Amino-containing insoluble polymer solution without solubilizer, preparation method and application thereof

By combining weak acid ions with amino-containing insoluble polymers and removing the solubilizer by dialysis or extraction, the problem of solubilizers affecting material properties in the prior art is solved, and a polymer solution without solubilizers is prepared, which is suitable for many applications. It has excellent performance in various application scenarios, especially in the fields of biomedical and wound repair.

CN115058025BActive Publication Date: 2024-10-29STOMATOLOGICAL HOSPITAL AFFILIATED TO ZUNYI MEDICAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210730653.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-10-29
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

In the existing technology, when preparing amino-containing insoluble polymer solutions, it is often necessary to use solubilizers, which leads to a reduction in the biocompatibility of the material and a lack of water or solvent resistance in solid products, which limits its application scenarios.

Method used

The method of combining weak acid ions with amino-containing insoluble polymers is used to remove cosolvents through dialysis or extraction to prepare a polymer solution without solubilizers, retaining the polymers and solvents to ensure that the original properties of the materials remain unchanged.

Benefits of technology

It achieves the preparation of solvent-free polymer solutions, maintains the biocompatibility and mechanical properties of the material, and is suitable for the use of liquid materials and solid products, especially in the fields of biomedicine and wound repair, showing excellent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115058025B_ABST
    Figure CN115058025B_ABST
Patent Text Reader

Abstract

The present application provides a method for preparing an amino-containing insoluble polymer solution without a solubilizer in the technical field of material preparation, wherein a solution of an amino-containing insoluble polymer (such as chitosan, type I collagen, linear polyethyleneimine, polyamide, etc.) is treated into a polymer solution state in which amino groups are combined with weak acid ions, and impurities in the solution are removed by dialysis, thereby obtaining an amino-containing insoluble polymer solution without a solubilizer. The amino-containing insoluble polymer solution prepared by the present invention is different from the situation in which a solubilizer is present, and the strong intermolecular hydrogen bonding effect can be restored by simply removing the solvent, thereby restoring it to an insoluble solid state. The amino-containing insoluble polymer solution without a solubilizer prepared by the present invention can solve the scenario in which only liquid materials can be used, and can effectively avoid the influence of the solubilizer on the properties of the material, such as acetic acid can reduce the biocompatibility of chitosan materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material preparation, and in particular to an amino-containing insoluble polymer solution without a solubilizing agent, a preparation method and application thereof. Background Art

[0002] Amino-containing insoluble polymers refer to polymers containing amino groups that cannot be directly dissolved by water or organic solvents. Typical representatives include chitosan (CS), type I collagen (COL-I), branched polyethyleneimine and polyamide. Among them, CS and COL-I are taken as examples. As natural polymers, they have excellent biocompatibility and can be used in various fields such as medicine, food, beauty, health care, and chemical industry. Although CS and COL-I have huge application potential and excellent biosafety, it is difficult for us to see products made of CS and COL-I materials in our lives. The main reason is that CS and COL-I contain a large number of hydrogen bonds within and between molecules, making them difficult to dissolve and process, and the addition of solubilizers such as acetic acid will reduce the biocompatibility of CS and COL-I and the solvent resistance of the solid obtained by removing the solvent. Therefore, the use of amino-containing insoluble polymers such as CS and COL-I is limited by the fact that solutions can only be obtained through solubilizers. The chemical structure of CS is used to illustrate the intermolecular and intramolecular hydrogen bond structure of amino-containing insoluble polymers, as follows:

[0003]

[0004] The arrows represent the intermolecular hydrogen bonds and intramolecular hydrogen bonds of CS.

