Preparation method and application of Co9S8 / Co-N / CP electrode
Co9S8/Co-N/CP electrode materials were synthesized by hydrothermal method to form a heterojunction interface, which solved the kinetic resistance problem of OER reaction in electrocatalytic water decomposition, improved the dual-functional performance of the catalytic activity and electrode, and achieved high efficiency electrocatalytic water decomposition.
Patent Information
- Application Number
- CN202210738415.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-27
AI Technical Summary
The kinetic resistance of the OER reaction in electrocatalytic water decomposition is relatively large, resulting in limited electrocatalytic double hydrolysis reaction rate. The existing cobalt-based electrocatalysts are insufficient in the catalytic activity of alkaline electrolytes, and low-cost, high conductivity and high Active electrocatalyst.
Co9S8/Co-N/CP electrode materials were synthesized by hydrothermal method, and the nano-multi-level structure and electronic structure of Co9S8 and Co-N on carbon paper are regulated to form a heterojunction interface, thereby improving catalytic activity and dual-function electrolysis of electrodes. Water performance.
The high activity and durability of Co9S8/Co-N/CP electrodes are achieved, the catalytic performance of OER and HER reactions is optimized, the kinetic resistance of the electrode is reduced, and the efficiency and stability of electrocatalytic water decomposition are improved.
Smart Images

Figure CN115181992B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of composite materials and catalytic electrode materials, and relates to a preparation method and application of an electrode, and in particular to a preparation method and application of a Co9S8 / Co-N / CP electrode. Background Art
[0002] Hydrogen is a green energy source for sustainable development and is considered to be the best alternative to fossil energy. Electrocatalytic water splitting is an effective means of producing hydrogen, which can alleviate the pressure of energy consumption to a large extent and reduce the environmental problems caused by CO2 produced by the combustion of fossil fuels. The electrocatalytic water splitting process involves the HER reaction with two electron transfer and the OER reaction with four electron transfer. Among them, the reaction kinetic resistance of the multi-step transfer step of OER is large, and a large amount of energy is required to start the process, which is an important factor restricting the rate of electrocatalytic double hydrolysis reaction. In order to overcome the obstacles in the OER reaction, it is urgent to develop low-cost, high-conductivity and high-activity electrocatalysts. Cobalt-based electrocatalysts are highly valued by researchers because of their good catalytic activity in alkaline electrolytes.
[0003] The catalytic activity of electrocatalysts depends on the number of active centers and the intrinsic catalytic activity of the active centers. In a large number of strategies for optimizing cobalt-based materials, the activity of electrocatalysts is often related to the crystal structure, specific surface area and conductivity of the catalyst, but its intrinsic catalytic activity is often ignored. However, enhancing the electrocatalytic activity of each active site can improve the overall performance of the electrocatalyst. For example, the chemical state, bond energy and electronic structure of the catalyst will affect the intrinsic catalytic activity of the catalyst. First, the disorder of active atoms produced by surface defects can improve the adsorption / desorption energy of active sites for catalytic intermediates. Second, self-doping and heteroatom doping can change the electronic structure of the material and enhance the catalytic performance; third, constructing a heterojunction structure, whose active interface has the advantages of two separate components in the crystal structure, thereby enhancing the electrolysis performance of cobalt-based catalysts. Summary of the invention
[0004] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for preparing a Co9S8 / Co-N / CP electrode material with a heterojunction structure. The method can adjust the nano-multilevel structure of Co9S8 / Co-N grown on carbon paper and achieve the regulation of the electronic structure of the heterojunction interface by regulating the relative content of S and N in Co9S8 / Co-N / CP. It can be used in the fields of electrocatalytic water decomposition and is of great significance to the improvement of catalytic electrode performance and mass production.
[0005] Technical solution: In view of the above technical problems to be solved, the technical solution of the present invention is as follows:
[0006] A method for preparing a Co9S8 / Co-N / CP electrode, characterized in that the method comprises the following steps:
[0007] 1) ultrasonically washing the carbon paper with ethanol and deionized water in sequence and then drying it, placing the washed and dried carbon paper in a mixed solution containing concentrated sulfuric acid and concentrated nitric acid, soaking it at high temperature, and washing it with deionized water until it is neutral after naturally cooling to room temperature and drying it overnight to obtain functionalized carbon paper;
[0008] 2) preparing a mixed solution II of deionized water and isopropanol, then dissolving Co(NO3)2·6H2O and C6H9NO6 in the mixed solution II and stirring, then placing the functionalized carbon paper prepared in step 1) into the inner lining of the reactor, and preparing Co-N / CP through the first hydrothermal reaction and the first calcination; 10 ml to 20 ml of the mixed solution II is added to each piece of functionalized carbon paper, and the size of the functionalized carbon paper is 2 cm×2 cm;
[0009] 3) C2H5NS and CoCl2·6H2O are dissolved in deionized water to form a mixed solution III and stirred; the mixed solution III is transferred to the inner lining of the reactor, and then the Co-N / CP prepared in step 2) is placed in the mixed solution III, and the sample Co9S8 / Co-N / CP is obtained after a second hydrothermal reaction and a second calcination; 10ml to 20ml of the mixed solution III is added to each piece of Co-N / CP.
