Insulated oil and gas pipeline

By using polymeric materials containing cycloolefin compounds and ruthenium carbene catalysts as heat insulation layer on oil and gas transportation pipelines, combined with anti-corrosion layer, the problems of pipeline blockage and heat loss in high temperature environments are solved, and excellent thermal insulation, mechanics and Corrosion resistance improves conveying efficiency and economy.

CN115160719BActive Publication Date: 2024-11-22PAIMAI NEW MATERIALS (CHENGDU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210833723.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-08-06
Filing Date
2022-07-15
Publication Date
2024-11-22
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

Existing oil and gas transportation pipelines are prone to gas-water hydrolysis and waxy deposition in high temperature environments, resulting in shrinkage or blockage of pipeline channels, affecting oil and gas transportation efficiency, and the existing thermal conductivity of the insulation materials is insufficient, affecting economic benefits.

Method used

The insulation layer made of a double bond-containing cycloolefin compound and a ruthenium carbene catalyst through polymerization reaction, combined with organic fillers and inorganic fillers to form a heat-insulating material with low thermal conductivity, and coated with anti-corrosion layer and protection on the steel pipe. Coating to improve corrosion resistance.

Benefits of technology

It achieves excellent thermal insulation, mechanical properties and corrosion resistance, reduces heat loss and corrosion damage, and improves oil and gas transportation efficiency and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115160719B_ABST
    Figure CN115160719B_ABST
Patent Text Reader

Abstract

The invention discloses an insulated oil and gas pipeline, belonging to the field of oil and gas transportation pipelines. The insulated pipeline comprises a steel pipe and an insulation layer, wherein the insulation layer is prepared by polymerization reaction of raw materials including the following components: a cycloolefin compound containing one or more double bonds and at least one bridge ring, and a ruthenium carbene catalyst; wherein the mass ratio of the olefin compound to the ruthenium carbene catalyst is (2000-1000000): 1. The insulated oil and gas pipeline of the invention has excellent thermal insulation performance, mechanical performance and corrosion resistance, and can be used to prepare underground oil pipelines, submarine oil pipelines, and geothermal pipelines for transporting oil and gas, and provides additional protection for the pipeline on the premise of meeting the safe transportation of materials in the pipeline, preventing the loss of heat in the pipeline, and improving the transportation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil and gas transportation pipelines, and in particular relates to an insulated oil and gas pipeline. Background Art

[0002] With the development of the oil industry, especially offshore oil drilling, the requirements for thermal insulation and protection of offshore oil pipelines are gradually increasing. Multilayer fluid transmission pipes are common fluid transmission pipes in offshore oil construction that are stable and low-heat resistant. The biggest challenges they currently face are gas-water hydrolysis and wax deposition. The occurrence of these two phenomena is related to the fluid temperature. In extreme cases, the pipeline channel will be narrowed or blocked, resulting in reduced production. In some cases, the pipeline may even be required to be replaced. Therefore, in order to maintain the high-temperature working conditions of the oil pipeline in the seabed environment, it is usually necessary to coat the outside of the oil pipeline with a low conductivity insulation layer to prevent the formation of hydrolysis and wax deposition, which affects the transmission efficiency of the pump.

[0003] In addition to offshore oil drilling, onshore oil production also faces the same problem. Waxing in oil wells that produce paraffin-based and intermediate-based crude oil is an important factor affecting the pump inspection cycle of oil wells. When the wellbore lifts crude oil, heat is lost along the way, and the crude oil temperature is lower than the initial crystallization temperature of the wax. Wax crystal particles will precipitate and deposit on the surface of the oil flow and rods and pipes, especially when producing oil from old wells. At present, oil fields widely use anti-wax measures such as chemical or biological wax removal, magnetic wax removal, and sonic wax removal, as well as wax removal measures such as hot washing, electric heating pump rods, industrial frequency skin heating, and machinery to solve this problem. However, this measure has high fixed asset investment and requires operating expenses such as electricity and steam energy, which seriously affects the economic benefits of mining. Therefore, it is of great significance to develop an insulation material that can be used for underground oil pipelines.

[0004] In addition to oil extraction, the pipes used in underground heat source extraction also need to have excellent thermal insulation properties. At present, the use of underground heat sources is gradually increasing in various places, and the existing thermal fluid extraction does not take insulation, resulting in large heat losses. Some areas have begun to try to use vacuum insulated pipes to extract geothermal water, but vacuum insulated pipes are expensive, which seriously affects the economic benefits of heat extraction. Therefore, various thermal extraction companies are also seeking to use various thermal insulation pipes to try to solve this problem.

[0005] Chinese patent application with application number CN201480043569.4 discloses a thermal insulation material, which comprises: a resin composition comprising a cyclic olefin composition and a catalyst composition comprising at least one metal carbene olefin metathesis catalyst, wherein the cyclic olefin composition comprises 10.0 mol% to 80.0 mol% of at least one cyclic olefin containing polyunsaturation and 20.0 mol% to 90.0 mol% of at least one cyclic olefin containing monounsaturation, wherein the at least one cyclic olefin containing polyunsaturation is selected from dicyclopentadiene, tricyclopentadiene, cyclopentadiene tetramer, cyclopentadiene pentamer, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-isopropenyl-2-norbornene, 5-propenyl-2-norbornene and 5-butenyl-2-norbornene, and wherein the at least one cyclic olefin containing monounsaturation is selected from C2-12 hydrocarbon-substituted norbornene. However, the thermal conductivity of the thermal insulation material is 0.175 W / (m·K), and its thermal insulation performance needs to be further improved. Summary of the invention

[0006] The object of the present invention is to provide a heat-insulating pipeline having excellent heat-insulating properties, mechanical properties and corrosion resistance, and the heat-insulating pipeline can be used in the field of oil and gas transportation.

[0007] The present invention provides an insulated pipeline, which comprises a steel pipe and an insulating layer. The insulating layer is prepared by polymerization reaction of raw materials including the following components: a cycloolefin compound containing one or more double bonds and at least one bridge ring, and a ruthenium carbene catalyst; wherein the mass ratio of the olefin compound to the ruthenium carbene catalyst is (2000-1000000):1.