[0005] Take CS as an example to illustrate the common preparation methods of amino-containing insoluble polymer solutions. At present, the methods for preparing CS solutions are mainly divided into the following four types. 1. The most commonly used method is to dissolve CS in an acidic solution such as acetic acid, formic acid or hydrochloric acid (mainly acetic acid) of a certain concentration. This method is relatively simple and low-cost. The CS solution needs to undergo an acid-base reaction to restore its original polymer structure. The resulting solid product has a large number of pores and poor mechanical properties. 2. Use a mixture of alkalis such as sodium hydroxide to help CS dissolve. This method will significantly reduce the molecular weight of CS and affect the mechanical properties. The biocompatibility of the solubilizers used in the above two methods is poor, and the liquid CS products cannot be directly used to prepare biomedical fields. In addition, the solubilizer is easy to remain in the solid product of CS, which will also affect the use of CS in the biomedical field. 3. The molecular weight of CS is severely reduced by degradation treatment, so that it can be directly soluble in water. This method obtains solubility at the expense of the molecular weight of CS, and almost loses the mechanical properties required by CS as a polymer material. 4. Chemically modify the CS dissolved by the solubilizer to destroy the strong hydrogen bonding of CS, so that it can be directly dissolved in water or organic solvents. Methods 3 and 4 significantly change the molecular structure of CS, destroy the property that CS solid is insoluble in water, and it is difficult to use it directly as a solid material, which greatly limits the use scenarios of CS materials. The following two methods do not belong to the conventional methods for preparing CS solutions and are not the key contents of the present invention.

[0006] In summary, it can be seen from the method of preparing CS solution that the current method of preparing amino-containing insoluble polymer solution is difficult to get rid of the use of solubilizers, which greatly limits the use of amino-containing insoluble polymer solution. For example, acetic acid as a solubilizer will reduce the biocompatibility of CS and COL-I solutions, which is not conducive to use as biomedical materials. Therefore, the use of amino-containing insoluble polymers such as CS and COL-I has been difficult to break through. It is not that the properties of the materials themselves are not good enough, but the method of preparing amino-containing insoluble polymer solutions affects the performance of the materials themselves. In addition, the presence of solubilizers will make the solid products prepared from amino-containing insoluble polymer solutions not resistant to water or solvents, and it is difficult to use them as stable solid products. For this reason, it is very important to prepare amino-containing insoluble polymer solutions without solubilizers for the use of such materials. Summary of the invention

[0007] The present invention aims at the deficiencies of the prior art and provides a new method for preparing a solubilizer-free solution of an amino-containing insoluble polymer in order to overcome the problem that a solubilizer exists in the conventional dissolution method of the existing amino-containing insoluble polymer, and the solution containing the solubilizer destroys the original properties of the amino-containing insoluble polymer, thereby affecting the use of the polymer material.

[0008] One of the purposes of the present invention is to provide a method for preparing an amino-containing insoluble polymer solution without a solubilizer, wherein the amino-containing insoluble polymer is dissolved with a solubilizer, and then a salt or acid composed of weak acid ions is added to obtain a solution in which the weak acid ions are combined with the amino groups in the amino-containing insoluble polymer, and impurities are removed to retain only the polymer and the solvent, thereby preparing an amino-containing insoluble polymer solution without a solubilizer.

[0009] Furthermore, the method for removing impurities is dialysis or extraction. During extraction, a solvent that is insoluble in the amino-containing insoluble polymer solution but can dissolve the amino-containing insoluble polymer is added to the amino-containing insoluble polymer solution containing the solubilizer, and the added solvent is also difficult to dissolve impurity components other than the amino-containing insoluble polymer to achieve purification. The present invention can remove more than 99% of the solubilizer by extraction or dialysis.

[0010] Furthermore, the solubilizer is an acid or alkaline solution. When the solubilizer is an acid, the weak acid ions are different from the acid ions of the solubilizer, and the reactivity of the weak acid ions is weaker than that of the acid ions.

[0011] Furthermore, the solubilizer is formic acid, hydrochloric acid, acetic acid or a mixed solution containing sodium hydroxide.

[0012] Further, the weak acid ion is CO3 2- 、HCO3 - 、F - , ClO - 、SiO3 3- , S 2- , CN - 、SCN - 、NO2 - 、SO3 2- 、HPO4 2- , HS - 、AlO2 - BrO - , BO3 3- Or one of the other acid ions.

[0013] Furthermore, the salt composed of weak acid ions is one of potassium borate, sodium silicate, ammonium borate, sodium sulfite, sodium hydrosulfide, ammonium bicarbonate, sodium aluminate, sodium hypochlorite, magnesium bicarbonate, sodium carbonate, ammonium acetate, calcium bicarbonate or sodium hypochlorite, and the acid composed of weak acid ions is silicic acid, sulfurous acid, boric acid, hypochlorous acid, acetic acid or carbonic acid.

