(tert-butoxycarbonyl)aspartate, 5-benzyl N-(tert-butoxycarbonyl)glutamate. Esters, N-(tert-butoxycarbonyl)asparagine, N-(tert-butoxycarbonyl)-S-benzylcysteine, N-(tert-butoxycarbonyl)-O-benzylthreonine, N-(tert-butoxycarbonyl)-O-benzyltyrosine, N-(tert-butoxycarbonyl)-O-tert-butyltyrosine, N-(tert-butoxycarbonyl)-N-benzyloxycarbonyllysine, N-(tert-butoxycarbonyl)-3,4-difluorophenylalanine, N-(tert-butoxycarbonyl)-4-fluorophenylalanine, N-(tert-butoxycarbonyl)-N1-formyltryptophan, N-(tert-butoxycarbonyl)glutamine, N-(tert-butoxycarbonyl)-4-hydroxyproline, N-(tert-butoxycarbonyl)-4-nitrophenylalanine, N-(tert-butoxycarbonyl)-p-toluenesulfonylhistidine,
[0055] N-(Benzyloxycarbonyl)glycine, N-(Benzyloxycarbonyl)alanine, N-(Benzyloxycarbonyl)valine, N-(Benzyloxycarbonyl)leucine, N-(Benzyloxycarbonyl)isoleucine, N-(Benzyloxycarbonyl)methionine, N-(Benzyloxycarbonyl)serine, N-(Benzyloxycarbonyl)threonine, N-(Benzyloxycarbonyl)proline, N-(Benzyloxycarbonyl)histidine, N-(Benzyloxycarbonyl)phenylalanine, N-(Benzyloxycarbonyl)tyrosine, N-(Benzyloxycarbonyl)tryptophan, O-benzyl-N-(Benzyloxycarbonyl)serine, 4-benzyl N-(Benzyloxycarbonyl)aspartate, 5-benzyl N-(Benzyloxycarbonyl)glutamate, N-(Benzyloxycarbonyl) N-(Benzyloxycarbonyl)-asparagine, N-(Benzyloxycarbonyl)-S-benzylcysteine, N-(Benzyloxycarbonyl)-O-benzylthreonine, N-(Benzyloxycarbonyl)-O-benzyltyrosine, N-(Benzyloxycarbonyl)-O-tert-butyltyrosine, N-(Benzyloxycarbonyl)-N-benzyloxycarbonyllysine, N-(Benzyloxycarbonyl)-3,4-difluorophenylalanine, N-(Benzyloxycarbonyl)-4-fluorophenylalanine, N-(Benzyloxycarbonyl)-N1-formyltryptophan, N-(Benzyloxycarbonyl)glutamine, N-(Benzyloxycarbonyl)-4-hydroxyproline, N-(Benzyloxycarbonyl)-4-nitrophenylalanine, N-(Benzyloxycarbonyl)-p-toluenesulfonylhistidine,
[0056] N-(9-fluorenylmethoxycarbonyl)glycine, N-(9-fluorenylmethoxycarbonyl)alanine, N-(9-fluorenylmethoxycarbonyl)valine, N-(9-fluorenylmethoxycarbonyl)leucine, N-(9-fluorenylmethoxycarbonyl)isoleucine, N-(9-fluorenylmethoxycarbonyl)methionine, N-(9-fluorenylmethoxycarbonyl)serine, N-(9-fluorenylmethoxycarbonyl)threonine, N-(9-fluorenylmethoxycarbonyl) methoxycarbonyl) proline, N-(9-fluorenylmethoxycarbonyl)-histidine, N-(9-fluorenylmethoxycarbonyl)phenylalanine, N-(9-fluorenylmethoxycarbonyl)tyrosine, N-(9-fluorenylmethoxycarbonyl)tryptophan, O-benzyl-N-(9-fluorenylmethoxycarbonyl)serine, N-(9-fluorenylmethoxycarbonyl)aspartic acid 4-benzyl ester, N-(9-fluorenylmethoxycarbonyl)glutamic acid 5-benzyl ester, N -(9-fluorenylmethoxycarbonyl)asparagine, N-(9-fluorenylmethoxycarbonyl)-S-benzylcysteine, N-(9-fluorenylmethoxycarbonyl)-O-benzylthreonine, N-(9-fluorenylmethoxycarbonyl)-O-benzyltyrosine, N-(9-fluorenylmethoxycarbonyl)-O-tert-butyltyrosine, N-(9-fluorenylmethoxycarbonyl)-N-benzyloxycarbonyllysine, N-(9-fluorenylmethoxycarbonyl)-3 ,4-difluorophenylalanine, N-(9-fluorenylmethoxycarbonyl)-4-fluorophenylalanine, N-(9-fluorenylmethoxycarbonyl)-N1-formyltryptophan, N-(9-fluorenylmethoxycarbonyl)glutamine, N-(9-fluorenylmethoxycarbonyl)-4-hydroxyproline, N-(9-fluorenylmethoxycarbonyl)-4-nitrophenylalanine, N-(9-fluorenylmethoxycarbonyl)-p-toluenesulfonylhistidine,
