A hydrogen fuel cell catalyst and preparation method thereof

By using fullerene support and PtAu alloy structure in hydrogen fuel cell catalysts, the problem of insufficient initial activity and stability of the catalyst is solved, the high initial activity and durability are improved, and the low platinum catalyst activity in the prior art is solved Problems of low and poor stability.

CN115101767BActive Publication Date: 2024-11-22WUXI WEIFU ENVIRONMENT PROTECTION CATALYST
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210925144.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-03
Publication Date
2024-11-22
Estimated Expiration
2042-08-03

AI Technical Summary

Technical Problem

The initial activity and stability of existing hydrogen fuel cell catalysts are insufficient, especially low platinum catalysts have problems of low activity and poor stability, and the initial activity of platinum alloy catalysts is relatively low, making it difficult to significantly improve without increasing costs.

Method used

Fullerene is used as the carrier, Pt and PtAu alloy are used as the active components, and are designed through multi-layer structure, including fullerene as the inner layer, PtAu alloy as the middle layer, and the outermost layer is loaded with Pt, through ball milling, ultrasonication, heating, reduction and Catalysts with high initial activity and high stability are prepared by calcining.

Benefits of technology

The initial activity and stability of the catalyst are improved, the dispersion and utilization of precious metals are enhanced, the precipitation and agglomeration migration of Pt are reduced, and the durability of the catalyst is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115101767B_ABST
    Figure CN115101767B_ABST
Patent Text Reader

Abstract

The present invention provides a hydrogen fuel cell catalyst, which includes a carrier, the carrier is fullerene, the fullerene surface is loaded with PtAu alloy, and the PtAu alloy surface is loaded with Pt. The hydrogen fuel cell catalyst of the present invention uses fullerene as a carrier, Pt and Au as active components, loads precious metals by a polyol reduction method, then alloys by high-temperature calcination, and finally loads Pt on the alloy surface by hydrogen reduction to obtain a high-load and highly dispersed Pt-PtAu / fullerene catalyst; since the fullerene itself is spherical, elliptical, tubular, etc. and has a high specific surface area, the metal dispersion is increased and the utilization rate of the precious metal is improved; the surface modification treatment can enhance the proton conduction ability, and the carrier modified with perfluorosulfonic acid resin further enhances the conduction ability of H protons and the hydrophobicity of the carrier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to electrocatalytic technology, and in particular to a hydrogen fuel cell catalyst and a preparation method thereof. Background Art

[0002] As fossil energy is becoming increasingly depleted, it is urgent to find alternative new energy sources. Hydrogen energy, as an efficient, clean, safe and sustainable secondary energy source, has attracted much attention in recent years. Hydrogen energy can penetrate into all aspects of traditional energy, including transportation, long-term energy storage, industrial fuel, portable equipment and other fields. Hydrogen fuel cells are considered to have broad development prospects due to their excellent performance in hydrogen energy utilization efficiency, power density, emissions and other aspects.

[0003] As the core material of hydrogen fuel cells, catalysts account for a large proportion of the cost of the entire fuel cell stack; and the initial activity and stability of the catalyst are important indicators to measure its performance. Catalysts are needed to accelerate the reaction at the two poles of proton exchange membrane fuel cells. At present, the research on catalysts mainly includes platinum-carbon catalysts, platinum alloy catalysts, low-platinum catalysts and non-platinum catalysts. In the research on non-platinum catalysts in patent CN113725449A, the spinel NiCo 2 O4 catalyst does not introduce precious metal platinum, but the performance of the catalyst is far behind that of platinum-based catalysts. Low-platinum catalysts also have the problem of low activity. Due to problems such as carrier corrosion and migration and agglomeration of precious metals, the stability of platinum-carbon binary catalysts is poor.

[0004] For platinum alloy catalysts, the incorporation of transition metals can improve the performance of the catalyst. In patent CN113258090A, the stability of the alloy catalyst was improved by doping with transition metals Fe, Co, and Ni, but the initial activity was low; therefore, on the basis of not increasing the cost of the catalyst, developing a new hydrogen fuel cell catalyst and its preparation method, which has high initial activity and significantly improved the stability of the catalyst, has become the top priority of research. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a hydrogen fuel cell catalyst and a preparation method thereof. The present invention is based on research on a platinum alloy catalyst and improves the stability of the catalyst by structural modification. The catalyst uses fullerene as a carrier, Pt and a PtAu alloy as active components, and has a three-layer structure with fullerene as an inner layer, a PtAu alloy as a middle layer, and a Pt layer as an outermost layer. An alloy catalyst with high initial activity is prepared, and the durability of the catalyst is significantly improved.

