A green low-temperature preparation method for supported high-entropy alloy materials and their electrocatalytic application

By adding a reducing agent to a carbon-containing metal salt solution, the carbon-bearing high-entropy alloy material was prepared in one-step manner, which solved the problems of high energy consumption in the preparation of existing high-entropy alloys and difficulty in treating waste liquids, and achieved low-temperature green preparation and high electricity Catalytic activity, suitable for hydrogen precipitation and oxygen reduction reactions.

CN115101764BActive Publication Date: 2024-11-12DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210509301.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-10
Publication Date
2024-11-12
Estimated Expiration
2042-05-10

AI Technical Summary

Technical Problem

The existing high entropy alloy materials are energy-consuming and use surfactants and organic solvents, which leads to complex preparation and difficult-to-treat waste liquids, making it difficult to achieve green low-temperature preparation and efficient application in electrocatalytic reactions.

Method used

By adding appropriate reducing agent to the carbon-containing metal salt solution, a one-step method is used to prepare carbon-bearing high-entropy alloy material, controlling the concentration and proportion of metal salts, carbon carriers and reducing agents, achieving low-temperature preparation, avoiding heating and other Additives provide high-entropy alloy material with a single face-centered cubic structural phase, which is suitable for hydrogen precipitation and oxygen reduction reactions.

Benefits of technology

It has achieved low energy consumption and green preparation of high-entropy alloy materials, with high electrocatalytic activity, suitable for hydrogen precipitation and oxygen reduction reactions, and the proportion and loading of metal atoms are controllable, suitable for a variety of needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115101764B_ABST
    Figure CN115101764B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of electrocatalysts, and specifically relates to a green low-temperature preparation method and electrocatalytic application of a supported high-entropy alloy material. The present invention uses a low-temperature aqueous phase method, without adding a surfactant or a reduction control agent, and after reduction by a reducing agent and filtering and washing, a carbon-supported high-entropy alloy material is prepared in one step. The high-entropy alloy material prepared by the method has a controllable element atomic content (5 to 35%), a controllable element composition (Pt / Pd / Cr / Mn / Fe / Co / Ni / Cu / Zn), a controllable high-entropy alloy loading (5 to 60wt%), and has electrocatalytic activity for hydrogen evolution reaction and oxygen reduction reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalysts and relates to a green low-temperature preparation method and electrocatalytic application of a supported high-entropy alloy material. Background Art

[0002] Environmental problems caused by fossil energy consumption and greenhouse gas emissions are currently urgent problems that need to be solved worldwide. In order to propose good solutions to energy and environmental problems, the main research ideas are focused on the green hydrogen energy route, which is mainly to convert the electricity from renewable energy into hydrogen as an energy carrier through water electrolysis, and then use hydrogen-oxygen fuel cells to release and apply chemical energy. However, in the process of the above energy conversion and application, multiple electrocatalytic reactions are involved. The appropriate selection of electrocatalysts can effectively improve the energy conversion efficiency. The precious metal Pt has excellent electrocatalytic activity for the hydrogen evolution reaction (HER) of water electrolysis and the oxygen reduction reaction (ORR) of fuel cells, but Pt is expensive and scarce, so the selection of other metals to form alloys with Pt has attracted widespread attention. The introduction of other metals can regulate the electronic structure of Pt, thereby affecting its adsorption energy for reactants and reaction intermediates, improving the electrocatalytic intrinsic activity of Pt and reducing the amount of Pt, thereby improving the commercialization process of the green hydrogen energy route.

[0003] Among many types of alloys, high entropy alloys have become a current research hotspot because of their high entropy effect, lattice distortion effect, hysteresis diffusion effect and cocktail effect, which can effectively optimize the electronic structure of active sites and improve stability. High entropy alloys are defined as alloys containing 5 or more elements, with the atomic percentage of each element greater than 5% and less than 35%, and have a simple single-phase solid solution structure. Existing high entropy alloy preparation methods usually involve high reduction temperatures, rapid temperature rise and fall, addition of surfactants or use of organic solvents, etc., which have high energy consumption and are prone to produce more waste liquid containing surfactants or organic solvents, causing difficulties in synthesis and post-processing. Therefore, exploring green and efficient preparation of high entropy alloy materials and applying them to electrocatalytic reactions has become a key issue.