[0014] Further, the method specifically includes the following steps: specifically includes the following steps: (1) dissolving the amino-containing insoluble polymer in an acid or alkaline solution;

[0015] (2) a. For a solution of an amino-containing insoluble polymer dissolved in an acid as a solubilizer, a salt composed of weak acid ions is added, and the reaction ability of the weak acid ions is weaker than that of the acid ions of the solubilizer. The cations of the salt containing the weak acid ions can combine with the acid ions of the solubilizer, so that the weak acid ions combine with the amino groups of the amino-containing insoluble polymer and maintain a solution state; b. For a solution of an amino-containing insoluble polymer dissolved in an alkaline solution as a solubilizer, an excess of a weak acid composed of weak acid ions is added, and the weak acid can react with the base to generate a salt having weak acid ions. In addition, the excess weak acid combines with the amino-containing insoluble polymer to obtain a solution state in which the weak acid ions combine with the amino groups;

[0016] (3) removing impurities in the solution by dialysis or extraction to obtain a solution without solubilizing agents and containing only the amino-containing insoluble polymer and a solvent, namely, the amino-containing insoluble polymer solution; and replacing the solvent in the amino-containing insoluble polymer solution with organic solvents having different water contents to obtain amino-containing insoluble polymer solutions dissolved in different solvents.

[0017] Furthermore, the amino-containing insoluble polymer includes polysaccharide, type I collagen, linear polyethyleneimine, polypeptide polymer, silk protein or polyamide. For different amino-containing insoluble polymers, the selected salt or acid containing weak acid radical cannot be used as a solubilizing agent for the corresponding amino-containing insoluble polymer, nor does it have the property of directly dissolving the amino-containing insoluble polymer. For example, acetic acid will dissolve chitosan, and acetate radical cannot be selected as the salt or acid of the weak acid radical.

[0018] Working principle and beneficial effects of the present invention: Since the amino-containing insoluble polymer cannot be directly dissolved by water or organic solvent to obtain a solution, the present invention first obtains a solution in which weak acid ions and the amino groups of the amino-containing insoluble polymer are combined, and then the weak acid ions and other impurities in the solution can be removed by extraction or dialysis to obtain an amino-containing insoluble polymer solution without solubilizers. Note: A solution in which weak acid ions and the amino groups of the amino-containing insoluble polymer can be obtained by adjusting the weak acid ion component in the dialysate. By adjusting the solvent in the dialysate, amino-containing insoluble polymer solutions dissolved in different solvents can be obtained.

[0019] The second purpose of the present invention is to provide an amino-containing insoluble polymer solution without solubilizers, which can fully guarantee the original properties of the amino-containing insoluble polymer and is suitable for the use of liquid materials. For example, the liquid CS material can fully exert its molecular structure, and its antibacterial effect far exceeds that of the solid state; and without solubilizers such as acetic acid, the CS solution can maintain good biocompatibility and solve the problem that the CS solution is difficult to use as a biomedical material.

[0020] The amino-containing insoluble polymer solution without a solubilizer will return to the insoluble polymer solid state after the solvent is removed, which is helpful for the preparation of amino-containing insoluble polymer solid products. However, the amino-containing insoluble polymer solution material of the prior art has a solubilizer, so when it is directly prepared into a solid state (water-containing gel state), it still contains a solubilizer, and the material will dissolve in water or an organic solvent. This characteristic is not conducive to the preparation of solid products. The amino-containing insoluble polymer solution obtained by the present invention does not contain a solubilizer, and will not change the physical and chemical properties of the amino-containing insoluble polymer material. After being directly dried into a solid state, it will still restore its property of being difficult to dissolve in water or an organic solvent. This is also one of the advantages of the amino-containing insoluble polymer solution prepared by the present invention.

[0021] The present invention designs a method for preparing an amino-containing insoluble polymer solution without a solubilizer, which can solve the current dilemma that the amino-containing insoluble polymer solution can only be obtained by reducing the molecular weight of the amino-containing insoluble polymer or relying on a solubilizer. In addition, the amino-containing polymer solution without a solubilizer is conducive to solving the problem of difficulty in characterizing such substances, is conducive to maintaining the original properties of the polymer without being affected by the solubilizer, and can also be directly used as a liquid polymer material.