[0006] The technical solution adopted by the present invention is:

[0007] A hydrogen fuel cell catalyst, wherein: the hydrogen fuel cell catalyst comprises a carrier, the carrier is fullerene, the surface of the fullerene is loaded with a PtAu alloy, and the surface of the PtAu alloy is loaded with Pt.

[0008] A method for preparing a hydrogen fuel cell catalyst, wherein: the preparation method comprises the following steps:

[0009] S1. Carrier crushing: Weigh 5 g of fullerene, add the fullerene into a ball mill, ball mill for 0.5 to 1 h, and cool;

[0010] S2. Purification of the carrier: Add the fullerene crushed in step S1 to the 1,2,3-trimethylbenzene solution containing diazabicyclic ring, mix and stir for 0.5-2h, and then filter and separate;

[0011] S3. Modification of vector:

[0012] S31, weighing the filtered fullerene obtained in step S2 and mixing it with a strong oxidizing solution, ultrasonically dispersing, heating and stirring for 0.5-2h, filtering and washing, to obtain carrier 1;

[0013] S32, adding the carrier 1 obtained by filtration in S31 to the alcohol solution of perfluorosulfonic acid resin, stirring for 0.5 to 1 hour and then filtering and separating to obtain carrier 2;

[0014] S33, drying the carrier 2 separated in S32 at a temperature of 60°C to 80°C for 4 to 6 hours to obtain a carrier 3;

[0015] S4. Precious metal loading:

[0016] S41, dissolving chloroauric acid and chloroplatinic acid in an organic solvent, adding the carrier three obtained in step S33, and performing ultrasonic mixing and shear emulsification to obtain a mixed solution one;

[0017] S42, adjusting the pH of the mixed solution 1 obtained in step S41 to 9-13 with an alkaline solution to obtain a suspension;

[0018] S43, adding the suspension of step S42 into a reactor for heating and reduction to obtain a mixed solution II;

[0019] S44, cooling the mixed solution after the reaction in step S43, and allowing it to stand for precipitation and separation;

[0020] S45, filtering the product obtained in step S44, and repeatedly washing with deionized water until the conductivity of the filtrate is less than 100 μs / cm;

[0021] S46, vacuum drying the solid product separated in step S45 at 60-80° C. for 12-20 h;

[0022] S47, calcining the product obtained in step S46 at 800-1000° C. for 2-8 hours under an inert atmosphere, and cooling;

[0023] S48, dissolving the cooled product of step S47 in an organic solution, adding potassium tetrachloroplatinate, ultrasonically mixing, shearing and emulsifying, to obtain a mixed solution three;

[0024] S49, adjusting the pH of the mixed solution 3 obtained in step S48 to neutral with an alkaline solution to obtain a suspension;

[0025] S410, filtering the suspension in step S49;

[0026] S411, calcining and reducing the product obtained in step S10 under a hydrogen atmosphere to obtain a hydrogen fuel cell catalyst.

[0027] Preferably, in the method for preparing the hydrogen fuel cell catalyst, the dosage of fullerene in step S2 is 1-10%, and the concentration of diazabicycle is 0.5-5M.

[0028] Preferably, in the method for preparing the hydrogen fuel cell catalyst, the strong oxidizing solution in step S31 is one or more of hydrochloric acid, sulfuric acid, nitric acid and hydrogen peroxide, and the doping amount of fullerene is 1-10%.

[0029] Preferably, in the method for preparing the hydrogen fuel cell catalyst, the alcohol in step S32 is one or more of methanol, ethanol, propanol, ethylene glycol and isopropanol, the dosage of the perfluorosulfonic acid resin is 0.1-5%, and the dosage of the carrier one is 1-10%.

[0030] Preferably, the method for preparing the hydrogen fuel cell catalyst is characterized in that: the organic solvent in step S41 is one or more of ethanol, ethylene glycol and isopropanol, the molar ratio of chloroauric acid to chloroplatinic acid is 1:1-4, and the concentration of chloroplatinic acid is 1-10 g / L; the time of ultrasonic mixing in steps S41 and S48 is 0.5-2 h, and the time of shear emulsification is 0.2-1 h; the alkaline solution used in steps S42 and S49 is 0.1-1 M NaOH solution or KOH solution.