[0057] N-(2,2,2-trichloroethoxycarbonyl)glycine, N-(2,2,2-trichloroethoxycarbonyl)alanine, N-(2,2,2-trichloroethoxycarbonyl)valine, N-(2,2,2-trichloroethoxycarbonyl)leucine, N-(2,2,2-trichloroethoxycarbonyl)isoleucine, N-(2,2,2-trichloroethoxycarbonyl)methionine, N-(2,2,2-trichloroethoxycarbonyl)serine, N-(2,2,2-trichloroethoxycarbonyl)threonine, N-(2 ,2,2-trichloroethoxycarbonyl)proline, N-(2,2,2-trichloroethoxycarbonyl)histidine, N-(2,2,2-trichloroethoxycarbonyl)phenylalanine, N-(2,2,2-trichloroethoxycarbonyl)tyrosine, N-(2,2,2-trichloroethoxycarbonyl)tryptophan, O-benzyl-N-(2,2,2-trichloroethoxycarbonyl)serine, N-(2,2,2-trichloroethoxycarbonyl)aspartic acid 4-benzyl ester, N-(2,2,2-trichloroethoxycarbonyl)glutamic acid 5-benzyl ester, N-(2,2,2-trichloroethoxycarbonyl) asparagine, N-(2,2,2-trichloroethoxycarbonyl)-S-benzylcysteine, N-(2,2,2-trichloroethoxycarbonyl)-O-benzylthreonine, N-(2,2,2-trichloroethoxycarbonyl)-O-benzyltyrosine, N-(2,2,2-trichloroethoxycarbonyl)-O-tert-butyltyrosine, N-(2,2,2-trichloroethoxycarbonyl)-N-benzyloxycarbonyllysine, N-(2,2,2-trichloroethoxycarbonyl) N-(2,2,2-trichloroethoxycarbonyl)-3,4-difluorophenylalanine, N-(2,2,2-trichloroethoxycarbonyl)-4-fluorophenylalanine, N-(2,2,2-trichloroethoxycarbonyl)-N1-formyltryptophan, N-(2,2,2-trichloroethoxycarbonyl)glutamine, N-(2,2,2-trichloroethoxycarbonyl)-4-hydroxyproline, N-(2,2,2-trichloroethoxycarbonyl)-4-nitrophenylalanine, N-(2,2,2-trichloroethoxycarbonyl)-p-toluenesulfonylhistidine,
[0058] N-(allyloxycarbonyl)glycine, N-(allyloxycarbonyl)alanine, N-(allyloxycarbonyl)valine, N-(allyloxycarbonyl)leucine, N-(allyloxycarbonyl)isoleucine, N-(allyloxycarbonyl)methionine, N-(allyloxycarbonyl)serine, N-(allyloxycarbonyl)threonine, N-(allyloxycarbonyl)proline, N-(allyloxycarbonyl)-histidine, N-(allyloxycarbonyl)phenylalanine, N-(allyloxycarbonyl)tyrosine, N-(allyloxycarbonyl)tryptophan, O-benzyl-N-(allyloxycarbonyl)serine, 4-benzyl N-(allyloxycarbonyl)aspartate, 5-benzyl N-(allyloxycarbonyl)glutamate, N-(allyloxycarbonyl) N-(allyloxycarbonyl)-asparagine, N-(allyloxycarbonyl)-S-benzylcysteine, N-(allyloxycarbonyl)-O-benzylthreonine, N-(allyloxycarbonyl)-O-benzyltyrosine, N-(allyloxycarbonyl)-O-tert-butyltyrosine, N-(allyloxycarbonyl)-N-benzyloxycarbonyllysine, N-(allyloxycarbonyl)-3,4-difluorophenylalanine, N-(allyloxycarbonyl)-4-fluorophenylalanine, N-(allyloxycarbonyl)-N1-formyltryptophan, N-(allyloxycarbonyl)glutamine, N-(allyloxycarbonyl)-4-hydroxyproline, N-(allyloxycarbonyl)-4-nitrophenylalanine, N-(allyloxycarbonyl)-p-toluenesulfonylhistidine.
[0059] Among them, preferred are N-(tert-butoxycarbonyl)glycine, N-(tert-butoxycarbonyl)alanine, N-(tert-butoxycarbonyl)leucine, N-(tert-butoxycarbonyl)methionine, N-(tert-butoxycarbonyl)serine, N-(tert-butoxycarbonyl)proline, and N-(tert-butoxycarbonyl)-4-hydroxyproline.
[0060] The weight average molecular weight of the (meth)acrylic polymer is, for example, 2,000 to 50,000. The weight average molecular weight can be measured by, for example, gel permeation chromatography as described in the following Examples.