[0008] Furthermore, the mass ratio of the olefin compound to the ruthenium carbene catalyst is (2000-80000):1;

[0009] And / or, the olefin compound comprises one or more of dicyclopentadiene or its derivatives, tricyclopentadiene or its derivatives, tetracyclopentadiene or its derivatives, norbornene or its derivatives, and the content of dicyclopentadiene or its derivatives is 25wt.% to 100wt.%;

[0010] And / or, the structure of the ruthenium carbene catalyst is as shown in Formula I:

[0011]

[0012] Among them, L 1 , L 3 Each independently selected from electron donating groups;

[0013] n is 0 or 1;

[0014] m is 0, 1 or 2;

[0015] k is 0 or 1,

[0016] X 1 , X 2 Each independently selected from anionic ligands;

[0017] L 2 is an electron-donating group, R 1 , R 2 Each independently selected from H, a hydrocarbon group, a group containing a heteroatom, or R 1 and R 2 Connect into a ring;

[0018] Or, R 1 and R 2 Connect into a ring, L 2 and R 2 Connect into a ring.

[0019] Further, the mass ratio of the olefin compound to the ruthenium carbene catalyst is (3000-50000):1, preferably 3000:1, 4000:1, 5000:1, 10000:1, 20000:1, 25000:1, 40000:1, 50000:1;

[0020] And / or, the derivative is a product obtained by modification with one or more functional groups, wherein the functional groups are selected from C 1~10 Alkyl, C 1~10 Alkoxy, C 1~10 One or more of an alkylene group, a hydroxyl group, a carboxyl group, an anhydride group, a phenyl group, a halogen group, an amino group, an acrylate group, and a methacrylate group; preferably, the C 1~10 The alkyl group is selected from methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl or decyl, and the C 1~10 The alkoxy group is selected from methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy or decyloxy, wherein the C 1~10 The alkylene group is selected from methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene or decylene;

[0021] And / or, in the olefin compound, the content of dicyclopentadiene or its derivatives is 36wt.% to 73wt.%;

[0022] And / or, the structure shown in Formula I is Formula II or Formula III:

[0023]

[0024] Among them, R3 , R 4 , R 5 , R 6 Each independently selected from hydrogen, halogen, unsubstituted or replaced by R a Substituted with the following groups: C 1~5 Alkyl, C 1~5 Alkoxy; R a Selected from phenyl, C 1~5 Alkyl, halogen;

[0025] X 1 , X 2 Each independently selected from halogen, preferably chlorine;

[0026] R 7 Selected from phenyl, C 2~4 Alkenyl, C 2~4 Alkynyl, C 1~5 Alkyl, C 1~5 Alkoxy;

[0027] R 8 Selected from PPh 3 , PCy 3 or

[0028] R 9 Selected from C 1~3 Alkyl, C 1~3 Alkoxy;

[0029] R 10 Selected from nitro, C 1~5 Alkyl, C 1~5 Alkoxy, SO 2 NMe 2 .

[0030] Further, the olefin compound comprises the following components: component 1: dicyclopentadiene; component 2: tricyclopentadiene; component 3: tetracyclopentadiene; component 4: one or more of dicyclopentadiene derivatives, norbornene or their derivatives;

[0031] And / or, the ruthenium carbene catalyst is selected from one or more of the following structures:

[0032]

[0033]

[0034] Furthermore, in the olefin compound, the mass ratio of component 1 to component 2 is 1:(0.10-0.90), preferably 1:(0.30-0.74);

[0035] And / or, in the olefin compound, the mass ratio of component 1 to component 3 is 1:(0.01-0.09), preferably 1:(0.02-0.07);

[0036] And / or, in the olefin compound, the mass ratio of component 1 to component 4 is 1:(0-1.50), preferably 1:(0.04-1.24).

[0037] Further, the composition of the olefin compound is: 70wt.% dicyclopentadiene, 25wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 3wt.% hydroxydicyclopentadiene;

[0038] Or, the composition of the olefin compound is: 55wt.% dicyclopentadiene, 27wt.% tricyclopentadiene, 2.4wt.% tetracyclopentadiene, 15.6wt.% hydroxydicyclopentadiene;

[0039] Or, the composition of the olefin compound is: 42wt.% dicyclopentadiene, 31wt.% tricyclopentadiene, 3wt.% tetracyclopentadiene, 24wt.% nadic anhydride;

[0040] Or, the composition of the olefin compound is: 73wt.% of dicyclopentadiene, 22wt.% of tricyclopentadiene, 1.6wt.% of tetracyclopentadiene, and 3.4wt.% of nadic anhydride;

[0041] Or, the composition of the olefin compound is: 36wt.% of dicyclopentadiene, 18wt.% of tricyclopentadiene, 1.4wt.% of tetracyclopentadiene, and 44.6wt.% of 5-ethylidene-2-norbornene;

[0042] Or, the composition of the olefin compound is: 65wt.% dicyclopentadiene, 25wt.% tricyclopentadiene, 2wt.% tetracyclopentadiene, and 8wt.% 5-ethylidene-2-norbornene.

[0043] Furthermore, it also contains one or more of the following raw materials: organic filler, inorganic filler, thermosetting resin, organic solvent;

[0044] Preferably, the organic filler is one or more of polystyrene, styrene-butadiene-styrene block copolymer, ethylene propylene copolymer, acrylonitrile-butadiene-styrene plastic, styrene-ethylene-butylene-styrene block copolymer, adhesion promoter, light stabilizer, antioxidant, adhesion aid or flame retardant; the inorganic filler is one or more of calcium carbonate, aluminum oxide, magnesium oxide, boron nitride or glass beads; the thermosetting resin is one or more of epoxy resin, benzoxazine resin, cyanate resin, bismaleimide resin, polyphenylene ether resin, phenolic resin; the organic solvent is one or more of dichloromethane, toluene, methyl ethyl ketone, butanone, tetrahydrofuran, N,N-dimethylformamide.

[0045] The flame retardant is selected from one or more of ammonium polyphosphate, red phosphorus, decabromodiphenylethane, hexabromocyclododecane, DOPO, DiDOPO, and triphenyl phosphate.

[0046] Furthermore, it also contains one or more of the following raw materials: antioxidant, toughening agent, bonding aid, glass microspheres;

[0047] Preferably, the antioxidant is one or more of antioxidant TPP, antioxidant 164, antioxidant 1076, antioxidant 1010, antioxidant BHT, antioxidant CA, antioxidant BHA, antioxidant TNP, and antioxidant DLTP; the toughening agent is one or more of ethylene propylene copolymer, ethylene propylene diene monomer rubber EPDM, SEBS, SBS, POE, and EMA; the bonding aid is an isocyanate or a silane coupling agent, and the silane coupling agent is preferably one or more of A151, A171, A172, KH550, KH560, and KH570, and the isocyanate is preferably diphenylmethane diisocyanate.