[0031] Preferably, in the method for preparing the hydrogen fuel cell catalyst, the heating reduction temperature in step S43 is 80-190° C., and the heating reduction time is 0.5-10 min; the filtration in steps S45 and S410 adopts positive pressure filtration or suction filtration; and the inert atmosphere in step S47 is nitrogen or argon.

[0032] Preferably, in the method for preparing the hydrogen fuel cell catalyst, the organic solvent in step S48 is one or two of methanol, ethanol, ethylene glycol, n-propanol and isopropanol; the dosage of the product in step S48 is 0.1-4%, and the concentration of potassium tetrachloroplatinate is 1-10 g / L.

[0033] Preferably, in the method for preparing the hydrogen fuel cell catalyst, the calcination temperature in step S411 is 200-300° C. and the calcination time is 2-8 hours.

[0034] Preferably, in the method for preparing the hydrogen fuel cell catalyst, the noble metal content of the hydrogen fuel cell catalyst obtained in step S411 is 40-60%.

[0035] Advantages of the present invention:

[0036] (1) The hydrogen fuel cell catalyst of the present invention uses fullerene as a carrier, Pt and Au as active components, loads precious metals by a polyol reduction method, then alloys by high-temperature calcination, and finally loads Pt on the alloy surface by hydrogen reduction to obtain a high-load and highly dispersed Pt-PtAu / fullerene catalyst; since fullerene itself is spherical, elliptical, tubular, etc. and has a high specific surface area, the metal dispersion is increased and the utilization rate of precious metals is improved; the surface modification treatment can enhance the proton conduction ability, and the carrier modified with perfluorosulfonic acid resin further enhances the H proton conduction ability and the hydrophobic property of the carrier.

[0037] (2) The hydrogen fuel cell catalyst of the present invention has a unique structure with fullerene as the inner layer, PtAu alloy as the middle layer, and a layer of Pt loaded on the outermost layer. First, the PtAu alloy is loaded on the surface of the fullerene to reduce the corrosion of the carrier. The introduction of the inert metal Au and the alloying treatment can reduce the precipitation of Pt and enhance the stability. Then, the outermost layer of Pt is embedded in the gaps on the surface of the PtAu alloy, which improves the dispersion of Pt and strengthens the anchoring, reduces the agglomeration and migration of the active component Pt, enhances the initial activity and improves the stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a comparison chart of the initial activity of the catalysts of Examples 1-2 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with specific drawings and embodiments.

[0040] Example 1

[0041] A method for preparing a hydrogen fuel cell catalyst comprises the following steps:

[0042] S1. Weigh 5 g of fullerene and add it into a ball mill with a mass ratio of large, medium and small balls of 2:5:3, and crush it at 400 rpm for 1 hour;

[0043] S2. Take 1 g of the crushed fullerene carrier and add it to 100 g of 1,2,3-trimethylbenzene solution, add 15 g of diazabicyclic and mix and stir for 2 h, then filter and separate;

[0044] S3. Modification of vector:

[0045] S31. The separated fullerene carrier was mixed with 1M hydrogen peroxide solution, ultrasonically dispersed for 20 minutes, heated and stirred for 2h, and then filtered to obtain a carrier;

[0046] S32. The filtered carrier was added to 100 g of ethanol solution, 0.8 g of perfluorosulfonic acid resin was added, and the carrier was separated by filtration after stirring for 0.5 h;

[0047] S33, drying the carrier 2 separated in S32 at a temperature of 40° C. for 6 h to obtain a carrier 3;

[0048] S4. Precious metal loading:

[0049] S41. Weigh chloroauric acid and chloroplatinic acid (0.2 g each of Au and Pt), dissolve in 80 g of ethanol and 20 g of water, add 1 g of the treated carrier III, mix by ultrasonication for 0.5 h, and emulsify by shearing for 0.5 h to obtain a mixed solution I;

[0050] S42. Adjust the pH to 13 with 0.5 M potassium hydroxide solution to obtain a suspension;

[0051] S43. The suspension was added to a reactor and heated at 90 ° C for 5 min to obtain a mixed solution II;

[0052] S44. Cooling down, allowing to settle until separation and then positive pressure filtration;

[0053] S45. Repeatedly washing with deionized water until the conductivity of the filtrate is less than 100 μs / cm;