[0022] Taking CS as an example, CS solution without solubilizer can be used directly as a wound antibacterial agent without the problem of acetic acid as a solubilizer easily causing inflammatory reaction. The solid product obtained after drying the CS solution without solubilizer will not dissolve in water or organic solvents, which is different from the water-resistant property of CS solid containing solubilizer.

[0023] Taking CS as an example, the preparation method of the amino-containing insoluble polymer solution without a solubilizer is described. The present invention first dissolves CS by a traditional method, including dissolving CS by an acidic solution and an alkali-containing mixed solution as a solubilizer. Then a CS solution containing a solubilizer in a traditional form is obtained, and a salt of a weak acid ion is added to the CS solution with an acid as a solubilizer. The cation reactivity of the salt is stronger than that of the amino group of CS, and the reactivity of the weak acid ion of the salt is weaker than that of the anion formed by the acid as a solubilizer and the amino group of CS. Salt treatment of the CS solution containing a solubilizer can obtain a solution in which weak acid ions are combined with amino groups in the amino-containing insoluble polymer, and the weak acid ions and other impurities can be removed by pure water dialysis. After dialysis and purification, an amino-containing insoluble polymer solution without a solubilizer is obtained. Replacing the dialysate with other organic solvents can obtain an amino-containing insoluble polymer solution dissolved in an organic solvent. During extraction, a solvent that is insoluble in the amino-containing insoluble polymer solution but can dissolve the amino-containing insoluble polymer is added to the amino-containing insoluble polymer solution containing the solubilizer, and the added solvent is also insoluble in the impurity components of the non-amino-containing insoluble polymer. The present invention can remove more than 99% of the impurities of the non-amino-containing insoluble polymer and the solvent by extraction or dialysis.

[0024] The third object of the present invention is to provide applications of amino-containing insoluble polymer solutions, including applications in the preparation of biomedical materials, applications in the preparation of flocculants or metal ion chelating agents, and applications in the preparation of wound repair drugs.

[0025] The present invention can also prepare hydrogels by physical or chemical cross-linking, or prepare solids such as coatings, films, sheets or sponges after drying. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the process of the preparation method of the present invention;

[0027] Figure 2 The H NMR spectra of the products at each stage of the preparation process of CS aqueous solution in Example 9 ( 1 H NMR);

[0028] Figure 3 The pH test diagram of the CS solution and CS-HOAc prepared in Example 9 at 1% solid content;

[0029] Figure 4 Schematic diagram of detecting the biocompatibility of the CS solution in Example 9 to L929 at different concentrations by CCK-8 staining method;

[0030] Figure 5 Schematic diagram of the properties of the CS solution and CS-HOAc membrane after water treatment in Example 9;

[0031] Figure 6 Schematic diagram of the sterilization rate of CS solutions with different molecular weights at different concentrations against Staphylococcus aureus in Examples 7-9;

[0032] Figure 7 Schematic diagram of the statistical changes in wound area of ​​wound repair in C57BL6 mice with CS and COL-I solutions;

[0033] Figure 8 It is a schematic diagram of the turbidity removal rate of kaolin turbid solution at different concentrations of CS solution in Examples 7-9;

[0034] Fig. 9 Schematic diagram of the removal rate of various metal ions at different concentrations of CS solution in Example 9. DETAILED DESCRIPTION

[0035] The following is further described in detail through specific implementation methods:

[0036] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that all these embodiments are for further illustrating the present invention and shall not be construed as limiting the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art according to the above-mentioned content of the present invention still belong to the protection scope of the present invention.

[0037] Table 1 is a list of preparation conditions for the amino-containing water-soluble polymer solution of the present invention.

[0038]

[0039] CS is a typical representative of amino-containing poorly water-soluble polymers. In the present invention, CS is used to represent amino-containing poorly water-soluble polymers to illustrate the method of the present invention for preparing an amino-containing poorly water-soluble polymer solution without a solubilizing agent.

[0040] Example 1-23

[0041] The present invention first dissolves CS by using an acid or alkaline solution, and then obtains a solution in which weak acid radical ions are combined with amino groups of CS by chemical reaction.