[0048] Furthermore, the thermal insulation layer is prepared by polymerization reaction of the following raw materials in parts by weight: 100 parts of olefin compounds, 0.5-5 parts of antioxidants, 0-10 parts of toughening agents, 0-5 parts of bonding aids, 0-80 parts of glass microspheres, and ruthenium carbene catalysts; the glass microspheres are preferably hollow glass microspheres;

[0049] Preferably, the thermal insulation layer is prepared by polymerization reaction of raw materials containing the following parts by weight: 100 parts of olefin compounds, 1-2 parts of antioxidants, 2-8 parts of toughening agents, 0-3 parts of bonding aids, 0-50 glass beads, and ruthenium carbene catalysts.

[0050] Furthermore, the thermal insulation layer is prepared by polymerization reaction of raw materials containing the following parts by weight: 100 parts of olefin compounds, 1 part of antioxidant, 2 parts of toughening agent, 3 parts of bonding aid, 24-50 parts of glass microspheres, and ruthenium carbene catalyst.

[0051] Furthermore, the thermal conductivity of the thermal insulation layer is 0.160 W / (mK) or less, preferably 0.152 W / (m·K) or less, and more preferably 0.107 to 0.152 W / (m·K).

[0052] Furthermore, the method for preparing the thermal insulation layer comprises the following steps:

[0053] The ruthenium carbene catalyst is dissolved in an organic solvent, then evenly mixed with the remaining raw materials, injected into a mold for polymerization reaction and molding.

[0054] Furthermore, the organic solvent is dichloromethane or toluene, and the molding conditions include keeping warm at 35-100° C. for 10-50 minutes.

[0055] Furthermore, the molding conditions are: firstly keeping the temperature at room temperature for 10 to 30 minutes, and then keeping the temperature at 50 to 90° C. for 20 to 40 minutes.

[0056] In the present invention, "room temperature" refers to 25±5°C.

[0057] Furthermore, the thermal insulation pipe also includes one or more of an anti-corrosion layer, a protective coating, and an adhesive layer.

[0058] Further, the anti-corrosion layer includes one or more of epoxy phenolic resin or its derivatives, polyphenylene sulfide or its derivatives, fluoropolymer or its derivatives, polyimide or its derivatives;

[0059] and / or, the protective coating is composed of a solid polymeric material;

[0060] And / or, the adhesive layer consists of a liquid adhesive.

[0061] Furthermore, the insulated pipe also includes a second insulation layer, the second insulation layer is composed of a material with insulation function, and the insulation layer is closer to the steel pipe than the second insulation layer.

[0062] Further, the second insulation layer includes one or more of thermoplastic plastics, plastic foams, and composite foams;

[0063] Or, the second thermal insulation layer comprises one or more of foamed polypropylene homopolymer or copolymer, polybutylene, polyethylene, polystyrene, high impact polystyrene, modified polystyrene, cross-linked or partially cross-linked polypropylene, cross-linked or partially cross-linked polyethylene;

[0064] Or, the second insulation layer comprises one or more of polycarbonate, polyphenylene oxide, polypropylene, polybutadiene, polyamide, polybutylene terephthalate, polyethylene terephthalate, acrylonitrile-butadiene-styrene, acrylonitrile-styrene-acrylate, polyetherimide, polymethylpentene, cycloolefin copolymer, and partially cross-linked thermoplastic elastomer; the polyamide is preferably polyamide 12 or 612;

[0065] Or, the second thermal insulation layer comprises an epoxy-modified polymer network, the modified polymer network comprises an epoxy-urethane hybrid system or an epoxy-olefin hybrid system, and its operating temperature is 90° C. to 140° C.;

[0066] Alternatively, the second thermal insulation layer includes one or more elastomers selected from the group consisting of HNBR, nitrile rubber, silicone rubber, ethylene-propylene diene monomer rubber, and butyl rubber.

[0067] Furthermore, the heat-insulating pipeline includes a steel pipe and a heat-insulating layer from the inside to the outside; preferably, an adhesive layer is included between the steel pipe and the heat-insulating layer;

[0068] Or, the insulated pipeline includes a steel pipe, an anti-corrosion layer and an insulation layer in sequence from the inside to the outside; preferably, an adhesive layer is included between the steel pipe and the anti-corrosion layer, and an adhesive layer is included between the anti-corrosion layer and the insulation layer;

[0069] Alternatively, the insulated pipe includes a steel pipe, an anti-corrosion layer, an insulation layer and a protective coating from the inside to the outside; preferably, an adhesive layer is included between the steel pipe and the anti-corrosion layer, an adhesive layer is included between the anti-corrosion layer and the insulation layer, and an adhesive layer is included between the insulation layer and the protective coating.

[0070] In the present invention, "plurality" means two or more.

[0071] Compared with the prior art, the insulated pipe of the present invention comprises an insulating layer made of the specific insulating material of the present invention, and the specific insulating material has the following beneficial effects:

[0072] (1) The thermal conductivity of the thermal insulation material is as low as 0.107-0.152 W / (m·K), and the thermal insulation performance is excellent;

[0073] (2) The thermal insulation material has excellent mechanical properties. Therefore, even without adding an additional protective coating, the thermal insulation pipe of the present invention also has excellent mechanical properties;

[0074] (3) The thermal insulation material has excellent anti-corrosion properties and can protect the transport pipeline from being corroded by acid, alkali or salt water. Therefore, even without an additional anti-corrosion layer, the thermal insulation pipeline of the present invention also has excellent anti-corrosion properties.

[0075] On the basis of the above-mentioned beneficial effects of the specific thermal insulation material, the thermal insulation pipe of the present invention including the thermal insulation layer made of the specific thermal insulation material also has excellent thermal insulation performance, mechanical properties and corrosion resistance.

[0076] In addition, the insulated pipe of the present invention may be coated with a protective coating to further resist deep static pressure.

[0077] The thermal insulation pipe of the present invention may also be coated with an anti-corrosion layer to further improve the anti-corrosion performance.