[0004] Therefore, compared with the reported articles or patents, the present invention can effectively prepare a carbon-supported high-entropy alloy material with a single face-centered cubic structure phase in one step by simply adding an appropriate reducing agent to a carbon-containing metal salt solution, and the material has electrocatalytic activity and is suitable for hydrogen evolution reaction and oxygen reduction reaction. Summary of the invention

[0005] The purpose of the present invention is to provide a simple preparation method and application of a carbon-supported high entropy alloy material that can be used for hydrogen evolution and oxygen reduction reactions in view of the deficiencies in the prior art. By rationally controlling the concentration of the metal salt solution, the amount of carbon carrier and the reducing agent added, a one-step method is used to obtain a supported high entropy alloy material with controllable element atomic content (5-35%), controllable element composition (Pt / Pd / Cr / Mn / Fe / Co / Ni / Cu / Zn), and controllable metal loading (5-60wt%). Since only metal salts, carbon and reducing agents participate in the reaction during the preparation process and no heating is required, the energy consumption is low and no other difficult-to-treat waste liquid is generated, which belongs to a green preparation route. The high entropy alloy material obtained by this method has electrocatalytic activity suitable for hydrogen evolution reaction and oxygen reduction reaction.

[0006] The technical solution of the present invention:

[0007] A green low-temperature preparation method for a supported high-entropy alloy material comprises the following steps:

[0008] The carbon carrier is dispersed in water, ultrasonicated for 0.5 to 1.5 hours, and then the mixed solution is placed in a water bath, and a metal salt aqueous solution and a reducing agent aqueous solution are added successively under the conditions of controlling the rotation speed to be greater than 200 rpm and the temperature to be 0 to 25°C, and reacted for 0.5 to 2 hours; the final mixed solution is filtered and washed until the filtrate is neutral; dried and ground to finally obtain a carbon-supported high entropy alloy material;

[0009] The carbon carrier is dispersed in the aqueous solution at a concentration of 0.1 to 2 mg mL -1 ;

[0010] The concentration of the metal salt aqueous solution is 0.1 to 30 mmol L -1 , preferably 10 to 30 mmol L -1 ;

[0011] The concentration of the reducing agent aqueous solution is 0.5 to 300 mmol L -1 , preferably 100 to 300 mmol L -1 ;

[0012] The loading amount of the high entropy alloy in the carbon-supported high entropy alloy material is 5-60wt%.

[0013] Based on the above technical solution, preferably, the metal types include five or more of platinum (Pt), palladium (Pd), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), and zinc (Zn).

[0014] Based on the above technical scheme, preferably, any one of the metal atoms accounts for 5 to 35% of the total metal atoms, preferably, the chromium, manganese, iron, cobalt, nickel, copper, and zinc account for 5 to 20% of the total metal atoms, and platinum and palladium account for 20 to 35% of the total metal atoms, and the volume of the actual added metal salt solution is calculated based on the atomic ratio and the concentration of the metal salt aqueous solution.

[0015] Based on the above technical solution, preferably, the volume of the reducing agent aqueous solution is equal to that of the metal salt aqueous solution, that is, the volume of the reducing agent aqueous solution is equal to the total volume of the metal salt solution actually added.

[0016] Based on the above technical solution, preferably, when the metal contains platinum, the Pt metal salt includes one or a mixture of two or more of chloroplatinic acid, chloroplatinous acid, potassium chloroplatinate, potassium chloroplatinite, sodium chloroplatinate, sodium chloroplatinite, ammonium chloroplatinate, and ammonium chloroplatinite;

[0017] When the metal contains palladium, the Pd metal salt includes one or a mixture of two or more of palladium chloride, potassium chloropalladate, potassium chloropalladate, sodium chloropalladate, sodium chloropalladate, and ammonium tetrachloropalladate;

[0018] When the metal contains chromium, the Cr metal salt includes one or a mixture of two or more of chromium chloride (III), chromium chloride (II), chromium nitrate, and chromium sulfate;

[0019] When the metal contains manganese, the Mn metal salt includes one or a mixture of two or more of manganese chloride, manganese nitrate, and manganese sulfate;

[0020] When the metal contains iron, the Fe metal salt includes one or a mixture of two or more of ferric chloride, ferrous chloride, ferric nitrate, ferrous nitrate, ferric sulfate, and ferrous sulfate;