[0042] Here, the most commonly used acetic acid (HOAc) aqueous solution is used to dissolve CS, and the preparation method of CS solution is described in detail according to Example 9 in Table 1. The specific method is as follows: Figure 1 As shown, first, 0.7mmol of 1% acetic acid is added dropwise to 1mmol of CS raw material (CS-raw material) in a stirring state, and stirred at 20℃ for 2h until the CS-raw material is completely dissolved. At this time, the HOAc aqueous solution reacts with the amino groups on CS, destroying the hydrogen bonds within and between CS molecules, and the resulting solution is CS-HOAc. 0.73mmol of ammonium bicarbonate (NH4HCO3) aqueous solution is added dropwise to the stirring CS-HOAc solution. The ammonium radical activity of NH4HCO3 is higher than that of the amino groups on CS, so the acetic acid bound to CS can be replaced; and the hydrolyzed bicarbonate and carbonate components can be combined with CS to maintain a stable solution state. After the addition of NH4HCO3, the reaction is carried out at a temperature of 5-80℃ for 20min. The molar amounts of HOAc and NH4HCO3 can change during the entire reaction process. The excess bicarbonate and carbonate in ammonium bicarbonate will be released in the form of CO2 gas. The ammonium radicals of HOAc and NH4HCO3 combine to form ammonium acetate impurities, which can be purified by extraction or dialysis to obtain a CS aqueous solution containing only CS and water.

[0043] The CS aqueous solution is dialyzed by organic solvents of different gradient concentrations to obtain a CS solution dissolved in an organic solvent.

[0044] In Example 9, bicarbonate or carbonate is combined with CS and then purified to obtain a CS aqueous solution. The chemical flow of the entire process is shown as follows:

[0045]

[0046] Among them, ammonium bicarbonate represents a salt containing weak acid ions, and can also be replaced by other salts with similar effects.

[0047] In Examples 1-18, the CS raw material is dissolved by different methods, and then a solution in which weak acid ions are combined with amino groups of CS is prepared. These treatment methods are similar to those of Example 9 and will not be described in detail. The substances and amounts used in preparing CS solutions by different methods are detailed in the typical examples introduced in Table 1.

[0048] It should be noted that the molar fraction of CS in Table 1 refers to the molar fraction of its repeating unit, that is, the molar fraction of nitrogen in CS.

[0049] In Examples 19-23, except for CS, the preparation methods of solutions of other amino-containing insoluble polymers (such as type I collagen, linear polyethyleneimine, polyamide, etc.) are similar to the preparation method of CS solution, that is, the amino-containing insoluble polymer is first combined with weak acid ions, and then impurities are removed by dialysis or extraction to obtain an aqueous solution of the amino-containing insoluble polymer.

[0050] like Figure 2 As shown in the figure, since CS raw materials are not directly soluble in water or organic solvents, there is no single CS 1 HNMR data from CS-HOAc 1 It can be seen from the H NMR graph that the position below 2ppm is the alkyl structure connected to the carbon, so the position of the methyl group on the acetyl group that has not been removed in CS can be obtained, which is represented by g'. Since CS-HOAc contains acetate, the hydrogen of the alkyl group on the acetate is at 1.8ppm. It is worth mentioning that the peak at 4.7ppm is the overlapping peak of active hydrogen -OH and -NH, and a and a' are connected to two ether bonds, and the peaks of hydrogen on them also overlap at 4.7ppm. The hydrogens marked as c~f and c'~f' are on the alkyl group connected to the oxygen atom, and they overlap at 3.2~4.0ppm. Since the alkyl groups marked as b and b' are connected to the amino group, they are displayed at 2.8ppm.

[0051] CS-NH4HCO3 obtained by treating CS-HOAc with NH4HCO3 1The H NMR curve is not significantly different from the data of CS-HOAc between 1.4 and 4.4 ppm. This is because CS combines with the carbonate of NH4HCO3, while the acetate combines with the ammonium of ammonium bicarbonate. The positions of the hydrogen atoms on each alkyl group and the peak areas do not change significantly, so there is no obvious difference in the H NMR spectrum ( Figure 2 ).