[0054] S46. The separated product was dried under vacuum at 60° C. for 12 h;

[0055] S47. Calcinated at 800 ° C for 4 h under argon atmosphere and cooled;

[0056] S48. After cooling, 100 g of ethanol solution was added, potassium tetrachloroplatinate (Pt0.6 g) was weighed, ultrasonically mixed for 30 minutes, sheared and emulsified for 30 minutes to obtain a mixed solution III;

[0057] S49. The pH of the solution was adjusted to be close to neutral with 0.1 M potassium hydroxide solution to obtain a suspension;

[0058] S410. The suspension of step S49 is filtered and separated;

[0059] S411. The product obtained in step S410 is calcined at 300 degrees Celsius for 2 hours in a hydrogen atmosphere to obtain a hydrogen fuel cell catalyst.

[0060] Example 2

[0061] A method for preparing a hydrogen fuel cell catalyst comprises the following steps:

[0062] S1. Weigh 5 g of fullerene and add it into a ball mill with a mass ratio of large, medium and small balls of 2:5:3. Crush it in a ball mill at 400 rpm for 1 hour.

[0063] S2. Take 1 g of the crushed fullerene carrier and add it to 100 g of 1,2,3-trimethylbenzene solution, add 15 g of diazabicyclic and mix and stir for 2 h, then filter and separate;

[0064] S3. Modification of vector:

[0065] S31. The separated fullerene carrier was mixed with 1M hydrogen peroxide solution, ultrasonically dispersed for 20 minutes, heated and stirred for 2h, and then filtered to obtain a carrier;

[0066] S32. The filtered carrier was added to 100 g of ethanol solution, 0.8 g of perfluorosulfonic acid resin was added, and the carrier was separated by filtration after stirring for 0.5 h;

[0067] S33, drying the carrier 2 separated in S32 at a temperature of 60° C. for 5 h to obtain a carrier 3;

[0068] S4. Precious metal loading:

[0069] S41. Weigh chloroauric acid and chloroplatinic acid (0.1 g Au and 0.4 g Pt), dissolve in 200 g ethanol and 50 g water, add 1 g of the treated fullerene carrier, mix by ultrasonication for 0.5 h, and emulsify by shearing for 0.5 h to obtain a mixed solution 1;

[0070] S42. Adjust the pH to 13 with 0.5 M potassium hydroxide solution to obtain a suspension;

[0071] S43. The suspension was added to the reactor and heated at 90 ° C for 5 minutes to obtain a mixed solution II;

[0072] S44. Cooling down, allowing to settle until separation and then positive pressure filtration;

[0073] S45. Repeatedly washing with deionized water until the conductivity of the filtrate is less than 100 μs / cm;

[0074] S46. The separated product was dried under vacuum at 60° C. for 12 h;

[0075] S47. Calcinated at 800 ° C for 4 h under argon atmosphere and cooled;

[0076] S48. After cooling, 100 g of ethanol solution was added, potassium tetrachloroplatinate (Pt0.5 g) was weighed, ultrasonically mixed for 30 minutes, sheared and emulsified for 30 minutes to obtain a mixed solution III;

[0077] S49. The pH of the solution was adjusted to be close to neutral with 0.1 M potassium hydroxide solution to obtain a suspension;

[0078] S410. The suspension of step S49 is filtered and separated;

[0079] S411. The product obtained in step S410 is calcined at 300 degrees Celsius for 2 hours in a hydrogen atmosphere to obtain a hydrogen fuel cell catalyst.

[0080] Comparative Example 1

[0081] A method for preparing a hydrogen fuel cell catalyst comprises the following steps:

[0082] S1. Weigh 5 g of fullerene and add it into a ball mill with a mass ratio of large, medium and small balls of 2:5:3. Crush it in a ball mill at 400 rpm for 1 hour.