[0021] When the metal contains cobalt, the Co metal salt includes one or a mixture of two or more of cobalt (III) chloride, cobalt (II) chloride, cobalt nitrate, and cobalt sulfate;

[0022] When the metal contains nickel, the Ni metal salt includes one or a mixture of two or more of nickel chloride, nickel nitrate, and nickel sulfate;

[0023] When the metal contains copper, the Cu metal salt includes one or a mixture of two or more of cupric chloride, cuprous chloride, cupric nitrate, and copper sulfate; the Zn metal salt solution includes one or a mixture of two or more of zinc chloride, zinc nitrate, zinc sulfate, and zinc acetate.

[0024] Based on the above technical solution, preferably, the reducing agent is sodium borohydride, potassium borohydride, magnesium borohydride or a mixture of two or more thereof, but is not limited thereto.

[0025] Based on the above technical solution, preferably, the carbon carrier material is one or a mixture of two or more of carbon black, activated carbon, carbon fiber, carbon nanotube, and graphene, but is not limited thereto.

[0026] Based on the above technical solution, preferably, the drying time is 1 to 5 hours and the drying temperature is 60 to 80°C.

[0027] The present invention also relates to protecting the supported high entropy alloy material obtained by the above preparation method, which has high electrocatalytic activity.

[0028] The present invention also relates to the application of protecting the above-mentioned supported high entropy alloy material in hydrogen evolution and oxygen reduction reactions.

[0029] The present invention adopts a low-temperature water phase method, without adding a surfactant or a reduction control agent, and prepares a carbon-supported high-entropy alloy material in one step after reduction by a reducing agent and filtering and washing.

[0030] Compared with the preparation and application of reported high entropy alloy materials, the present invention has the following advantages:

[0031] a) The preparation method adopted by the present invention does not use high temperature, surfactants and organic solvents, and has the characteristics of low energy consumption and environmental friendliness.

[0032] b) The metal atom ratio and loading amount of the high entropy alloy material prepared by the present invention are precisely controllable and can be widely applied to various needs.

[0033] c) The high entropy alloy material prepared by the present invention can be prepared by selecting any five or more components of platinum, palladium, chromium, manganese, iron, cobalt, nickel, copper and zinc, which has high universality.

[0034] d) The supported high entropy alloy material prepared by the present invention has electrocatalytic activity for hydrogen evolution reaction and oxygen reduction reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Example 1 Preparation of Pt x X-ray diffraction (XRD) spectrum of MnFeNiCu / C-1 high entropy alloy sample;

[0036] Figure 2 Example 1 Preparation of Pt x Thermogravimetric analysis (TGA) curve of MnFeNiCu / C-1 high entropy alloy sample;

[0037] Figure 3Example 1 Preparation of Pt x Acidic HER curve of MnFeNiCu / C-1 high entropy alloy sample;

[0038] Figure 4 Example 1 Preparation of Pt x Acidic ORR curve of MnFeNiCu / C-1 high entropy alloy sample;

[0039] Figure 5 Example 2 Preparation of Pt x X-ray diffraction (XRD) spectrum of MnFeNiCu / C-2 high entropy alloy sample;

[0040] Figure 6 Example 2 Preparation of Pt x Thermogravimetric analysis (TGA) curve of MnFeNiCu / C-2 high entropy alloy sample;

[0041] Figure 7 Example 2 Preparation of Pt x Acidic HER curve of MnFeNiCu / C-2 high entropy alloy sample;

[0042] Figure 8 Example 2 Preparation of Pt x Acidic ORR curves of MnFeNiCu / C-2 high entropy alloy samples. DETAILED DESCRIPTION

[0043] The present invention will be further described in the following examples, but the present invention is not limited thereto.

[0044] Example 1

[0045] 25 mg of carbon black was diluted to 2 mg mL -1 The mixture was dispersed in deionized water and ultrasonicated for 0.5 h. The mixture was then placed in a water bath and the speed was controlled at 600 rpm and the temperature was 0 °C. First, 20 mmol L -1 chloroplatinate (0.84 mL), manganese nitrate (0.63 mL), iron nitrate (0.63 mL), nickel nitrate (0.63 mL), and copper nitrate (0.63 mL) aqueous solution were added to control the atomic proportion of Pt to 25.0% and the atomic proportion of the other elements to 18.7%. Then 3.38 mL of 200 mmol L -1 The sodium borohydride aqueous solution was used as a reducing agent and the reaction was carried out for 1 hour. The final mixed solution was filtered and washed until the filtrate was neutral; it was dried at 70°C for 4 hours and ground to finally obtain a supported high entropy alloy material with a loading of 20wt%.