[0061] The content ratio of the (meth)acrylic polymer relative to the entire resist underlayer film-forming composition is 0.01 to 1.00 wt %, preferably 0.01 to 0.90 wt %, preferably 0.01 to 0.80 wt %, preferably 0.01 to 0.70 wt %, preferably 0.01 to 0.60 wt %, preferably 0.01 to 0.50 wt %, preferably 0.01 to 0.49 wt %, preferably 0.01 to 0.45 wt %, preferably 0.01 to 0.4 wt %, preferably 0.01 to 0.3 wt %, and preferably 0.01 to 0.2 wt %.
[0062] Examples of the crosslinking catalyst (curing catalyst) included as an optional component in the resist underlayer film-forming composition of the present invention include sulfonic acid compounds and carboxylic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate (pyridinium p-toluenesulfonate), pyridinium p-hydroxybenzenesulfonate (pyridinium p-phenolsulfonate), pyridinium trifluoromethanesulfonate, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzene disulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid. When the crosslinking catalyst is used, the content of the crosslinking catalyst is, for example, 0.1% to 50% by mass, preferably 1% to 30% by mass, relative to the crosslinking agent. Examples of the crosslinking agent included as an optional component in the resist underlayer film-forming composition of the present invention include hexamethoxymethylmelamine, tetramethoxymethylbenzoguanamine, 1,3,4,6-tetrakis(methoxymethyl)glycoluril (tetramethoxymethylglycoluril) (POWDERLINK (registered trademark) 1174), 1,3,4,6-tetrakis(butoxymethyl)glycoluril, 1,3,4,6-tetrakis(hydroxymethyl)glycoluril, 1,3-bis(hydroxymethyl)urea, 1,3,3,3-tetrakis(butoxymethyl)urea, and 1,3,3,3-tetrakis(methoxymethyl)urea. When the crosslinking agent is used, the content ratio of the crosslinking agent is, for example, 1% to 50% by mass, preferably 5% to 30% by mass, relative to the polymer.
[0063] In the composition for forming an underlayer film of a resist of the present invention, in order to prevent the generation of pinholes, streaks, etc. and further improve the coating property against surface unevenness, a surfactant may be further added. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl aryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; and other nonionic surfactants. Fluorine-containing surfactants such as EFtop EF301, EF303, EF352 (manufactured by Tocem Products Co., Ltd., trade name), Megafac F171, F173, R-30 (manufactured by Dainippon Ink and Chemicals, Inc., trade name), Fluorad FC430, FC431 (manufactured by Sumitomo 3M Limited, trade name), Asahi Guard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, SC106 (manufactured by Asahi Glass Co., Ltd., trade name); and silicone oxide polymers such as KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The blending amount of these surfactants is usually 2.0% by mass or less, preferably 1.0% by mass or less, based on the total solids of the composition for forming an underlayer film of a resist of the present invention. These surfactants may be added alone, or may be added in combination of two or more kinds.
[0064] <EUV Resist Underlayer Film, Method for Manufacturing EUV Resist Underlayer Film>
[0065] The underlayer film of a resist according to the present invention can be manufactured by coating the above-described composition for forming an underlayer film of a resist on a semiconductor substrate and firing it.
[0066] Examples of the semiconductor substrate for coating the composition for forming an underlayer film of a resist of the present invention include silicon wafers, germanium wafers, and compound semiconductor wafers such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.
[0067] When a semiconductor substrate having an inorganic film formed on the surface is used, the inorganic film is formed by, for example, ALD (atomic layer deposition) method, CVD (chemical vapor deposition) method, reactive sputtering method, ion plating method, vacuum evaporation method, spin coating method (spin-on glass: SOG). Examples of the inorganic film include polycrystalline silicon film, silicon oxide film, silicon nitride film, BPSG (Boro-Phospho Silicate Glass) film, titanium nitride film, titanium oxynitride film, tungsten film, gallium nitride film, and gallium arsenide film.
[0068] On such a semiconductor substrate, the resist underlayer film forming composition of the present invention is applied by a suitable coating method such as a spin coater or a coater. Then, a heating means such as a hot plate is used to bake to form a resist underlayer film. As baking conditions, a baking temperature of 100°C to 400°C and a baking time of 0.3 minutes to 60 minutes are appropriately selected. Preferably, the baking temperature is 120°C to 350°C and the baking time is 0.5 minutes to 30 minutes, and more preferably, the baking temperature is 150°C to 300°C and the baking time is 0.8 minutes to 10 minutes.