[0052] As for the purified CS-NH4HCO3, that is, the CS solution obtained by removing ammonium acetate, almost no acetate was observed, and the peak area of ​​the alkyl group in the acetate was reduced from the original 2.4 to 0.01. It can be seen that more than 99% of the acetate has been removed by dialysis, and the extremely small amount of acetate residue can be ignored. Therefore, it can be considered that the CS aqueous solution without solubilizer was successfully prepared ( Figure 2 ).

[0053] Figure 2 The upper left center is the chemical formula of CS, and the upper right is the chemical formula of chitin contained in the CS raw material itself. CS usually contains a small amount of chitin, so it has both the upper left and upper right chemical formulas.

[0054] Figure 3 Table 1 shows the pH test of the CS solution and CS-HOAc prepared in Example 9 at 1% solid content. The pH of the HOAc solution at 1% content is very low, only 2.38. When the high molecular weight CS is combined with the HOAc solution with 70% molar number of its repeating units, the pH of the 1% solid content CS-HOAc increases to 5.42. The pH of the CS aqueous solution obtained in Example 9 is 7.39, which matches the weak alkaline nature of the amino group of CS, and can also indirectly indicate that the present invention successfully prepared the CS solution.

[0055] Figure 4 The effect of the CS solution in Example 9 on the growth of mouse fibroblasts (L929) was detected by CCK-8 staining. The L929 group cultured without CS solution was used as a blank group. Figure 5 It can be seen that whether it is a low concentration (CS solution concentration = 320 μg / mL) or a high concentration (CS solution concentration = 640 μg / mL), the CS solution has almost no toxicity to L929, showing good biocompatibility.

[0056] In summary, through the introduction of Examples 1-8 of the present invention, a CS solution has been successfully prepared, the pH of which is weakly alkaline and has excellent biocompatibility.

[0057] Application Example 1

[0058] The CS solutions prepared in Examples 1 to 18 can be dried to form films, and then the water-insoluble property of CS can be restored, so that water-resistant solid products can be prepared. Figure 5 As shown, taking Example 9 as an example, the CS solution is dried and prepared into a film with water resistance, while the CS-HOAc film is not water resistant.

[0059] The CS solution prepared by the present invention can be combined with non-water-resistant products such as paper straws that are widely used in response to environmental protection. The CS solution is coated on the paper straws and dried to form a film, thereby obtaining a degradable and water-resistant CS coating-modified paper straw. Specifically, the paper straws are soaked in a CS solution with a solid content of 2% and a molecular weight of more than 500 kDa, then taken out immediately, and then dried at 60°C in a rotating state. Repeatedly performing the CS soaking and drying operations on the paper straws can obtain paper straws whose surface is protected by a water-blocking CS layer.

[0060] In addition to being used for coating modification of non-water-resistant paper straws, under the same principle, the CS solution prepared by the present invention can also be prepared into various polymer products, actively responding to the current development requirements of degradable and environmentally friendly plastics around the world.

[0061] Application Example 2

[0062] CS is a well-known good natural antibacterial agent, but CS without any treatment is in a solid state and cannot effectively expose its molecular structure and fully exert its antibacterial properties. The water-soluble CS solution prepared by using Examples 1 to 18 can theoretically fully exert its antibacterial properties. Here, only the antibacterial effect on Staphylococcus aureus is introduced.

[0063] Figure 6 Here, the CS solution dissolved in acetic acid, CS-HOAc, and CS solution are compared to introduce the antibacterial properties of CS solution. The specific method is to mix 200 μL of 5×10 5 cfu / mL of Staphylococcus aureus were added to the culture medium with different contents of CS liquid and cultured at 37°C for 18 hours. Then, the antibacterial effects of different antimicrobial groups were counted by plating on solid culture medium.

[0064] Figure 6 The figure is a comparison of the antibacterial ability of the CS solutions in Examples 7-9 and the CS-HOAc in Example 7 against Staphylococcus aureus. It can be seen that the antibacterial effect of CS solutions of different molecular weights is very good, and the antibacterial rate almost reaches 100% when the concentration of the CS solution exceeds 1‰. The antibacterial ability of CS-HOAc is also very strong, but when its concentration is as high as 0.8%, it is difficult to completely eliminate Staphylococcus aureus. Therefore, the CS solution prepared by the present invention can be used as an antibacterial material.