[0010] Preferably, in step 1) of the present invention, the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed solution 1 is 3:1; the temperature used for soaking at high temperature is 70-85°C, and the soaking time is 1-3h; the drying temperature used for drying overnight is 60-80°C.
[0011] Preferably, in step 2) adopted in the present invention, the volume ratio of isopropanol and deionized water in the mixed solution 2 is 7:1-6; the molar ratio of Co(NO3)2·6H2O and C6H9NO6 is 1:1-2:1; the temperature of the first hydrothermal reaction is 140°C-180°C; the temperature of the first calcination is 500°C, the heating rate is 3°C / min, and the calcination time is 2 hours.
[0012] Preferably, the molar ratio of C2H5NS and CoCl2·6H2O used in the present invention is 1:1 to 2:1; the temperature of the second hydrothermal reaction is 120°C-140°C; the temperature of the second calcination is 450 to 600°C, the heating rate is 1 to 3°C / min, and the calcination time is 1 to 2 hours.
[0013] Preferably, the molar ratio of C2H5NS to CoCl2·6H2O used in the present invention is 4:3.
[0014] A Co9S8 / Co-N / CP electrode material prepared based on the method described above.
[0015] As mentioned above, the application of Co9S8 / Co-N / CP electrode material in water electrolysis material.
[0016] The innovation of the present invention lies in the OER, HER and electrocatalytic double hydrolysis performance of the self-supporting Co-N / CP and Co9S8 / Co-N / CP synthesized by the hydrothermal method. Using carbon paper as a substrate, the morphology of the crystals and the arrangement of the crystals on the surface of the carbon paper can be regulated, the exposed active sites on the electrode surface can be increased, and the transmission rate of electrons and protons can be increased. The hydrothermal vulcanization method can not only reduce the harm of harmful gases generated during the vulcanization process to the human body, but also the method is simple to operate and has a high repetition rate.
[0017] Beneficial effects: Compared with the prior art, the present invention has the following advantages: the Co9S8 / Co-N / CP heterojunction structure can optimize the interaction between Co9S8 and Co-N, and can strengthen the interaction between the active substance and the carbon paper, thereby improving the structural stability of the catalytic electrode in the electrolyte, and ultimately achieving the improvement of the dual-functional water electrolysis performance of Co9S8 / Co-N / CP.
[0018] The invention discloses a preparation method of a Co9S8 / Co-N / CP electrode material. The method comprises the following steps: dissolving Co(NO3)2·6H2O and nitrilotriacetic acid in a mixed solution of isopropanol and water at a molar ratio of 5:4 by a hydrothermal method, placing functionalized carbon paper in the system after obtaining a uniformly mixed system, carrying out a first hydrothermal reaction at 140°C-180°C, and obtaining Co-N / CP after calcination; dissolving C2H5NS and CoCl2·6H2O in different molar ratios of 1:1-2:1 in deionized water, placing Co-N / CP in the solution, carrying out a second hydrothermal reaction at a temperature of 120°C-140°C, taking out the carbon paper, washing, drying and calcining in sequence, and obtaining a Co9S8 / Co-N / CP integrated electrode material with a heterojunction structure. Compared with the existing technology, since the electrode material is hydrothermally synthesized in steps and different Co salts are added during the synthesis process, the electronic structure and charge density between Co-S-Co and Co-SN are adjusted, and the Co9S8 / Co-N heterojunction structure finally grown on carbon paper is more solid than the nanomaterial synthesis technology using the same Co salt. Not only does it provide a large number of exposed active sites for the electrolytic water catalyst, increasing the active surface area of the catalyst, but the electronic structure of its heterojunction interface further improves the adsorption / desorption of the intermediates produced in the electrolytic water catalytic process of the electrode material, thereby improving the activity and durability of the electrocatalytic water decomposition performance. In the present invention, the present invention designs a Co9S8 / Co-N / CP self-supporting material with a heterojunction structure. The nano multi-level structure of the material can not only provide a large specific surface area, but its adjustable S and N relative content can make the heterojunction interface electronic structure of the electrode material further improve the adsorption / desorption of active intermediates in the electrolytic water process on the catalytic electrode surface, thereby improving the catalytic activity of the catalyst for OER and HER reactions. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 They are SEM images of samples (A) Co-N / CP, (B) Co9S8 / Co-N / CP (1:1), (C) Co9S8 / Co-N / CP (4:3) and (D) Co9S8 / Co-N / CP (2:1) in Examples 1, 2 and 3 of the present invention, respectively.