[0069] The thickness of the EUV resist lower layer film to be formed is, for example, 0.001 μm (1 nm) to 10 μm, 0.002 μm (2 nm) to 1 μm, 0.005 μm (5 nm) to 0.5 μm (500 nm), 0.001 μm (1 nm) to 0.05 μm (50 nm), 0.002 μm (2 nm) to 0.05 μm (50 nm), 0.003 μm (1 nm) to 0.05 μm (50 nm), )~0.05μm(50nm), 0.004μm(4nm)~0.05μm(50nm), 0.005μm(5nm)~0.05μm(50nm), 0.003μm(3nm)~0.03μm(30nm), 0.003μm(3nm)~0.02μm(20nm), 0.005μm(5nm)~0.02μm(20nm). When the temperature during baking is lower than the above range, crosslinking sometimes becomes insufficient. On the other hand, when the temperature during baking is higher than the above range, the resist lower film sometimes decomposes due to heat.
[0070] <Method for Manufacturing Patterned Substrate, Method for Manufacturing Semiconductor Device>
[0071] The method for manufacturing a patterned substrate is carried out through the following steps. Usually, a photoresist layer is formed on an EUV resist underlayer film for manufacturing. As a photoresist formed by coating and firing on the EUV resist underlayer film by a method known per se, there is no particular limitation as long as it is a photoresist that is sensitive to the light used in exposure. Both negative photoresists and positive photoresists can be used. There are positive photoresists composed of novolac resin and 1,2-naphthoquinone diazosulfonic acid ester, chemically amplified photoresists composed of a binder having a group that increases the alkali dissolution rate by acid decomposition and a photoacid generator, chemically amplified photoresists composed of a low molecular weight compound that increases the alkali dissolution rate of the photoresist by acid decomposition, an alkali-soluble binder, and a photoacid generator, chemically amplified photoresists composed of a binder having a group that increases the alkali dissolution rate by acid decomposition, a low molecular weight compound that increases the alkali dissolution rate of the photoresist by acid decomposition, and a photoacid generator, and resists containing metal elements, etc. For example, JSR Corporation's product name V146G, Shipley's product name APEX-E, Sumitomo Chemical's product name PAR710, Shin-Etsu Chemical's product names AR2772 and SEPR430, etc. can be cited. In addition, for example, fluorine atom-containing polymer photoresists such as those described in Proc. SPIE, Vol. 3999, 330-334 (2000), Proc. SPIE, Vol. 3999, 357-364 (2000), and Proc. SPIE, Vol. 3999, 365-374 (2000) can be cited.
[0072] In addition, WO2019 / 188595, WO2019 / 187881, WO2019 / 187803, WO2019 / 167737, WO2019 / 167725, WO2019 / 187445, WO2019 / 167419, WO2019 / 123842, WO2019 / 054282, WO2019 / 058945, WO2019 / 058890, WO2019 / 039290, WO2019 / 044259, WO2019 / 044231, WO2019 / 026549, WO2018 / 193954, WO2019 / 172054, W O2019 / 021975, WO2018 / 230334, WO2018 / 194123, Japanese Special Opening 2018-180525, WO2018 / 190088, Japanese Special Opening 2018-070596, Japanese Special Opening 2018-028090, Japanese Special Opening 2016-153409, Japanese Special Opening 2016-130240, Japanese Special Opening 2016-108325, Japanese Special Opening 2016-047920, Japanese Special Opening 2016-035570, Japan This special issue 2016-035567, Japan’s special issue 2016-035565, Japan’s special issue 2019-101417, Japan’s special issue 2019-117373 , Japanese Special Opening 2019-052294, Japanese Special Opening 2019-008280, Japanese Special Opening 2019-008279, Japanese Special Opening 2019-003176, Japanese Special Opening 2019-003175, Japanese Special Opening 2018-197853, Japanese Special Opening 2019-191298, Japanese Special Opening 2019-0 61217, Japanese Special Opening 2018-045152, Japanese Special Opening 2018-022039, Japanese Special Opening 2016-090441, Japanese Special Opening 2015-10878, Japanese Special Opening 2012-168279, Japanese Special Opening 2012-022621, Japanese Special Opening 2012-022258, Japanese Special Opening 20 11-043749, Japanese Patent Application Laid-Open No. 2010-181857, Japanese Patent Application Laid-Open No. 2010-128369, WO2018 / 031896, Japanese Patent Application Laid-Open No. 2019-113855, WO2017 / 156388, WO2017 / 066319, Japanese Patent Application Laid-Open No. 2018-41099, WO2016 / 065120, WO2015 / 026482, Japanese Patent Application Laid-Open No. 2016-29498, Japanese Patent Application Laid-Open No. 2011-253185, etc., so-called resist compositions, radiation-sensitive resin compositions, high-resolution patterning compositions based on organic metal solutions, and metal-containing resist compositions, but are not limited thereto.
[0073] Examples of the resist composition include the following compositions.
[0074] A photosensitive or radiation-sensitive resin composition comprising a resin A and a compound represented by the general formula (1), wherein the resin A comprises a repeating unit having an acid-decomposable group in which a polar group is protected by a protecting group that is detached by the action of an acid.
[0075]
[0076] In the general formula (11), m represents an integer of 1-6.
[0077] R1 and R2 each independently represent a fluorine atom or a perfluoroalkyl group.