[0083] S2. Take 1 g of the crushed fullerene carrier and add it to 100 g of 1,2,3-trimethylbenzene solution, add 15 g of diazabicyclic and mix and stir for 2 h, then filter and separate;

[0084] S3. Weigh chloroauric acid and chloroplatinic acid (0.2 g Au and 0.2 g Pt respectively), dissolve in 80 g ethanol and 20 g water, add 1 g treated fullerene carrier, mix by ultrasonic for 0.5 h, and emulsify by shear for 0.5 h;

[0085] S4. Adjust the pH to 13 with 0.5 M potassium hydroxide solution to obtain a suspension;

[0086] S5. The suspension was added to the reactor and heated at 90 ° C for 5 minutes;

[0087] S6. Cool down, let stand and settle until separation, filter under positive pressure, and wash repeatedly with deionized water until the filtrate conductivity is less than 100 μs / cm;

[0088] S7. The separated product was dried under vacuum at 60°C for 12h;

[0089] S8. Calcinated at 800 ° C for 4 h under argon atmosphere and cooled;

[0090] S9. After cooling, add 100 g of ethanol solution, weigh potassium tetrachloroplatinate (including Pt0.6 g), ultrasonically mix for 30 minutes, and shear emulsify for 30 minutes;

[0091] S10. The pH of the solution was adjusted to be close to neutral with 0.1 M potassium hydroxide solution to obtain a suspension, which was separated by filtration;

[0092] S11. Calcinate and reduce the mixture at 300 degrees Celsius for 2 hours in a hydrogen atmosphere to obtain a hydrogen fuel cell catalyst.

[0093] Comparative Example 2

[0094] A method for preparing a hydrogen fuel cell catalyst comprises the following steps:

[0095] S1. Weigh 5 g of fullerene and add it into a ball mill with a mass ratio of large, medium and small balls of 2:5:3. Crush it in a ball mill at 400 rpm for 1 hour.

[0096] S2. Take 1 g of the crushed fullerene carrier and add it to 100 g of 1,2,3-trimethylbenzene solution, add 15 g of diazabicyclic and mix and stir for 2 h, then filter and separate;

[0097] S3. The separated fullerene carrier was mixed with 1M hydrogen peroxide solution, ultrasonically dispersed for 20 minutes, heated and stirred for 2 hours, and then filtered;

[0098] S4. The filtered carrier was added to 100g of ethanol solution, 0.8g of perfluorosulfonic acid resin was added, stirred for 0.5h, filtered and separated, and dried;

[0099] S5. Weigh chloroauric acid and chloroplatinic acid (0.2 g Au and 0.8 g Pt), dissolve in 400 g ethanol and 100 g water, add 1 g of the treated fullerene carrier, mix by ultrasonication for 0.5 h, and emulsify by shearing for 0.5 h;

[0100] S6. Adjust the pH to 13 with 0.5 M potassium hydroxide solution to obtain a suspension;

[0101] S7. The suspension was added to the reactor and heated at 90 ° C for 5 minutes;

[0102] S8. Cooling down, standing and settling until separation, positive pressure filtration, and repeated washing with deionized water until the filtrate conductivity is less than 100 μs / cm;

[0103] S9. The separated product was dried under vacuum at 60°C for 12h;

[0104] S10. Calcinate at 800°C for 4 h in an argon atmosphere and cool to obtain a PtAu alloy catalyst.

[0105] The catalysts prepared in Example 1-2 and Comparative Example 1-2 were evaluated for initial catalyst activity.

[0106] The current density at 0.9 V was compared by linear sweep voltammetry. The larger the current density, the higher the activity. Figure 1 At 0.9V, the current density of Example 1 and Example 2 is close, and greater than that of Comparative Example 1, while that of Comparative Example 2 is the smallest. Compared with Comparative Example 1, Example 1 shows that due to the pretreatment of the carrier graphene, the carrier surface has more defect holes, which are helpful for the dispersion and anchoring of precious metals; compared with Comparative Example 2, the initial activity of the three-layer Pt-PtAu / fullerene catalyst is significantly better than that of the traditional alloy catalyst. This is because the outermost layer of the three-layer catalyst is more stably agglomerated than Comparative Example 2 when loaded with Pt, and it is not easy to agglomerate and collapse, and Pt fits more firmly on the gaps and defects of the PtAu alloy. After 30,000 cycles through the electrochemical workstation, the half-wave potential of the three-layer Pt-PtAu / fullerene catalyst at 0.9V remains almost unchanged, and the stability is significantly improved.