[0046] like Figure 1The XRD results show that the product obtained in this example is a high entropy alloy solid solution with a single face-centered cubic (FCC) structure.

[0047] like Figure 2 , TGA determined the Pt content of the product obtained in this example x The loading of MnFeNiCu was 20 wt%.

[0048] like Figure 3 The high entropy alloy material prepared in this example has excellent acidic HER activity, 10 mAcm -2 The overpotential at is only 8.1mV.

[0049] like Figure 4 The high entropy alloy material prepared in this embodiment has excellent acidic ORR activity, and the half-wave potential is 0.85Vvs.RHE.

[0050] Example 2

[0051] 25 mg of carbon black was diluted to 0.5 mg mL -1 The mixture was dispersed in deionized water and ultrasonicated for 0.5 h. The mixture was then placed in a water bath and the speed was controlled at 600 rpm and the temperature was 5 °C. First, 20 mmol L -1 Sodium chloroplatinate (0.73 mL), manganese nitrate (0.73 mL), iron nitrate (0.73 mL), nickel nitrate (0.73 mL), and copper nitrate (0.73 mL) aqueous solutions were added to control the atomic ratio of all atoms to be 20.0%, and then 3.65 mL of 200 mmol L -1 The sodium borohydride aqueous solution was used as a reducing agent and the reaction was continued for 1 hour. The final mixed solution was filtered and washed until the filtrate was neutral; dried at 70°C for 2 hours and ground to finally obtain a supported high entropy alloy material with a loading of 20 wt%.

[0052] like Figure 5 The XRD results show that the product obtained in this example is a high entropy alloy solid solution with a single FCC.

[0053] like Figure 6 , TGA determined the Pt content of the product obtained in this example x The loading of MnFeNiCu was 20 wt%.

[0054] like Figure 7 The high entropy alloy material prepared in this example has excellent acidic HER activity, 10 mAcm -2 The overpotential at is only 9.1mV.

[0055] like Figure 8The high entropy alloy material prepared in this embodiment has excellent acidic ORR activity, and the half-wave potential is 0.83 V vs. RHE.

[0056] Example 3

[0057] 40 mg of carbon black was diluted to 1 mg mL -1 The mixture was dispersed in deionized water and ultrasonicated for 1 h. The mixture was then placed in a water bath and the speed was controlled at 400 rpm and the temperature was 15 °C. First, 15 mmol L -1 2.51 mL of sodium chloroplatinate (2.51 mL), manganese nitrate (5.53 mL), ferric sulfate (5.53 mL), nickel sulfate (5.53 mL), and cupric chloride (5.53 mL) aqueous solution were added to control the atomic proportion of Pt to 10.2% and the atomic proportion of the other elements to 22.4%. Then 24.62 mL of 300 mmol L -1 The potassium borohydride aqueous solution was used as a reducing agent and the reaction was carried out for 1.5 hours. The final mixed solution was filtered and washed until the filtrate was neutral; it was dried at 65°C for 5 hours and ground to finally obtain a supported high entropy alloy material with a loading of 40wt%.

[0058] Example 4

[0059] 25 mg of carbon black was diluted to 1 mg mL -1 The mixture was dispersed in deionized water and ultrasonicated for 0.75 h. The mixture was then placed in a water bath and the speed was controlled at 800 rpm and the temperature was 25 °C. First, 12 mmol L -1 Sodium chloroplatinate (1.00 mL), cobalt (II) chloride (1.38 mL), ferric chloride (1.38 mL), nickel chloride (1.38 mL), and copper chloride (1.38 mL) aqueous solution were added to control the atomic proportion of Pt to 15.2% and the atomic proportion of the other elements to 21.2%. Then 6.52 mL of 200 mmol L -1 The potassium borohydride aqueous solution was used as a reducing agent and the reaction was carried out for 1.5 hours. The final mixed solution was filtered and washed until the filtrate was neutral; dried at 60°C for 3 hours and ground to finally obtain a supported high entropy alloy material with a loading of 20wt%.