[0078] In summary, the insulated pipe of the present invention has excellent thermal insulation properties, mechanical properties and corrosion resistance, and can be used to prepare underground oil pipelines, submarine oil pipelines, and geothermal pipelines for transporting oil and gas. It provides additional protection for the pipeline while ensuring the safe transportation of materials in the pipeline, prevents the loss of heat in the pipeline, and improves the transportation efficiency.

[0079] The heat-insulated pipe preparation method of the present invention is safe, environmentally friendly, low in energy consumption, and suitable for industrial production.

[0080] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.

[0081] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0082] Figure 1 It is a schematic diagram of the cross-sectional structure of an insulated oil and gas pipeline 10 according to the present invention, comprising a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, a protective coating 4, an adhesive layer 5, an insulating layer 6, and a protective coating 7.

[0083] Figure 2 It is a schematic diagram of the cross-sectional structure of an insulated oil and gas pipeline 12 according to the present invention, comprising a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulating layer 6, and a protective coating 7.

[0084] Figure 3 It is a schematic diagram of the cross-sectional structure of the insulated oil and gas pipeline 14 according to the present invention, including a steel pipe 1, an anti-corrosion layer 22, an insulation layer 6, and a protective coating 7.

[0085] Figure 4 It is a schematic diagram of the cross-sectional structure of the insulated oil and gas pipeline 16 according to the present invention, including a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulating layer 6, an adhesive layer 9, a second insulating layer 8, and a protective coating 7.

[0086] Figure 5 It is a schematic diagram of the cross-sectional structure of the insulated oil and gas pipeline 17 according to the present invention, including a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulation layer 6, a second insulation layer 8, and a protective coating 7.

[0087] Figure 6 It is a schematic diagram of the cross-sectional structure of an insulated oil and gas pipeline 18 according to the present invention, including a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, a protective coating 4, an adhesive layer 5, and an insulating layer 6.

[0088] Figure 7 It is a schematic diagram of the cross-sectional structure of the insulated oil and gas pipeline 20 according to the present invention, including a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, and an insulation layer 6.

[0089] Figure 8 It is a schematic diagram of the cross-sectional structure of the insulated oil and gas pipeline 24 according to the present invention, including a steel pipe 1, an anti-corrosion layer 2, and an insulation layer 6.

[0090] Fig. 9 It is a schematic diagram of the cross-sectional structure of the insulated oil and gas pipeline 26 according to the present invention, including a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulating layer 6, an adhesive layer 9, and a second insulating layer 8.

[0091] Fig.10 It is a schematic diagram of the longitudinal cross-sectional structure of the pipe joint area of ​​two insulated oil and gas pipelines welded together, including a steel pipe 1, an anti-corrosion layer 22, an insulation layer 6, a protective coating 7, an on-site joint insulation layer 13, an on-site joint anti-corrosion layer 15, a chamfered end 19, and a welding area 11.

[0092] The above-mentioned thermal insulation layer 6 is composed of a thermal insulation material in embodiments 1 to 14. DETAILED DESCRIPTION

[0093] The raw materials and equipment used in the present invention are all known products, which are obtained by purchasing commercially available products. The glass microspheres used in the following examples are commercially available hollow glass microspheres.

[0094] The raw material parts described in the following examples are parts by weight.

[0095] In the following examples, the compositions of the olefin mixtures A to F containing a bridged ring structure and having one or more double bonds are respectively:

[0096] Olefin mixture A containing a bridged ring structure and one or more double bonds: 70 wt.% dicyclopentadiene, 25 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, and 3 wt.% hydroxydicyclopentadiene.

[0097] Olefin mixture B containing a bridged ring structure and one or more double bonds: 55 wt.% dicyclopentadiene, 27 wt.% tricyclopentadiene, 2.4 wt.% tetracyclopentadiene, 15.6 wt.% hydroxydicyclopentadiene.

[0098] Olefin mixture C containing a bridged ring structure and one or more double bonds: 42 wt.% of dicyclopentadiene, 31 wt.% of tricyclopentadiene, 3 wt.% of tetracyclopentadiene, and 24 wt.% of nadic anhydride.

[0099] Olefin mixture D containing a bridged ring structure and one or more double bonds: 73 wt.% of dicyclopentadiene, 22 wt.% of tricyclopentadiene, 1.6 wt.% of tetracyclopentadiene, and 3.4 wt.% of nadic anhydride.

[0100] Olefin mixture E containing a bridged ring structure and one or more double bonds: 36 wt.% of dicyclopentadiene, 18 wt.% of tricyclopentadiene, 1.4 wt.% of tetracyclopentadiene, and 44.6 wt.% of 5-ethylidene-2-norbornene.

[0101] Olefin mixture F containing a bridged ring structure and having one or more double bonds: 65 wt.% dicyclopentadiene, 25 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, 8 wt.% 5-ethylidene-2-norbornene.

[0102] In the following examples, 1 # Catalyst ~ 10 # The catalysts were purchased from commercial products. The structures are as follows:

[0103] Embodiment 1:

[0104] 3400 g of olefin mixture A having one or more double bonds and containing a bridged ring structure were added with 34 g of antioxidant 1076, 68 g of toughening agent ethylene propylene copolymer, 68 g of bonding agent diphenylmethane diisocyanate (abbreviated as MDI), 34 g of bonding agent KH550, and 68 g of ruthenium carbene catalyst solution (a ruthenium carbene catalyst dissolved in dichloromethane), and mixed well to obtain a mixture; the ruthenium carbene catalyst here is 1 # The mass ratio of the catalyst, olefin mixture A and ruthenium carbene catalyst is 25000:1.

[0105] The mixture was poured into a mold, placed at room temperature for 20 minutes, then placed in an oven and heated to 70°C, kept warm for 30 minutes, and then the mold was opened to obtain a thermal insulation material.

[0106] The specifications of the thermal insulation materials produced in Example 1 to Example 14 are: outer diameter 100 mm, inner diameter 76 mm, length 1000 mm, and thickness 12 mm.

[0107] Embodiment 2:

[0108] 3400 g of olefin mixture A having one or more double bonds and containing a bridged ring structure were added with 34 g of antioxidant 1076, 272 g of toughening agent ethylene propylene copolymer, 68 g of bonding agent MDI, 34 g of bonding agent KH550, and 68 g of ruthenium carbene catalyst solution (a ruthenium carbene catalyst dissolved in dichloromethane), and mixed well to obtain a mixture; the ruthenium carbene catalyst was 1 # The mass ratio of the catalyst, olefin mixture A and ruthenium carbene catalyst is 25000:1.