[0020] Figure 2 The SEM images of Co9S8 / Co-N / CP obtained at different ratios of Co(NO3)2·6H2O and C6H9NO6 in Examples 4 and 5 of the present invention are respectively shown. (A) SEM image of Co9S8 / Co-N / CP obtained at n Co(NO3)2·6H2O:nC6H9NO6=1:1 in Example 4; (B) SEM image of Co9S8 / Co-N / CP obtained at n Co(NO3)2·6H2O:nC6H9NO6=1:1 in Example 5 6=SEM image of Co9S8 / Co-N / CP obtained at 2:1.
[0021] Figure 3 The following are SEM images of Co9S8 / Co-N / CP obtained in different ratios of deionized water and isopropanol in Examples 6 and 7 of the present invention. (A) V in Example 6 H2O :V 异丙醇 =7:3 obtained Co9S8 / Co-N / CP SEM image; (B) V in Example 7 H2O :V 异丙醇 =7:6 obtained SEM image of Co9S8 / Co-N / CP.
[0022] Figure 4 These are the XRD spectra of Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (4:3) and Co9S8 / Co-N / CP (2:1) in Examples 1, 2 and 3 of the present invention.
[0023] Figure 5 It is the full XPS spectra of Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (4:3) and Co9S8 / Co-N / CP (2:1) in Examples 1, 2 and 3 of the present invention.
[0024] Figure 6 (A) LSV curve of oxygen evolution of CP, Co-N / CP, Co9S8Co-N / CP (1:1), Co9S8Co-N / CP (4:3) and Co9S8Co-N / CP (2:1) in 1 mol / L KOH solution in Examples 1, 2 and 3 of the present invention; (B) histogram of overpotential at given current density (20 mA cm-2 and 50 mA cm-2); (C) Tafel curve; (D) it curve.
[0025] Figure 7 (A) LSV curve of hydrogen evolution of CP, Co-N / CP, Co9S8Co-N / CP (1:1), Co9S8Co-N / CP (4:3) and Co9S8Co-N / CP (2:1) in 1 mol / L KOH solution in Examples 1, 2 and 3 of the present invention; (B) histogram of overpotential at given current density (20 mA cm-2 and 50 mA cm-2); (C) Tafel curve; (D) it curve.
[0026] Figure 8These are the AC impedance spectra of (A) CP, Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (4:3) and Co9S8 / Co-N / CP (2:1) in 1 mol / L KOH solution in Examples 1, 2 and 3; (B) equivalent circuit diagram.
[0027] Fig. 9 These are the double hydrolysis LSV curves of (A) Pt / C / CP∥RuO2 / CP, Co-N / CP∥Co-N / CP, Co9S8 / Co-N / CP∥Co9S8 / Co-N / CP and after 1500 cycles in Example 3; (B) it curve. DETAILED DESCRIPTION
[0028] The following examples can further illustrate the preparation of the composite material of the present invention and the preparation and electrochemical performance of its electrode material.
[0029] Example 1 Preparation and application of Co9S8 / Co-N / CP electrode material
[0030] 1) Carbon paper (CP) functionalization: The carbon paper was cut into small squares with an area of about 2×2 cm, and the carbon paper was ultrasonically washed with ethanol and deionized water in sequence, and then dried at 60°C for 12 h. Then, the washed and dried carbon paper was placed in a mixed solution and treated at 75°C for 2 h. After cooling naturally to room temperature, it was washed with deionized water until neutral and dried at 60°C overnight.
