A rapid manufacturing method for substrate-free light source

By directly attaching phosphor to the flip chip and using processes such as mold flip and dam enclosure, the existing substrate-free light-emitting diode packaging process is solved, and the efficient and low-cost packaging process is achieved. .

CN115148722BActive Publication Date: 2024-11-29AMICC OPTO ELECTRONICS TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210823381.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-13
Publication Date
2024-11-29
Estimated Expiration
2042-07-13

AI Technical Summary

Technical Problem

The existing substrateless light-emitting diode packaging process is complex, has low production efficiency, high cost, and is highly dependent on equipment, which requires multiple equipment to work together.

Method used

Using the positive and negative poles of the flip chip itself as the pad, directly attaching phosphor to the flip chip to form a new light emitting diode package, and through mold flip, dam glue, white silicone, adhesive and fluorescent film The combined process of packaging.

Benefits of technology

Improves production efficiency, reduces loss and equipment dependence, simplifies process flow, reduces production costs, and ensures high-precision packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115148722B_ABST
    Figure CN115148722B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for rapidly manufacturing a substrate-free light source. Blue light flip chips with consistent luminous intensity and wavelength are arranged in an array according to a designed spacing in advance, and then white silica gel is filled in the gaps between the blue light flip chips and then baked and cured in an oven. After curing, the white silica gel is ground to the same height as the blue light flip chips using a grinder, and then a fluorescent film is attached to the top using an adhesive and baked and cured. Finally, the array flip chips with the fluorescent film attached are cut along the middle of the gap to form an independent light-emitting diode package. The present invention abandons the substrate and welding wires, uses the positive and negative poles of the flip chip itself as pads, and directly attaches fluorescent powder to the flip chip itself to form a new light-emitting diode package, which not only improves production efficiency and reduces losses, but also ensures high precision and reduces dependence on equipment. Traditional packaging equipment such as a die bonding machine, a wire bonding machine, a testing machine, and a packaging machine are not required, and the process is simpler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of light-emitting chip manufacturing, and in particular relates to a rapid manufacturing method of a substrate-free light source. Background Art

[0002] Since its birth, light-emitting diodes have been widely used in people's lives after 60 years of development. In order to meet the huge market demand, people have been conducting more and more in-depth research on the packaging process of light-emitting diodes. Especially in the field of lighting, the demand for light-emitting diodes is the largest. Therefore, the packaging process of light-emitting diodes needs to be simple and efficient enough to meet the huge market demand.

[0003] The traditional LED packaging process is mainly to package the flip chip on the substrate. The wires of the light-emitting flip chip are welded on the substrate, and the packaging glue with phosphor is filled in the substrate. Finally, the substrate is cut into single pieces for testing and packaging. The main disadvantage of this packaging process is that the process flow is complicated, the production efficiency is low and the cost is high.

[0004] The mainstream technology of LEDs nowadays is to abandon the substrate and welding wires, use the positive and negative poles of the flip chip itself as pads, directly attach phosphors to the flip chip itself to form a new LED package, and test and package this new package. However, in the existing substrate-free chip manufacturing process, not only is the process more complicated and requires massive transfer, but it is also highly dependent on equipment and requires the cooperation of multiple equipment. In the actual production process, it leads to low efficiency and high production costs. Summary of the invention

[0005] The purpose of the present invention is to provide a method for rapid manufacturing of a substrate-free light source, which abandons the substrate and welding wires, uses the positive and negative poles of the flip chip itself as welding pads, and directly attaches phosphors to the flip chip itself to form a new light-emitting diode package. This not only improves production efficiency and reduces losses, but also ensures high precision and reduces dependence on equipment. It does not require traditional packaging equipment such as a die bonder, a wire bonder, a tester, and a packaging machine, and the process is simpler.

[0006] The specific technical solutions of the present invention are as follows:

[0007] A method for rapidly manufacturing a substrate-free light source, the specific steps are as follows:

[0008] S1: Arrange a plurality of flip chips in an array at a certain pitch on the blue film I, and the light-emitting surface of the flip chips is attached to the blue film I;

[0009] S2: Use a mold transfer machine to transfer the blue film I carrying the arrayed flip chips onto the UV film I. At this time, the light-emitting surface of the flip chip faces upwards and the electrode surface faces downwards and is attached to the UV film I;

[0010] S3: Use dam glue to form a dam around the UV film I;

[0011] S4: Pour white silicone into the dam, fill it evenly between the flip chips until it is flush with the top surface of the dam, and bake it in an oven to cure;

[0012] S5: using a grinding device to grind the upper surface of the white silicone and the top surface of the dam until the upper surface of the white silicone and the top surface of the dam are flush with the light-emitting surface of the flip chip, and the light-emitting surface of the flip chip is exposed;

[0013] S6: spray adhesive on the light-emitting surface of the flip chip and the white silicone surface, attach the fluorescent film to the flip chip and the white silicone surface, flatten them with a jig, remove bubbles and put them into the oven for baking and curing;

[0014] S7: using ultraviolet light to irradiate the UV film I to make it fall off, and flipping the flip chip with the fluorescent film after it falls off and attaching it to the UV film II. At this time, the fluorescent film is attached to the UV film II, and the electrode surface of the flip chip faces upward;

[0015] S8: using a cutting machine to evenly cut along the center line of the spacing between two flip chips to form a plurality of independent light emitting diode packages;

[0016] S9: Attach the cut light emitting diode package to the blue film II. At this time, the electrode surface of the flip chip is attached to the blue film II with the surface facing downward and the UV film II facing upward. Then, UV film II is irradiated with ultraviolet light to make it fall off, and the waste materials around it are picked out to obtain a packaged light source.