[0065] like Figure 6As shown, # represents an antibacterial rate of 100%. The prefix of CS solution is L, which represents that the CS main body is low molecular weight (50 kDa), M represents medium molecular weight (500 kDa), and H represents high molecular weight (1000 kDa).

[0066] Application Example 3

[0067] The CS solution prepared in Example 9 was applied to a wound for wound healing by applying the type I collagen (COL-I) solution prepared in the same manner as in Example 19. Specifically, a wound with a diameter of about 1 cm was made on the back of a C57BL6 mouse, and then the repairing ability of sterilized gauze, CS-HOAc, CS solution, and COL-I solution on the wound of C57BL6 mice was observed at different times.

[0068] like Figure 7 As shown, the blank group was sterilized gauze as wound dressing. Figure 7 The changes in wound area of ​​wound repair in mice showed that the wound area of ​​mice was gradually reduced over time from 1 to 7 days. The repair effects of CS solution and COL-I solution on mouse wounds were better than those of CS-HOAc solution, and the repair effect of CS-HOAc solution was better than that of sterilized gauze. CS solution and COL-I solution were used for wound repair, which reduced the wound area of ​​C57BL6 mice to less than 8% on the 7th day, which was 39% of the wound area of ​​gauze dressing, showing excellent wound healing effect. Therefore, CS solution and COL-I solution have great application potential for wound repair.

[0069] Application Example 4

[0070] The CS components of the CS solutions prepared in Examples 1 to 18 carry positive charges, and generally turbid water contains a large number of solid inorganic particles with negative surface charges. Therefore, the CS solution can be used as a flocculant for water purification through neutralization.

[0071] In order to verify the water purification effect of CS solution, the CS solution in Examples 7-9 was used for measurement. Specifically, 1.0 g of kaolin particles with an average particle size of 5 μm was placed in 1 L of pure water, and then stirred at 300 r / min for 4 min to obtain simulated turbid water. Different contents of flocculants (i.e., water purifiers) were dropped into the turbid liquid, stirred at 3000 r / min for 5 min and allowed to stand for 2 min. The liquid at 1 cm below the liquid surface after standing was taken and the turbidity was measured with a turbidimeter.

[0072] In order to observe the water inflow effect of the CS solution in Examples 7-9, cationic polyacrylamide (CPAM), the most commonly used flocculant in industry, was used as a control group. Figure 8In the turbidity removal rate, it can be found that when the dosage of the water purifier (i.e., flocculant) is relatively low (at 0.3 mg / mL), the water purification effect of the CS solutions of Examples 7-9 is better than that of CS-HOAc and CPAM. At this time, the water purification effect of the high molecular weight CS solution in Example 9 is the best, and the turbidity removal rate reaches 96.5%. When the dosage of the water purifier is higher than 0.6 mg / mL and lower than 8.0 mg / mL, the water purification effect of the industrial flocculant is the most stable and excellent, and the water purification effect is about 96%. In contrast, as the dosage of the CS solution increases, the water purification effect of the turbid liquid gradually decreases. Overall, the water purification effect of the high molecular weight CS solution is better than that of the low molecular weight, while the water purification effect of the CS solution is weaker than that of CPAM and stronger than that of CS-HOAc.

[0073] Since CS-HOAc solution is obviously acidic and CPAM is not friendly to human organisms, the antibacterial and biofriendly CS solution can be used as a water purifier for drinking water.

[0074] Figure 7 is the turbidity removal rate of CS solution at different concentrations on kaolin turbid solution in Examples 7-9. Specifically, the prefixes L-, M-, and H- of CS represent the molecular weight and Figure 6 The same; CPAM is a cationic polyacrylamide with a molecular weight of 5000 kDa; the average particle size of kaolin is 5 μm.

[0075] Application Example 5

[0076] The CS solution of Example 9 has the amino structure of CS, which can be used to undergo a chelating reaction with metal ions and to adsorb metal ions in the solution.

[0077] Will Fig. 9 The substances containing different metal ions in the horizontal axis shown in the figure were prepared into 200 mg / mL solutions based on the metal ions. Then different amounts of metal ion adsorbents were added at 300 r / min. The CS-HOAc prepared in Example 9 was used as the control group.