[0109] The mixture was poured into a mold, placed at room temperature for 20 minutes, then placed in an oven and heated to 70°C, kept warm for 30 minutes, and then the mold was opened to obtain a thermal insulation material.

[0110] Embodiment three:

[0111] 15 g of antioxidant 1076, 30 g of toughening agent ethylene propylene copolymer, 30 g of bonding agent MDI, 15 g of bonding agent KH550, 360 g of glass microspheres K20, and 30 g of ruthenium carbene catalyst solution (a ruthenium carbene catalyst dissolved in dichloromethane) were added to 1500 g of olefin mixture A containing a bridged ring structure and one or more double bonds, and the mixture was uniformly mixed to obtain a mixture; the ruthenium carbene catalyst was 1 # The mass ratio of the catalyst, olefin mixture A and ruthenium carbene catalyst is 25000:1.

[0112] The mixture was poured into a mold, placed at room temperature for 20 minutes, then placed in an oven and heated to 70°C, kept warm for 30 minutes, and then the mold was opened to obtain a thermal insulation material.

[0113] Embodiment 4:

[0114] 18 g of antioxidant 1076, 36 g of toughening agent ethylene propylene copolymer, 36 g of bonding agent MDI, 18 g of bonding agent KH550, 900 g of glass microspheres K60, and 36 g of ruthenium carbene catalyst solution (a ruthenium carbene catalyst dissolved in dichloromethane) were added to 1800 g of olefin mixture A containing a bridged ring structure and one or more double bonds, and the mixture was uniformly mixed to obtain a mixture; the ruthenium carbene catalyst was 1 # The mass ratio of the catalyst, olefin mixture A and ruthenium carbene catalyst is 25000:1.

[0115] The mixture was poured into a mold, placed at room temperature for 20 minutes, then placed in an oven and heated to 70°C, kept warm for 30 minutes, and then the mold was opened to obtain a thermal insulation material.

[0116] Embodiment five:

[0117] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture B. # Catalyst replaced by 2 # Catalyst, and control the olefin mixture B and 2 # The mass ratio of the catalyst is 10000:1.

[0118] Embodiment six:

[0119] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture B. # Catalyst replaced with 3 # Catalyst, and control the olefin mixture B and 3 # The mass ratio of the catalyst is 20000:1.

[0120] Embodiment seven:

[0121] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture C. # Catalyst replaced by 4 # Catalyst, and control the olefin mixture C and 4 # The mass ratio of the catalyst is 5000:1.

[0122] Embodiment eight:

[0123] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture C. # Catalyst replaced with 5 # Catalyst, and control the olefin mixture C and 5 # The mass ratio of the catalyst is 10000:1.

[0124] Embodiment nine:

[0125] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture D. # Catalyst replaced with 6 # Catalyst, and control the olefin mixture D and 6 # The mass ratio of the catalyst is 40000:1.

[0126] Embodiment ten:

[0127] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture D. # Catalyst replaced with 7 # Catalyst, and control the olefin mixture D and 7 # The mass ratio of the catalyst is 20000:1.

[0128] Embodiment eleven:

[0129] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture E. # Catalyst replaced with 8 # Catalyst, and control the olefin mixture E and 8 # The mass ratio of the catalyst is 50000:1.

[0130] Embodiment 12:

[0131] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture E. # Catalyst replaced with 9 # Catalyst, and control the olefin mixture E and 9 # The mass ratio of the catalyst is 3000:1.

[0132] Embodiment 13:

[0133] The heat insulating material was prepared by referring to the preparation method of Example 1, except that the olefin mixture A in Example 1 was replaced by the olefin mixture F. # The catalyst is replaced with 10 catalyst, and the olefin mixture F is controlled to be 10 # The mass ratio of the catalyst is 4000:1.

[0134] Embodiment 14:

[0135] 1800 g of olefin mixture A containing a bridged ring structure and one or more double bonds was added with 18 g of antioxidant 1076 and 36 g of ruthenium carbene catalyst solution (a ruthenium carbene catalyst was dissolved in dichloromethane), and the mixture was uniformly mixed to obtain a mixture; the ruthenium carbene catalyst was 1 # The mass ratio of the catalyst, olefin mixture A and ruthenium carbene catalyst is 25000:1.

[0136] The mixture was poured into a mold, placed at room temperature for 20 minutes, then placed in an oven and heated to 70°C, kept warm for 30 minutes, and then the mold was opened to obtain a thermal insulation material.

[0137] Table 1. Raw material formula of thermal insulation materials in various embodiments (parts by weight)

[0138]

[0139] Embodiment 15: The heat-insulated oil and gas pipeline 10 of the present invention

[0140] The cross-sectional structure of the insulated oil and gas pipeline 10 of the present invention is as follows: Figure 1 The insulated oil and gas pipeline 10 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, a protective coating 4, an adhesive layer 5, an insulating layer 6, and a protective coating 7.

[0141] The steel pipe 1 is one or more sections of steel pipe, the adhesive layer 3 provides an adhesive effect between the anti-corrosion layer 2 and the protective coating 4, and the adhesive layer 5 provides an adhesive effect between the protective coating 4 and the thermal insulation layer 6. The protective coating 4 may also include a thermal insulation layer, and may include an extrudable thermoplastic or elastic resin.

[0142] Example 16: Insulated oil and gas pipeline 12 of the present invention

[0143] The cross-sectional structure of the insulated oil and gas pipeline 12 of the present invention is as follows: Figure 2 The insulated oil and gas pipeline 12 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulation layer 6, and a protective coating 7.

[0144] The adhesive layer 3 provides an adhesive effect between the anti-corrosion layer 2 and the thermal insulation layer 6 .

[0145] Embodiment 17: The heat-insulated oil and gas pipeline 14 of the present invention

[0146] The cross-sectional structure of the insulated oil and gas pipeline 14 of the present invention is as follows: Figure 3 The insulated oil and gas pipeline 14 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 22, an insulating layer 6, and a protective coating 7 in sequence.

[0147] Embodiment 18: The heat-insulated oil and gas pipeline 16 of the present invention

[0148] The cross-sectional structure of the insulated oil and gas pipeline 16 of the present invention is as follows: Figure 4 The insulated oil and gas pipeline 16 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulating layer 6, an adhesive layer 9, a second insulating layer 8, and a protective coating 7.