[0078] L1 represents -O-, -S-, -COO-, -SO2- or -SO3-.
[0079] L2 represents an alkylene group which may have a substituent or a single bond.
[0080] W1 represents a cyclic organic group which may have a substituent.
[0081] M + Represents a cation.
[0082] A composition for forming a metal-containing film for extreme ultraviolet or electron beam lithography, comprising a compound having a metal-oxygen covalent bond and a solvent, wherein the metal element constituting the compound belongs to the third to seventh periods of the third to fifteenth groups of the periodic table.
[0083] A radiation-sensitive resin composition containing a polymer and an acid generator, wherein the polymer has a first structural unit represented by the following formula (1) and a second structural unit containing an acid-dissociable group represented by the following formula (2).
[0084]
[0085] In formula (21), Ar is a group obtained by removing (n+1) hydrogen atoms from an aromatic hydrocarbon having 6 to 20 carbon atoms. 1 is a hydroxyl group, a mercapto group or a monovalent organic group having 1 to 20 carbon atoms. n is an integer of 0 to 11. When n is 2 or more, multiple R 1 Same or different, R 2 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group.
[0086] In formula (22), R 3 is a monovalent group having 1 to 20 carbon atoms and containing the acid dissociable group. Z is a single bond, an oxygen atom or a sulfur atom. 4 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group.
[0087] A resist composition comprising a resin (A1) and an acid generator, wherein the resin (A1) comprises a structural unit having a cyclic carbonate structure, a structural unit represented by formula (II), and a structural unit having an acid-labile group.
[0088]
[0089] In formula (II), R 2 represents an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, a hydrogen atom or a halogen atom, and X 1 Represents a single bond, -CO-O-* or -CO-NR 4 -*, *, represents the bond with -Ar, R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and Ar represents an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have one or more groups selected from the group consisting of a hydroxyl group and a carboxyl group.
[0090] A resist composition that generates acid by exposure and changes its solubility in a developer due to the action of the acid, wherein:
[0091] The invention comprises a base component (A) whose solubility in a developer changes due to the action of an acid and a fluorine additive component (F) which is decomposable in an alkali developer,
[0092] The fluorine additive component (F) contains a fluorine resin component (F1) having a structural unit (f1) containing an alkali dissociable group and a structural unit (f2) containing a group represented by the following general formula (f2-r-1).
[0093]
[0094] In formula (f2-r-1), Rf 21 Each is independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxyl group, a hydroxyalkyl group or a cyano group. n" is an integer of 0 to 2, and * is a bond.
[0095] The resist composition described above, wherein the structural unit (f1) comprises a structural unit represented by the following general formula (f1-1) or a structural unit represented by the following general formula (f1-2),
[0096]
[0097] In formula (f1-1) and (f1-2), R is independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogenated alkyl group having 1 to 5 carbon atoms. X is a divalent linking group having no acid dissociable site. aryl is a divalent aromatic cyclic group which may have a substituent. 01is a single bond or a divalent linking group. 2 Each independently is an organic group having a fluorine atom.
[0098] Examples of the resist film include the following films.
[0099] A resist film includes a base resin including a repeating unit represented by the following formula (a1) and / or a repeating unit represented by the following formula (a2), and a repeating unit that generates an acid bonded to a polymer main chain by exposure.
[0100]
[0101] In formula (a1) and (a2), R A are each independently a hydrogen atom or a methyl group, R 1 and R 2 Each is independently a tertiary alkyl group having 4 to 6 carbon atoms. 3 Each independently represents a fluorine atom or a methyl group. m represents an integer from 0 to 4. 1 X is a single bond, a phenylene group or a naphthylene group, or a linking group having 1 to 12 carbon atoms and containing at least one selected from an ester bond, a lactone ring, a phenylene group and a naphthylene group. 2 It is a single bond, an ester bond or an amide bond.
[0102] Examples of resist materials include the following.
[0103] A resist material comprising a polymer having a repeating unit represented by the following formula (a1) or (a2).
[0104]
[0105] In formula (b1) and (b2), R A X is a hydrogen atom or a methyl group. 1 is a single bond or an ester group. 2 is a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms or an arylene group having 6 to 10 carbon atoms, and a part of the methylene group constituting the alkylene group may be substituted with an ether group, an ester group or a lactone ring-containing group, and X 2 At least one hydrogen atom contained in is replaced by a bromine atom. 3 Rf is a single bond, an ether group, an ester group, or a linear, branched, or cyclic alkylene group having 1 to 12 carbon atoms, and a portion of the methylene groups constituting the alkylene group may be substituted with an ether group or an ester group. 1 ~Rf 4 are independently a hydrogen atom, a fluorine atom or a trifluoromethyl group, and at least one of them is a fluorine atom or a trifluoromethyl group. 1 and Rf 2 Can combine to form a carbonyl group. 1~R 5 Each is independently a linear, branched or cyclic alkyl group having 1 to 12 carbon atoms, a linear, branched or cyclic alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or an aryloxyalkyl group having 7 to 12 carbon atoms, and a part or all of the hydrogen atoms of these groups may be substituted with a hydroxyl group, a carboxyl group, a halogen atom, an oxo group, a cyano group, an amide group, a nitro group, a sultone group, a sulfone group or a sulfonium salt-containing group, and a part of the methylene groups constituting these groups may be substituted with an ether group, an ester group, a carbonyl group, a carbonate group or a sulfonate group. In addition, R 1 With R 2 They may bond to form a ring together with the sulfur atom to which they are bonded.