[0107] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a hydrogen fuel cell catalyst, characterized in that: The preparation method comprises the following steps: S1. Carrier crushing: Weigh 5 g of fullerene, add the fullerene into a ball mill, ball mill for 0.5 to 1 h, and cool; S2. Purification of the carrier: Add the fullerene crushed in step S1 to the 1,2,3-trimethylbenzene solution containing diazabicyclic ring, mix and stir for 0.5-2h, and then filter and separate; S3. Modification of vector: S31, weighing the filtered fullerene obtained in step S2 and mixing it with a strong oxidizing solution, ultrasonically dispersing, heating and stirring for 0.5-2h, filtering and washing, to obtain carrier 1; S32, adding the carrier 1 obtained by filtration in S31 to the alcohol solution of perfluorosulfonic acid resin, stirring for 0.5 to 1 hour and then filtering and separating to obtain carrier 2; S33, drying the carrier 2 separated in S32 to obtain a carrier 3; S4. Precious metal loading: S41, dissolving chloroauric acid and chloroplatinic acid in an organic solvent, adding the carrier three obtained in step S33, and performing ultrasonic mixing and shear emulsification to obtain a mixed solution one; S42, adjusting the pH of the mixed solution 1 obtained in step S41 to 9-13 with an alkaline solution to obtain a suspension; S43, adding the suspension of step S42 into a reactor for heating and reduction to obtain a mixed solution II; S44, cooling the mixed solution after the reaction in step S43, and allowing it to stand for precipitation and separation; S45, filtering the product obtained in step S44, and repeatedly washing with deionized water until the conductivity of the filtrate is less than 100 μs / cm; S46, vacuum drying the solid product separated in step S45 at 60-80° C. for 12-20 h; S47, calcining the product obtained in step S46 at 800-1000° C. for 2-8 hours under an inert atmosphere, and cooling; S48, dissolving the cooled product of step S47 in an organic solution, adding potassium tetrachloroplatinate, ultrasonically mixing, shearing and emulsifying, to obtain a mixed solution three; S49, adjusting the pH of the mixed solution 3 obtained in step S48 to neutral with an alkaline solution to obtain a suspension; S410, filtering the suspension in step S49; S411, calcining and reducing the product obtained in step S10 under a hydrogen atmosphere to obtain a hydrogen fuel cell catalyst; In step S2, the doping amount of fullerene is 1-10%, and the concentration of diazabicyclic is 0.5-5M; In step S32, the alcohol is one or more of methanol, ethanol, propanol, ethylene glycol and isopropanol, the doping amount of the perfluorosulfonic acid resin is 0.1-5%, and the doping amount of the carrier 1 is 1-10%; In step S41, the organic solvent is one or more of ethanol, ethylene glycol and isopropanol, the molar ratio of chloroauric acid to chloroplatinic acid is 1:1-4, and the concentration of chloroplatinic acid is 1-10 g / L; the ultrasonic mixing time in steps S41 and S48 is 0.5-2 h, and the shear emulsification time is 0.2-1 h; the alkaline solution used in steps S42 and S49 is 0.1-1 M NaOH solution or KOH solution; The heating reduction temperature in step S43 is 80-190° C., and the heating reduction time is 0.5-10 min. The filtration in steps S45 and S410 is performed by positive pressure filtration or suction filtration. The inert atmosphere in step S47 is nitrogen or argon. The hydrogen fuel cell catalyst obtained in step S411 has a precious metal content of 40-60%.

2. The method for preparing a hydrogen fuel cell catalyst according to claim 1, characterized in that: In step S31, the strong oxidizing solution is one or more of hydrochloric acid, sulfuric acid, nitric acid and hydrogen peroxide, and the doping amount of fullerene is 1-10%.

3. The method for preparing a hydrogen fuel cell catalyst according to claim 1, characterized in that: The organic solvent in step S48 is one or two of methanol, ethanol, ethylene glycol, n-propanol and isopropanol; the dosage of the product in step S48 is 0.1-4%, and the concentration of potassium tetrachloroplatinate is 1-10 g / L.

4. The method for preparing a hydrogen fuel cell catalyst according to claim 1, characterized in that: In the step S411, the calcination temperature is 200-300° C. and the calcination time is 2-8 hours.

Citation Information

Patent Citations

  • Transition metal doped Pt / C fuel cell catalyst and preparation method thereof

    CN113258090A

  • Fuel cell catalyst and preparation method and application thereof

    CN113725449A

  • Carbon fiber supported metal catalyst as well as preparation method and application thereof

    CN103545536A

  • Ordered Pt-Au / C composite catalyst and preparation method thereof, and application of ordered Pt-Au / C composite catalyst in fuel cell

    CN112864407A

  • Fuel cell catalyst, preparation method thereof and fuel cell

    CN114188559A