[0149] The adhesive layer 3 provides an adhesive effect between the anti-corrosion layer 2 and the thermal insulation layer 6. The adhesive layer 9 may have the same or different composition as one or both of the thermal insulation layer 6 and the second thermal insulation layer 8, and may be used as an adhesive between the thermal insulation layer 6 and the second thermal insulation layer 8.

[0150] The adhesive layer 9 is not necessarily required, and for example, when there is no second thermal insulation layer 8 or when the thermal insulation layer 6 and the second thermal insulation layer 8 can be directly bonded to each other, the adhesive layer 9 may not be included.

[0151] Example 19: Insulated oil and gas pipeline 17 of the present invention

[0152] The cross-sectional structure of the insulated oil and gas pipeline 17 of the present invention is as follows: Figure 5 The insulated oil and gas pipeline 17 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulation layer 6, a second insulation layer 8, and a protective coating 7.

[0153] The adhesive layer 3 provides an adhesive effect between the anti-corrosion layer 2 and the thermal insulation layer 6 .

[0154] Example 20: Insulated oil and gas pipeline 18 of the present invention

[0155] The cross-sectional structure of the insulated oil and gas pipeline 18 of the present invention is as follows: Figure 6 The insulated oil and gas pipeline 18 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, a protective coating 4, an adhesive layer 5, and an insulation layer 6.

[0156] The bonding layer 3 provides bonding between the anti-corrosion layer 2 and the protective coating 4 ; the bonding layer 5 provides bonding between the protective coating 4 and the thermal insulation layer 6 .

[0157] Embodiment 21: Insulated oil and gas pipeline 20 of the present invention

[0158] The cross-sectional structure of the insulated oil and gas pipeline 20 of the present invention is as follows: Figure 7 The insulated oil and gas pipeline 20 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, and an insulation layer 6 in sequence.

[0159] The adhesive layer 3 provides an adhesive effect between the anti-corrosion layer 2 and the thermal insulation layer 6 .

[0160] Embodiment 22: Insulated oil and gas pipeline 24 of the present invention

[0161] The cross-sectional structure of the heat-insulated oil and gas pipeline 24 of the present invention is as follows: Figure 8 The insulated oil and gas pipeline 24 includes: a steel pipe 1, an anti-corrosion layer 2, and an insulation layer 6 in order from the center of the pipeline outward.

[0162] Example 23: Insulated oil and gas pipeline 26 of the present invention

[0163] The cross-sectional structure of the insulated oil and gas pipeline 26 of the present invention is as follows: Fig. 9 The insulated oil and gas pipeline 26 includes, from the center of the pipeline outward, a steel pipe 1, an anti-corrosion layer 2, an adhesive layer 3, an insulating layer 6, an adhesive layer 9, and a second insulating layer 8 in sequence.

[0164] The adhesive layer 3 provides an adhesive effect between the anti-corrosion layer 2 and the thermal insulation layer 6 ; the adhesive layer 9 provides an adhesive effect between the thermal insulation layer 6 and the second thermal insulation layer 8 .

[0165] Example 24: Longitudinal cross-sectional view of the pipe joint area of ​​two insulated pipes welded together according to the present invention

[0166] The longitudinal cross-sectional structure of the pipe joint area of ​​two insulated oil and gas pipelines welded together according to the present invention is as follows: Fig.10 shown.

[0167] Fig.10 A longitudinal cross section including a weld area 11 where two steel pipes 1 are joined together to form part of a pipeline. When manufacturing coated / insulated pipes, the ends of the pipes 1 must remain bare to prevent damage to the coating during welding on site. Typically, the mainline coating is cut off from the end of the pipe 1 to form a chamfer spaced from the end of the pipe 1. The chamfering step is usually performed in a factory as part of the manufacturing process.

[0168] Fig.10 The steel pipes 1 shown have Figure 3 The main line coating (also called "line pipe coating") shown includes an anti-corrosion layer 22, a thermal insulation layer 6 and a protective coating 7. As mentioned above, the main line coating is cut off at a certain distance from the end of the pipeline 1. Fig.10 The pipeline 1 is shown with a particular mainline coating, but it will be appreciated that the pipeline 1 may have any of the insulating and protective coatings shown in the drawings or described herein.

[0169] The individual pipe sections 1 are connected together on site to form a continuous pipeline. The joints between the pipe sections are called "field joints" and are formed by butt welding the pipe sections 1 together and then applying a field joint insulation layer 13 on the weld area 11 (i.e. the white pipe area around the weld joint). These steps can be performed during the prefabrication of the multi-joint pipe string, or before laying the pipeline, when the pipeline is spooled onto or from a pipelaying vessel (called 4' joints).

[0170] After welding, the bare metal in the weld area 11 has a field joint corrosion protection layer 15, which may have the same composition and thickness as any of the corrosion protection layers or systems described above, and may have the same or different composition as the corrosion protection layer 22 of the main line coating. The field joint insulation layer 13 is then applied over the field joint corrosion protection layer 15 and the chamfered end 19 to substantially completely fill the weld area 11 to a thickness substantially the same as the main line coating. The field joint insulation layer 13 applied to the weld area may have the same or different composition as the insulation layer 6 and / or protective coating 7 of the main line coating.

[0171] In order to provide an effective field joint, the field joint insulation layer 13 is connected to the field joint anti-corrosion layer 15 and the chamfered end 19 of the main line coating. In order to achieve sufficient bonding with the field joint insulation layer 13, an adhesive and / or the chamfered end 19 of the main line coating may be surface cleaned to improve bonding with the field joint insulation layer 13.

[0172] As for the application method, the material used for the field joint insulation layer 13 is one of the insulation materials in Embodiments 1 to 14 of the present invention, which is applied to the welding area 11 by putting a mold on the outside of the pipe, pouring the insulation material into the mold according to the formula, heating and curing, and forming it. For example, by applying an annular mold on the welding area 11 and filling the mold cavity with the field joint insulation layer 13 in the form of molten resin. In another method, the field joint insulation layer 13 can also be applied by wrapping an extruded or pre-treated belt or applying a pre-formed shell.

[0173] The following is the preparation method of the control insulation material.

[0174] Comparative Example 1:

[0175] The ROMP polymer was prepared according to the method of Example 1 in CN 105452325 B.