[0106] A resist material comprising a base resin comprising a polymer containing a repeating unit represented by the following formula (a),
[0107]
[0108] In formula (a), R A is a hydrogen atom or a methyl group. 1 is a hydrogen atom or an acid-labile group, R 2 is a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or a halogen atom other than bromine. 1 X is a single bond or a phenylene group, or a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms which may contain an ester group or a lactone ring. 2 is -O-, -O-CH2- or -NH-. m is an integer of 1 to 4, and n is an integer of 0 to 3.
[0109] Examples of the metal-containing resist composition include the following compositions.
[0110] A coating comprising a metal oxo-hydroxyl network having organic ligands via metal-carbon bonds and / or metal-carboxylate bonds.
[0111] Inorganic oxygen / hydroxyl based compositions.
[0112] Examples of the coating solution include the following solutions.
[0113] A coating solution, comprising: an organic solvent; a first organometallic composition represented by the formula RzSnO(2-(z / 2)-(x / 2))(OH)x (where 0 < z ≤ 2 and 0 < (z + x) ≤ 4), the formula R’nSnX4-n (where n = 1 or 2), or a mixture thereof, where R and R’ are independently hydrocarbyl groups having 1 to 31 carbon atoms, and X is a ligand having a hydrolyzable bond to Sn or a combination thereof; and a hydrolyzable metal compound represented by the formula MX’v (where M is a metal selected from Groups 2 to 16 of the Periodic Table, v is a number from 2 to 6, and X’ is a ligand having a hydrolyzable M-X bond or a combination thereof).
[0114] A coating solution, comprising an organic solvent and a first organometallic compound represented by the formula RSnO(3 / 2 - x / 2)(OH)x (where 0 < x < 3), the solution containing from about 0.0025 M to about 1.5 M of tin, and R being an alkyl or cycloalkyl group having 3 to 31 carbon atoms, the alkyl or cycloalkyl group being bonded to tin at a secondary or tertiary carbon atom.
[0115] An aqueous inorganic patterning precursor solution, comprising a mixture of water, a metal lower oxide cation, a polyatomic inorganic anion, and a radiation-sensitive ligand containing a peroxide group.
[0116] Exposure is carried out through a mask (intermediate mask) for forming a prescribed pattern, for example, using i-ray, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet), or EB (electron beam), but the composition for forming an underlayer film of the resist in the present application is preferably suitable for EUV (extreme ultraviolet) exposure. In development, an alkali developer is used, and it is appropriately selected from a development temperature of 5°C to 50°C and a development time of 10 seconds to 300 seconds. As the alkali developer, for example, inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and ammonia water can be used, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-butylamine, tertiary amines such as triethylamine and methyldiethylamine, alkanolamines such as dimethylethanolamine and triethanolamine, quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline, and aqueous solutions of bases such as cyclic amines such as pyrrole and piperidine can be used. Moreover, an appropriate amount of alcohols such as isopropanol and surfactants such as non-ionic surfactants can be added to the aqueous solutions of the above bases for use. Among them, the preferred developer is a quaternary ammonium salt, and more preferably tetramethylammonium hydroxide and choline. Moreover, surfactants and the like can also be added to these developers. It is also possible to use the following method: as an alternative to the alkaline developer, development is carried out using an organic solvent such as butyl acetate, and the part where the alkali dissolution rate of the photoresist is not increased is developed. Through the above processes, a substrate with the resist patterned as described above can be manufactured.
[0117] Next, the resist underlayer film is dry-etched using the formed resist pattern as a mask. At this time, if the inorganic film is formed on the surface of the semiconductor substrate to be used, the surface of the inorganic film is exposed, and if the inorganic film is not formed on the surface of the semiconductor substrate to be used, the surface of the semiconductor substrate is exposed. Then, the substrate is processed by a method known per se (dry etching method, etc.) to manufacture a semiconductor device.
[0118] Example
[0119] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0120] The weight average molecular weight of the polymers shown in Synthesis Example 1 and Comparative Synthesis Example 1 in the present specification is the measurement result based on gel permeation chromatography (hereinafter referred to as GPC). A GPC apparatus manufactured by Tosoh Corporation was used for the measurement, and the measurement conditions and the like were as follows.
[0121] GPC columns: Shodex KF803L, Shodex KF802, Shodex KF801 (registered trademark) (Showa Denko K.K.)