[0060] Example 5

[0061] 15 mg of carbon black was diluted to 1 mg mL -1 The mixture was dispersed in deionized water and ultrasonicated for 0.5 h. The mixture was then placed in a water bath and the speed was controlled at 350 rpm and the temperature was 15 °C. First, 25 mmol L -1Aqueous solution of potassium chloroplatinate (0.43 mL), cobalt (III) chloride (0.32 mL), ferric chloride (0.32 mL), nickel chloride (0.32 mL), and zinc chloride (0.32 mL) was added to control the atomic proportion of Pt to 25.0% and the atomic proportion of the remaining elements to 18.75%. Then 1.71 mL of 150 mmol L -1 The magnesium borohydride aqueous solution was used as a reducing agent and the reaction was carried out for 0.5 h. The final mixed solution was filtered and washed until the filtrate was neutral; it was dried at 60°C for 2 h and ground to finally obtain a supported high entropy alloy material with a loading of 20 wt%.

Claims

1. A green low-temperature preparation method for a supported high-entropy alloy material, characterized in that: The following steps are involved: The carbon carrier is dispersed in water and ultrasonicated for 0.5-1.5 h. The mixed solution is then placed in a water bath. A metal salt aqueous solution and a reducing agent aqueous solution are added under the conditions of a rotation speed greater than 200 rpm and a temperature of 0-25 °C, and the reaction is carried out for 0.5-2 h. The final mixed solution is filtered and washed until the filtrate is neutral. The filtrate is dried to finally obtain a carbon-supported high entropy alloy material. The carbon carrier is dispersed in the aqueous solution at a concentration of 0.1-2 mg mL -1 ; The concentration of the metal salt aqueous solution is 0.1~30 mmol L -1 ; The concentration of the reducing agent aqueous solution is 0.5~300 mmol L -1 ; The loading amount of high entropy alloy in the carbon-supported high entropy alloy material is 5-60 wt%; The metal types include five of platinum, manganese or cobalt, iron, nickel, copper or zinc; Any metal atom accounts for 5-35% of the total metal atoms; The reducing agent is one or a mixture of two or more of sodium borohydride, potassium borohydride and magnesium borohydride.

2. The preparation method according to claim 1, characterized in that: The volumes of the reducing agent aqueous solution and the metal salt aqueous solution are equal.

3. The preparation method according to claim 1, characterized in that: When the metal contains platinum, the platinum metal salt includes one or a mixture of two or more of chloroplatinic acid, chloroplatinous acid, potassium chloroplatinate, potassium chloroplatinite, sodium chloroplatinate, sodium chloroplatinite, ammonium chloroplatinate, and ammonium chloroplatinite; When the metal contains manganese, the manganese metal salt includes one or a mixture of two or more of manganese chloride, manganese nitrate and manganese sulfate; When the metal contains iron, the iron metal salt includes one or a mixture of two or more of ferric chloride, ferrous chloride, ferric nitrate, ferrous nitrate, ferric sulfate, and ferrous sulfate; When the metal contains cobalt, the cobalt metal salt includes one or a mixture of two or more of cobalt (III) chloride, cobalt (II) chloride, cobalt nitrate, and cobalt sulfate; When the metal contains nickel, the nickel metal salt solution includes one or a mixture of two or more of nickel chloride, nickel nitrate, and nickel sulfate; When the metal contains copper, the copper metal salt solution includes one or a mixture of two or more of cupric chloride, cuprous chloride, copper nitrate, and copper sulfate; When the metal contains zinc, the zinc metal salt solution includes one or a mixture of two or more of zinc chloride, zinc nitrate, zinc sulfate and zinc acetate.

4. The preparation method according to claim 1, characterized in that: The carbon carrier is one or a mixture of two or more of carbon black, activated carbon, carbon fiber, carbon nanotube and graphene.

5. The preparation method according to claim 1, characterized in that: The drying time is 1~5 h, and the drying temperature is 60~80℃.

6. The supported high entropy alloy material obtained by the preparation method described in any one of claims 1 to 5.

7. Use of the supported high entropy alloy material according to claim 6 in hydrogen evolution and oxygen reduction reactions.