[0078] Fig. 9 The CS-HOAc and CS solutions in the 8 metal ions that are harmful to the human body have a certain removal effect. And as the amount of metal ion adsorbent increases, the adsorption effect is better. However, overall, the effect of these two adsorbents in removing metal ions is not ideal, but for Cr6 in potassium dichromate (K2Cr2O7), + The adsorption effect is the best.

[0079] Both CS solution and CS-HOAc prepared by traditional methods can adsorb a certain amount of metal ions and can be used as heavy metal ion adsorbents.

[0080] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing an amino-containing insoluble polymer solution without a solubilizing agent, Features: The amino-containing insoluble polymer is dissolved with a solubilizer, and then a salt or acid composed of weak acid ions is added to obtain a solution in which the weak acid ions are combined with the amino groups in the amino-containing insoluble polymer, and impurities are removed to retain only the polymer and the solvent, so as to prepare an amino-containing insoluble polymer solution without a solubilizer; wherein the amino-containing insoluble polymer includes chitosan, type I collagen, linear polyethyleneimine, polypeptide polymer, polyamide or silk fibroin; the solubilizer is an acid or alkaline solution, when the solubilizer is an acid, a salt composed of weak acid ions is added, and when the solubilizer is an alkaline solution, an excess of weak acid composed of weak acid ions is added; the weak acid ions are CO 3 2 ⁻、HCO 3 ⁻、F⁻、ClO⁻、SiO 3 3 ⁻、S 2 ⁻、CN⁻、SCN⁻、NO 2 ⁻、SO 3 2 ⁻、HPO 4 2 ⁻、HS⁻、AlO 2 ⁻、BrO⁻、BO 3 3 ⁻ or one of the other acid radical ions.

2. The preparation method according to claim 1, Features: Impurities can be removed by dialysis or extraction.

3. The preparation method according to claim 2, Features: The solubilizer is an acid or alkaline solution. When the solubilizer is an acid, the weak acid ions are different from the acid ions of the solubilizer, and the reaction activity of the weak acid ions is weaker than that of the acid ions.

4. The preparation method according to claim 3, Features: The solvent is formic acid, hydrochloric acid, acetic acid or a mixed solution containing sodium hydroxide.

5. The preparation method according to any one of claims 1 to 4, Features: The specific steps include: (1) Dissolve the amino-containing insoluble polymer in an acid or alkaline solution; (2) a. For a solution of an amino-containing insoluble polymer dissolved by an acid as a solubilizer, a salt composed of weak acid ions is added. The reaction ability of the weak acid ions is weaker than that of the acid ions of the solubilizer. The cations of the salt containing the weak acid ions can combine with the acid ions of the solubilizer, so that the weak acid ions combine with the amino groups of the amino-containing insoluble polymer and maintain a solution state. b. For a solution of an amino-containing insoluble polymer dissolved by an alkaline solution as a solubilizer, an excess of a weak acid composed of weak acid ions is added. The weak acid can react with the base to generate a salt having weak acid ions. In addition, the excess of the weak acid combines with the amino-containing insoluble polymer to obtain a solution state in which the weak acid ions combine with the amino groups. (3) Impurities in the solution are removed by dialysis or extraction to obtain a solution without solubilizing agents and containing only the amino-containing insoluble polymer and a solvent, namely, the amino-containing insoluble polymer solution. The solvent in the amino-containing insoluble polymer solution is replaced by organic solvents with different water contents to obtain amino-containing insoluble polymer solutions dissolved in different solvents.

6. An amino-containing insoluble polymer solution prepared by the method according to claim 5.

7. Use of the amino-containing insoluble polymer solution according to claim 6 in the preparation of biomedical materials.

8. Use of the amino-containing insoluble polymer solution according to claim 6 in the preparation of flocculants or metal ion chelating agents.

9. Use of the amino-containing insoluble polymer solution according to claim 6 in preparing a wound repair drug carrier.

Citation Information

Patent Citations

  • Chitosan quaternary phosphonium salt derivative and preparation method thereof

    CN101649007A

  • Polyamide solution system and preparation method thereof

    CN107312185A

  • Homogeneous Aqueous Solution Of Injectable Chitosan Having A Ph Close To Physiological Ph

    CN107660146A

  • Preparation method of temperature-sensitive hydrogel precursor

    CN109957150A

  • Near neutral aqueous chitosan solution, its dried product, and method of producing them