[0122] Column temperature: 40°C
[0123] Solvent: Tetrahydrofuran (THF)
[0124] Flow rate: 1.0ml / min
[0125] Standard sample: Polystyrene (manufactured by Tosoh Corporation)
[0126] <Synthesis example 1>
[0127] 15.00 g of poly(glycidyl methacrylate) (manufactured by Maruzen Petrochemical Co., Ltd.), 22.78 g of N-(tert-butoxycarbonyl)-β-alanine (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.56 g of ethyltriphenylphosphonium bromide (manufactured by ACROSS Co., Ltd.) were added to 100.72 g of propylene glycol monomethyl ether acetate and dissolved. After nitrogen substitution in the reaction vessel, the reaction was carried out at 80°C for 24 hours to obtain a polymer solution. The polymer solution did not become turbid even when cooled to room temperature, and had good solubility in propylene glycol monomethyl ether acetate. When GPC analysis was performed, the polymer in the obtained solution had a weight average molecular weight of 15,000 in terms of standard polystyrene, and a dispersity of 1.68. The polymer obtained in this synthesis example has a structural unit represented by the following formula (1a).
[0128]
[0129] <Comparative Synthesis Example 1>
[0130] 10.00 g of tert-butyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), 6.10 g of 2-hydroxyethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.96 g of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to 73.00 g of propylene glycol monomethyl ether and dissolved. After nitrogen substitution in the reaction container, the reaction was carried out at 80°C for 24 hours to obtain a polymer solution. The polymer solution did not become turbid even when cooled to room temperature, and had good solubility in propylene glycol monomethyl ether. When GPC analysis was performed, the polymer in the obtained solution had a weight average molecular weight of 3690 in terms of standard polystyrene, and a dispersity of 2.25. The polymer obtained in this synthesis example has structural units represented by the following formulas (1b) and (2b).
[0131]
[0132] <Example 1>
[0133] 0.11 g of tetramethoxymethyl glycoluril (manufactured by Nippon Cytec Industries, Ltd.) and 0.012 g of pyridinium p-phenolsulfonate (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed with 3.12 g of the polymer solution containing 0.047 g of the polymer obtained in Synthesis Example 1, and 263.41 g of propylene glycol monomethyl ether and 29.89 g of propylene glycol monomethyl ether acetate were added and dissolved. The mixture was then filtered using a polyethylene microfilter having a pore size of 0.05 μm to prepare a resist underlayer film-forming composition for lithography.
[0134] <Comparative Example 1>
[0135] 0.11 g of tetramethoxymethyl glycoluril (manufactured by Nippon Cytec Industries, Ltd.) and 0.012 g of pyridinium p-phenolsulfonate (manufactured by Tokyo Chemical Industry, Ltd.) were mixed with 3.12 g of the polymer solution containing 0.047 g of the polymer obtained in Comparative Synthesis Example 1, and 263.41 g of propylene glycol monomethyl ether and 29.89 g of propylene glycol monomethyl ether acetate were added and dissolved. The mixture was then filtered using a polyethylene microfilter having a pore size of 0.05 μm to prepare a resist underlayer film-forming composition for lithography.
[0136] [Solubility test of photoresist solvent]
[0137] The resist underlayer film-forming compositions of Example 1 and Comparative Example 1 were applied to a silicon wafer as a semiconductor substrate using a spin coater. The silicon wafer was placed on a hot plate and baked at 215° C. for 1 minute to form a resist underlayer film (film thickness 5 nm). These resist underlayer films were immersed in ethyl lactate and propylene glycol monomethyl ether, which are solvents used in photoresists, and it was confirmed that they were insoluble in these solvents.
[0138] [Formation of positive resist pattern using electron beam drawing apparatus]
[0139] On the film, the compositions for forming the resist underlayer film of Example 1 and Comparative Example 1 were respectively coated on a silicon wafer using a spin coater. The silicon wafer was baked on a hot plate at 215°C for 60 seconds to obtain a resist underlayer film with a film thickness of 5 nm. A positive resist solution for EUV was spin-coated on the resist underlayer film and heated at 100°C for 60 seconds to form an EUV resist film. For the resist film, an electron beam drawing device (ELS-G130) was used to expose it under specified conditions. After exposure, it was baked (PEB) at 110°C for 60 seconds, cooled to room temperature on a cooling plate, and developed with an alkaline developer (2.38% TMAH) to form a resist pattern with 25 nm lines / 50 nm spacing. A scanning electron microscope (manufactured by Hitachi High-Tech Nologis, CG4100) was used to measure the length of the resist pattern. In the formation of the above-mentioned resist pattern, the exposure amount for forming 25 nm line / 50 nm space (line and space (L / S=1 / 1)) was set as the optimum exposure amount.
[0140] The photoresist pattern thus obtained was observed from the top of the pattern and evaluated. A good resist pattern was considered "good", and an unfavorable state in which the resist pattern peeled off and collapsed was considered "collapsed".