[0017] Preferably, the difference between the longest main wavelength and the shortest main wavelength of the flip chips arranged and distributed on the blue film I is ≤2.5nm; the difference between the highest luminous intensity and the lowest luminous intensity of the flip chips is ≤5%.

[0018] Preferably, the difference between the longest main wavelength and the shortest main wavelength of the flip chips arranged and distributed on the blue film I is 1 nm.

[0019] Preferably, the difference between the highest luminous intensity and the lowest luminous intensity of the flip chip is 2%.

[0020] Preferably, the height of the dam body is 0.18 mm.

[0021] Preferably, the adhesive in step S6 is transparent silicone.

[0022] Beneficial effects: The present invention discloses a method for rapidly manufacturing a substrate-free light source, which has the following advantages:

[0023] (1) The present invention pre-screens the light intensity and wavelength of the flip chip, which not only ensures the high consistency of the light efficiency of the packaged light-emitting diode, but also eliminates the need for testing, simplifies the process, and reduces costs;

[0024] (2) The present invention directly packages the flip chips arranged in an array, without the need to transfer and rearrange the flip chips one by one, thereby improving production efficiency;

[0025] (3) The cutting process of the present invention cuts the packaged flip chip and retains it on the carrier film, so it can be directly used for patching without packaging, which further simplifies the production process and improves production efficiency.

[0026] (4) The present invention does not require traditional packaging equipment such as a die bonding machine, a wire bonding machine, a testing machine, and a packaging machine, thereby reducing the dependence of the process on the equipment, reducing production costs, and making the process simpler. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a schematic diagram of the front structure in step S1;

[0028] Figure 2 is a schematic diagram of the front structure in step S2;

[0029] Figure 3 is a schematic diagram of the front structure in step S3;

[0030] Figure 4 is a schematic diagram of the cross-sectional structure in step S3;

[0031] Figure 5 is a schematic diagram of the front structure in step S4;

[0032] Figure 6 is a schematic diagram of the cross-sectional structure in step S4;

[0033] Figure 7 is a schematic diagram of the front structure in step S5;

[0034] Figure 8 is a schematic diagram of the cross-sectional structure in step S5;

[0035] Fig. 9 is a schematic diagram of the front structure in step S6;

[0036] Fig.10 is a schematic diagram of the cross-sectional structure in step S6;

[0037] Fig.11 is a schematic diagram of the front structure in step S7;

[0038] Fig.12 is a schematic diagram of the cross-sectional structure in step S7;

[0039] Fig.13 is a schematic diagram of the front structure in step S8;

[0040] Fig.14 is a schematic diagram of the front structure in step S9;

[0041] Fig.15 is a schematic diagram of the cross-sectional structure in step S9;

[0042] Fig.16 This is a schematic diagram of the product structure of Example 1.

[0043] In the figure: blue light flip chip 1, blue film I2, UV film I3, dam 4, white silicone 5, adhesive 6, fluorescent film 7, UV film II8, blue film II9. DETAILED DESCRIPTION

[0044] Several improvements and modifications are made to the present invention below in conjunction with the accompanying drawings, and these improvements and modifications should also be considered as the protection scope of the present invention.

[0045] Example 1

[0046] The flip chip used in this embodiment 1 is a blue light flip chip, and its specific preparation steps are as follows:

[0047] S1: Arrange a plurality of blue light flip chips 1 in an array on the blue film I2 according to the design requirement spacing, and the light emitting surface of the blue light flip chips 1 is attached to the blue film I2, such as Figure 1 As shown, the difference between the longest main wavelength and the shortest main wavelength of the blue light flip chip 1 arranged and distributed on the blue film I is 1nm, and the highest luminous intensity and the lowest luminous intensity of the blue light flip chip 1 differ by 2%;

[0048] S2: Use a mold transfer machine to transfer the blue film I2 carrying the arrayed blue flip chips 1 to the UV film I3. At this time, the light-emitting surface of the blue flip chip 1 faces upward, and the electrode surface faces downward and is attached to the UV film I3, and the spacing between the blue flip chips 1 remains unchanged, such as Figure 2 As shown;

[0049] S3: Use dam glue to form a dam 4 around the UV film I, and the height of the dam 4 is 0.18mm, which is slightly higher than the height of the blue light flip chip 1 0.15mm. Figure 3 and Figure 4 As shown;

[0050] S4: Pour white silica gel 5 into the dam 4, fill it evenly between the blue light flip chips 1 until it covers the blue light flip chips 1 and is flush with the top surface of the dam 4, and bake it in an oven to cure. Figure 5 and 6As shown in the figure, the hardness of the silicone is required to be above shore D 50.