[0176] Comparative Example 2:

[0177] Using polypropylene injection extrusion, put the conventional polypropylene pellet formula into the injection molding machine according to a certain feeding ratio, heat it to 230℃ until the polypropylene is melted, and then inject it into the mold through the injection molding machine. After cooling, open the mold to obtain the thermal insulation material.

[0178] Comparative Example 3:

[0179] Use polyethylene injection extrusion, feed the conventional polyethylene pellet formula into the injection molding machine according to a certain feeding ratio, heat it to 210℃ until the polyethylene is melted, inject it into the mold through the injection molding machine, and open the mold after cooling to obtain the thermal insulation material to prepare the thermal insulation material.

[0180] Comparative Example 4:

[0181] Use tungsten or molybdenum catalyst system, select RIMTEC's Telene 1650A / B component (A component is composed of dicyclopentadiene and main catalyst WCl 6 WOCl 4The components A and B are mixed with dicyclopentadiene and the co-catalysts triethylaluminum, tributylaluminum, organic zinc and alkyl silicon); Telene 1750A / B components (the A component is mixed with dicyclopentadiene and the main catalysts tri-p-methylphenoxy molybdenum dichloride and trinonylphenoxy molybdenum dichloride, and the B component is mixed with dicyclopentadiene and the co-catalysts diethylaluminum monochloride and triethylaluminum); the A component and the B component are injected into the mold by an injection molding machine at a ratio of 1:1 to prepare the thermal insulation material.

[0182] The specifications of the thermal insulation materials produced in Comparative Examples 1 to 4 are: outer diameter 100 mm, inner diameter 76 mm, length 1000 mm, and thickness 12 mm.

[0183] The beneficial effects of the present invention are demonstrated by test examples below.

[0184] Test Example 1: Characterization of Mechanical Properties and Thermal Insulation Properties

[0185] 1. Test methods

[0186] The density, glass transition temperature, thermal conductivity, Shore hardness, tensile strength, tensile modulus, elongation, compressive strength, water absorption and impact strength of the thermal insulation materials obtained in the examples and the comparative examples were tested respectively. The test standards are shown in Tables 2-4.

[0187] 2. Test results

[0188] Table 2. Mechanical properties and thermal insulation performance characterization results of the thermal insulation materials obtained in Examples 1 to 5

[0189]

[0190]

[0191] Table 3. Mechanical properties and thermal insulation performance characterization results of the thermal insulation materials obtained in Examples 6 to 14

[0192]

[0193] Table 4. Mechanical properties and thermal insulation performance characterization results of the thermal insulation materials obtained in Comparative Examples 1 to 4

[0194]

[0195]

[0196] The above test results show that the thermal insulation material prepared by the present invention has excellent mechanical properties and thermal insulation properties. In addition, compared with the ROMP polymer of Example 1 of CN 105452325 B, the thermal conductivity of the thermal insulation material prepared by the present invention is significantly reduced, and the thermal insulation performance is significantly improved.

[0197] Test Example 2: Corrosion Resistance Test

[0198] 1. Test methods

[0199] Table 5. Corrosion resistance test methods and conditions

[0200]

[0201] 2. Test results

[0202] Table 6. Corrosion resistance test results

[0203] Material No. Front weight(g) Rear weight(g) Weight loss (g) Sample status (after test) Embodiment 1 13.389 13.3323 0.0567 There is deformation, no blistering, no expansion Embodiment 2 13.3447 13.3065 0.0382 There is deformation, no blistering, no expansion Embodiment 3 12.4916 12.433 0.0586 There is deformation, no blistering, no expansion

[0204] The above test results show that the heat insulating material prepared by the present invention has excellent anti-corrosion performance and can protect the conveying pipeline from being corroded by acid, alkali or salt water.

[0205] In summary, the present invention provides an insulated oil and gas pipeline. The insulated oil and gas pipeline of the present invention has excellent thermal insulation performance, mechanical properties and corrosion resistance, and can be used to prepare underground oil pipelines, submarine oil pipelines, and geothermal pipelines for transporting oil and gas, and provides additional protection for the pipeline on the premise of ensuring safe transportation of materials in the pipeline, preventing heat loss in the pipeline, and improving transportation efficiency.

Claims

1. An insulated pipeline, comprising a steel pipe and an insulating layer, wherein the insulating layer is prepared by polymerization of raw materials including the following components: a cycloolefin compound containing one or more double bonds and at least one bridge ring, and a ruthenium carbene catalyst; in, The mass ratio of the cycloolefin compound to the ruthenium carbene catalyst is (3000-50000):1; The ruthenium carbene catalyst is selected from one or more of the following structures: ; The composition of the cycloolefin compound is: 70 wt.% dicyclopentadiene, 25 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, and 3 wt.% hydroxydicyclopentadiene; Or, the composition of the cycloolefin compound is: 55 wt.% dicyclopentadiene, 27 wt.% tricyclopentadiene, 2.4 wt.% tetracyclopentadiene, and 15.6 wt.% hydroxydicyclopentadiene; Or, the composition of the cycloolefin compound is: 42 wt.% dicyclopentadiene, 31 wt.% tricyclopentadiene, 3 wt.% tetracyclopentadiene, and 24 wt.% nadic anhydride; Or, the composition of the cycloolefin compound is: 73 wt.% of dicyclopentadiene, 22 wt.% of tricyclopentadiene, 1.6 wt.% of tetracyclopentadiene, and 3.4 wt.% of nadic anhydride; Or, the composition of the cycloolefin compound is: 36 wt.% of dicyclopentadiene, 18 wt.% of tricyclopentadiene, 1.4 wt.% of tetracyclopentadiene, and 44.6 wt.% of 5-ethylidene-2-norbornene; Or, the composition of the cycloolefin compound is: 65 wt.% dicyclopentadiene, 25 wt.% tricyclopentadiene, 2 wt.% tetracyclopentadiene, 8 wt.% 5-ethylidene-2-norbornene; The thermal conductivity of the thermal insulation layer is 0.107-0.152 W / (m·K).

2. The thermal insulation pipe according to claim 1, Features: The mass ratio of the cycloolefin compound to the ruthenium carbene catalyst is 3000:1, 4000:1, 5000:1, 10000:1, 20000:1, 25000:1, 40000:1, and 50000:

1.