[0141] The obtained results are shown in Table 1. In addition, scanning microscope photographs (upper part of the pattern) of the resist pattern to which the composition of Example 1 was applied and the resist pattern of the comparative example are shown in Figure 1 and Figure 2 middle.
[0142] Table 1
[0143] 25nm line Example 1 good Comparative Example 1 collapse
[0144] [Formation of negative resist pattern using electron beam lithography system]
[0145] On the film, the compositions for forming the resist underlayer film of Example 1 and Comparative Example 1 were respectively coated on a silicon wafer using a spin coater. The silicon wafer was baked on a hot plate at 215°C for 60 seconds to obtain a resist underlayer film with a film thickness of 5 nm. A negative resist solution for EUV was spin-coated on the resist underlayer film and heated at 100°C for 60 seconds to form an EUV resist film. For the resist film, an electron beam drawing device (ELS-G130) was used to expose it under specified conditions. After exposure, it was baked (PEB) at 110°C for 60 seconds, cooled to room temperature on a cooling plate, and developed with butyl acetate to form a resist pattern with 25nm lines / 50nm spacing. A scanning electron microscope (manufactured by Hitachi High-Tech Nologis, CG4100) was used to measure the length of the resist pattern. In the formation of the above-mentioned resist pattern, the exposure amount for forming 25 nm line / 50 nm spacing (line and space (L / S=1 / 1)) was set as the optimum exposure amount.
[0146] The photoresist pattern thus obtained was observed from above the pattern and evaluated. A resist pattern having good quality at the same exposure amount was considered "good", and a resist pattern having residues between patterns was considered "defective".
[0147] The obtained results are shown in Table 1. In addition, scanning microscope photographs (upper part of the pattern) of the resist pattern to which the composition of Example 1 was applied and the resist pattern of the comparative example are shown in Figure 3 and Figure 4 middle.
[0148] Table 2
[0149] 25nm line Example 1 good Comparative Example 1 defect
[0150] Industrial Availability
[0151] The resist underlayer film forming composition according to the present invention can provide a composition for forming a resist underlayer film capable of forming a desired resist pattern, and a method for producing a substrate with a resist pattern and a method for producing a semiconductor device using the resist underlayer film forming composition.
Claims
1. A composition for forming an EUV resist underlayer film, comprising a (meth)acrylic polymer and an organic solvent, wherein the (meth)acrylic polymer has a basic organic group substituted with a protecting group in a side chain, and the composition for forming an EUV resist underlayer film does not contain a polymer other than the (meth)acrylic polymer, and the organic group is an acyloxy group having an amino group substituted with a protecting group or an acyloxy group having a nitrogen-containing heterocycle substituted with a protecting group. 2 . The EUV resist underlayer film-forming composition according to claim 1 , wherein the protecting group is selected from the group consisting of a tert-butoxycarbonyl group, a benzyloxycarbonyl group, a 9-fluorenylmethoxycarbonyl group, a 2,2,2-trichloroethoxycarbonyl group and an allyloxycarbonyl group.
3. The EUV resist underlayer film-forming composition according to claim 1 or 2, wherein the (meth)acrylic polymer is a polymer having a unit structure represented by the following formula (1): In formula (1), R1 represents a hydrogen atom or a methyl group, L represents a divalent linking group, and X represents an acyloxy group having an amino group substituted with a protecting group or an acyloxy group having a nitrogen-containing heterocyclic ring substituted with a protecting group.
4. The composition for forming an EUV resist underlayer film according to any one of claims 1 to 3, wherein A cross-linking catalyst is also included.
5. The composition for forming an EUV resist underlayer film according to any one of claims 1 to 4, wherein A cross-linking agent is also included.
6. An EUV resist underlayer film, characterized in that: A fired product of a coating film formed from the EUV resist underlayer film forming composition according to any one of claims 1 to 5.
7. A method for manufacturing a patterned substrate, comprising: a step of coating the EUV resist underlayer film forming composition according to any one of claims 1 to 5 on a semiconductor substrate and baking the coating to form an EUV resist underlayer film; a step of coating an EUV resist on the EUV resist underlayer film and baking the coating to form an EUV resist film; a step of exposing the semiconductor substrate coated with the EUV resist underlayer film and the EUV resist; and a step of developing and patterning the exposed EUV resist film.
8. A method for manufacturing a semiconductor device, characterized in that: Include: A step of forming an EUV resist underlayer film formed from the EUV resist underlayer film-forming composition according to any one of claims 1 to 5 on a semiconductor substrate, forming an EUV resist film on the EUV resist underlayer film, A process of forming an EUV resist pattern by irradiating an EUV resist film with light or electron beams and then developing the film. a step of etching the EUV resist underlayer film through the formed EUV resist pattern to form a patterned EUV resist underlayer film, and A step of processing a semiconductor substrate using the patterned EUV resist underlayer film.