[0051] S5: Use a grinding device to grind the white silicone 5 and the dam 4 until the thickness of the white silicone 5 and the height of the dam 4 are both 0.15 mm, flush with the light-emitting surface of the blue light flip chip 1. At this time, the white silicone 5 on the surface of the blue light flip chip 1 has been ground off and is prominent in the white silicone. Since the light-emitting surface of the blue light flip chip 1 is hard Al2O3, it is not affected during the grinding process. Figure 7 and 8 shown.

[0052] S6: spray adhesive 6 on the surface of blue flip chip 1 and white silicone 5, and attach fluorescent film 7 to the surface of blue flip chip 1 and white silicone 5, and flatten them with a jig, remove bubbles and then put them into an oven for baking and curing. Fig. 9 and 10 As shown, the adhesive is transparent silicone; the jig in the present invention is a prior art tool that can be used to flatten the film and remove bubbles.

[0053] S7: Use ultraviolet light to irradiate the UV film I3 to make it fall off, and flip the blue light flip chip 1 with the fluorescent film 7 after it falls off and attach it to the UV film II8. At this time, the fluorescent film 7 is attached to the UV film II8, and the electrode surface of the blue light flip chip 1 faces upwards. Fig.11 and 12 As shown;

[0054] S8: Use a cutting machine to evenly cut along the center line of the spacing between the blue flip chips to form multiple independent light emitting diode packages, such as Fig.13 As shown;

[0055] S9: attach the cut light emitting diode package to the blue film II9. At this time, the electrode surface of the blue flip chip 1 is attached to the blue film II9 with the surface facing downward and the UV film II8 facing upward. Then, UV film II8 is irradiated with ultraviolet light to make it fall off, and the waste around it is picked out. Fig.14 and 15 As shown, the packaged light source is obtained. Fig.16 shown.

[0056] In the present invention, the blue light flip chip can be arranged on the blue film I in a spacing array according to actual production requirements.

[0057] The above is only a practical description and is a preferred embodiment of the present invention. It should be noted that a person skilled in the art can make several improvements and modifications without departing from the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention.

Claims

1. A method for rapidly manufacturing a substrate-free light source, characterized in that: The specific steps are as follows: S1: Arrange a plurality of flip chips in an array at a certain pitch on the blue film I, and the light-emitting surface of the flip chips is attached to the blue film I; S2: Use a mold transfer machine to transfer the blue film I carrying the arrayed flip chips onto the UV film I. At this time, the light-emitting surface of the flip chip faces upwards and the electrode surface faces downwards and is attached to the UV film I; S3: Use dam glue to form a dam around the UV film I; S4: Pour white silicone into the dam, fill it evenly between the flip chips until it is flush with the top surface of the dam, and bake it in an oven to cure; S5: using a grinding device to grind the upper surface of the white silicone and the top surface of the dam until the upper surface of the white silicone and the top surface of the dam are flush with the light-emitting surface of the flip chip, and the light-emitting surface of the flip chip is exposed; S6: spray adhesive on the light-emitting surface of the flip chip and the white silicone surface, attach the fluorescent film to the flip chip and the white silicone surface, flatten them with a jig, remove bubbles and put them into the oven for baking and curing; S7: using ultraviolet light to irradiate the UV film I to make it fall off, and flipping the flip chip with the fluorescent film after it falls off and attaching it to the UV film II. At this time, the fluorescent film is attached to the UV film II, and the electrode surface of the flip chip faces upward; S8: using a cutting machine to evenly cut along the center line of the spacing between two flip chips to form a plurality of independent light emitting diode packages; S9: Attach the cut light emitting diode package to the blue film II. At this time, the electrode surface of the flip chip is attached to the blue film II with the surface facing downward and the UV film II facing upward. Then, UV film II is irradiated with ultraviolet light to make it fall off, and the waste materials around it are picked out to obtain a packaged light source.

2. The method for rapidly manufacturing a substrate-free light source according to claim 1, characterized in that: The difference between the longest main wavelength and the shortest main wavelength of the flip chips arranged and distributed on the blue film I is ≤2.5nm; the difference between the highest luminous intensity and the lowest luminous intensity of the flip chips is ≤5%.

3. The method for rapidly manufacturing a substrate-free light source according to claim 2, characterized in that: The difference between the longest main wavelength and the shortest main wavelength of the flip chips arranged and distributed on the blue film I is 1 nm.

4. The method for rapidly manufacturing a substrate-free light source according to claim 2, characterized in that: The difference between the highest and lowest luminous intensity of the flip chip is 2%.

5. The method for rapidly manufacturing a substrate-free light source according to claim 1, characterized in that: The height of the dam body of the dam is 0.18 mm.

6. The method for rapidly manufacturing a substrate-free light source according to claim 1, characterized in that: The adhesive in step S6 is transparent silica gel.

Citation Information

Patent Citations

  • Chip scale packaging method and structure for light-emitting device

    CN104851961A

  • White-light LED chip preparation method

    CN105720166A