3. The thermal insulation pipe according to claim 1, Features: It also contains one or more of the following raw materials: organic filler, inorganic filler, thermosetting resin, organic solvent; The organic filler is one or more of polystyrene, styrene-butadiene-styrene block copolymer, ethylene-propylene copolymer, acrylonitrile-butadiene-styrene plastic, styrene-ethylene-butylene-styrene block copolymer, adhesion promoter, light stabilizer, antioxidant, adhesion aid or flame retardant; the inorganic filler is one or more of calcium carbonate, aluminum oxide, magnesium oxide, boron nitride or glass microbeads; the thermosetting resin is one or more of epoxy resin, benzoxazine resin, cyanate resin, bismaleimide resin, polyphenylene ether resin and phenolic resin; the organic solvent is one or more of dichloromethane, toluene, methyl ethyl ketone, butanone, tetrahydrofuran and N,N-dimethylformamide.

4. The thermal insulation pipe according to claim 1, Features: It also contains one or more of the following raw materials: antioxidant, toughening agent, bonding aid, glass microspheres; The antioxidant is one or more of antioxidant TPP, antioxidant 164, antioxidant 1076, antioxidant 1010, antioxidant BHT, antioxidant CA, antioxidant BHA, antioxidant TNP, and antioxidant DLTP; the toughening agent is one or more of ethylene propylene copolymer, ethylene propylene diene monomer rubber EPDM, SEBS, SBS, POE, and EMA; and the bonding aid is isocyanate or silane coupling agent.

5. The heat-insulated pipe according to claim 4, Features: The silane coupling agent is one or more of A151, A171, A172, KH550, KH560, and KH570, and the isocyanate is diphenylmethane diisocyanate.

6. The thermal insulation pipe according to claim 5, Features: The thermal insulation layer is prepared by polymerization reaction of the following raw materials in parts by weight: 100 parts of cycloolefin compound, 0.5-5 parts of antioxidant, 0-10 parts of toughening agent, 0-5 parts of bonding agent, 0-80 parts of glass microspheres, and ruthenium carbene catalyst; The glass microspheres are hollow glass microspheres.

7. The thermal insulation pipe according to claim 6, Features: The thermal insulation layer is prepared by polymerization reaction of the following raw materials in parts by weight: 100 parts of cycloolefin compounds, 1-2 parts of antioxidants, 2-8 parts of toughening agents, 0-3 parts of bonding aids, 0-50 parts of glass microspheres, and ruthenium carbene catalysts.

8. The heat-insulated pipe according to claim 7, Features: The thermal insulation layer is prepared by polymerization reaction of the following raw materials in parts by weight: 100 parts of cycloolefin compounds, 1 part of antioxidant, 2 parts of toughening agent, 3 parts of bonding aid, 24-50 parts of glass microspheres, and ruthenium carbene catalyst.

9. The thermal insulation pipe according to any one of claims 1 to 8, Features: The preparation method of the thermal insulation layer comprises the following steps: The ruthenium carbene catalyst is dissolved in an organic solvent, then evenly mixed with the remaining raw materials, injected into a mold for polymerization reaction and molding.

10. The thermal insulation pipe according to claim 9, Features: The organic solvent is dichloromethane or toluene, and the molding conditions include keeping the temperature at 35-100° C. for 10-50 minutes.

11. The thermal insulation pipe according to any one of claims 1 to 8, Features: The thermal insulation pipe also includes one or more of an anti-corrosion layer, a protective coating, and an adhesive layer.

12. The thermal insulation pipe according to claim 11, Features: The anti-corrosion layer includes one or more of epoxy phenolic resin, polyphenylene sulfide, fluoropolymer, and polyimide; The protective coating is composed of a solid polymeric material; The adhesive layer consists of a liquid adhesive.

13. The thermal insulation pipe according to claim 11, Features: The insulated pipe also includes a second insulation layer, which is composed of a material with insulation function. The insulation layer is closer to the steel pipe than the second insulation layer.

14. The thermal insulation pipe according to claim 13, Features: The second insulation layer comprises one or more of thermoplastic plastics, plastic foams, and composite foams; Or, the second thermal insulation layer comprises one or more of foamed polypropylene homopolymer or copolymer, polybutylene, polyethylene, polystyrene, high impact polystyrene, modified polystyrene, cross-linked or partially cross-linked polypropylene, cross-linked or partially cross-linked polyethylene; Or, the second insulation layer comprises one or more of polycarbonate, polyphenylene oxide, polypropylene, polybutadiene, polyamide, polybutylene terephthalate, polyethylene terephthalate, acrylonitrile-butadiene-styrene, acrylonitrile-styrene-acrylate, polyetherimide, polymethylpentene, cycloolefin copolymer, and partially cross-linked thermoplastic elastomer; Or, the second insulation layer comprises an epoxy-modified polymer network, the modified polymer network comprises an epoxy-urethane hybrid system or an epoxy-olefin hybrid system, and its operating temperature is 90°C to 140°C; Alternatively, the second thermal insulation layer includes one or more elastomers selected from the group consisting of HNBR, nitrile rubber, silicone rubber, ethylene-propylene diene monomer rubber, and butyl rubber.

15. The thermal insulation pipe according to claim 14, Features: The polyamide is polyamide 12 or 612.

16. The thermal insulation pipe according to claim 11, Features: The thermal insulation pipeline includes a steel pipe and a thermal insulation layer from the inside to the outside; Or, the thermal insulation pipe includes a steel pipe, an anti-corrosion layer and a thermal insulation layer in sequence from the inside to the outside; Alternatively, the insulated pipe includes a steel pipe, an anti-corrosion layer, an insulation layer and a protective coating from the inside to the outside.

17. The thermal insulation pipe according to claim 16, Features: The heat-insulated pipeline comprises a steel pipe and a heat-insulating layer from the inside to the outside, and an adhesive layer is provided between the steel pipe and the heat-insulating layer; Or, the thermal insulation pipe includes a steel pipe, an anti-corrosion layer and a thermal insulation layer from the inside to the outside, an adhesive layer is included between the steel pipe and the anti-corrosion layer, and an adhesive layer is included between the anti-corrosion layer and the thermal insulation layer; Alternatively, the insulated pipe includes a steel pipe, an anti-corrosion layer, an insulation layer and a protective coating from the inside to the outside, an adhesive layer is included between the steel pipe and the anti-corrosion layer, an adhesive layer is included between the anti-corrosion layer and the insulation layer, and an adhesive layer is included between the insulation layer and the protective coating.