[0031] 2) Preparation of Co-N / CP: First, a mixed solution of deionized water and isopropanol (V H2O :V 异丙醇 =7:1), then Co(NO3)2·6H2O and C6H9NO6 (nCo(NO3)2·6H2O:nC6H9NO6=5:4) were dissolved in the above mixed solution, stirred for 2h, and the mixed solution was transferred to the lining of a 20mL reactor, and then the functionalized carbon paper was placed in the reactor lining, and reacted in a 180°C forced air drying oven for 18h. After the reaction was completed and naturally cooled to room temperature, the carbon paper was taken out and washed with deionized water several times, and dried in a vacuum drying oven at 60°C overnight to obtain a pink sample. The sample was placed in a porcelain boat, calcined after passing N2, and the obtained sample was recorded as Co-N / CP;
[0032] 3) Preparation of Co9S8 / Co-N / CP: C2H5NS and CoCl2·6H2O in a molar ratio of 1:1 were dissolved in deionized water and stirred for 30 min to form a clear solution. The mixed solution was then transferred to the lining of the reactor, and Co-N / CP (1×2 cm) was then placed in the solution, reacted in a blast drying oven at 130°C for 2 h, naturally cooled to room temperature, rinsed with deionized water 2 to 3 times, and dried in a vacuum drying oven at 60°C for 12 h. The sample was then placed in a porcelain boat and calcined in a tube furnace at 500°C in a N2 atmosphere for 2 h, with a heating rate of 3°C / min. The obtained sample was recorded as Co9S8 / Co-N / CP (1:1).
[0033] Example 2 Preparation and application of Co9S8 / Co-N / CP electrode material
[0034] 1) Carbon paper (CP) functionalization: The carbon paper was cut into small squares with an area of about 2×2 cm, and the carbon paper was ultrasonically washed with ethanol and deionized water in sequence, and then dried at 60°C for 12 h. Then, the washed and dried carbon paper was placed in a mixed solution and treated at 75°C for 2 h. After cooling naturally to room temperature, it was washed with deionized water until neutral and dried at 60°C overnight.
[0035] 2) Preparation of Co-N / CP: First, a mixed solution of deionized water and isopropanol (V H2O :V 异丙醇 =7:1), then Co(NO3)2·6H2O and C6H9NO6 (nCo(NO3)2·6H2O:nC6H9NO6=5:4) were dissolved in the above mixed solution, stirred for 2h, and the mixed solution was transferred to the lining of a 20mL reactor, and then the functionalized carbon paper was placed in the reactor lining, and reacted in a 180°C forced air drying oven for 18h. After the reaction was completed and naturally cooled to room temperature, the carbon paper was taken out and washed with deionized water several times, and dried in a vacuum drying oven at 60°C overnight to obtain a pink sample. The sample was placed in a porcelain boat, calcined after passing N2, and the obtained sample was recorded as Co-N / CP;
[0036] 3) Preparation of Co9S8 / Co-N / CP: C2H5NS and CoCl2·6H2O in a molar ratio of 2:1 were dissolved in deionized water and stirred for 30 min to form a clear solution. The mixed solution was then transferred to the lining of the reactor, and Co-N / CP (1×2 cm) was then placed in the solution, reacted in a blast drying oven at 130°C for 2 h, naturally cooled to room temperature, rinsed with deionized water 2 to 3 times, and dried in a vacuum drying oven at 60°C for 12 h. The sample was then placed in a porcelain boat and calcined under a N2 atmosphere. The obtained sample was recorded as Co9S8 / Co-N / CP (2:1).
[0037] Example 3 Preparation and application of Co9S8 / Co-N / CP electrode material
[0038] 1) Carbon paper (CP) functionalization: The carbon paper was cut into small squares with an area of about 2×2 cm, and the carbon paper was ultrasonically washed with ethanol and deionized water in sequence, and then dried at 60°C for 12 h. Then, the washed and dried carbon paper was placed in a mixed solution and treated at 75°C for 2 h. After cooling naturally to room temperature, it was washed with deionized water until neutral and dried at 60°C overnight.
[0039] 2) Preparation of Co-N / CP: First, a mixed solution of deionized water and isopropanol (V H2O :V 异丙醇 =7:1), then Co(NO3)2·6H2O and C6H9NO6 (nCo(NO3)2·6H2O:nC6H9NO6=5:4) were dissolved in the above mixed solution, stirred for 2h, and the mixed solution was transferred to the lining of a 20mL reactor, and then the functionalized carbon paper was placed in the reactor lining, and reacted in a 180°C forced air drying oven for 18h. After the reaction was completed and naturally cooled to room temperature, the carbon paper was taken out and washed with deionized water several times, and dried in a vacuum drying oven at 60°C overnight to obtain a pink sample. The sample was placed in a porcelain boat, calcined after passing N2, and the obtained sample was recorded as Co-N / CP;
[0040] 3) Preparation of Co9S8 / Co-N / CP: C2H5NS and CoCl2·6H2O in a molar ratio of 4:3 were dissolved in deionized water and stirred for 30 min to form a clear solution. The mixed solution was then transferred to the lining of the reactor, and Co-N / CP (1×2 cm) was then placed in the solution, reacted in a blast drying oven at 130°C for 2 h, naturally cooled to room temperature, rinsed with deionized water 2 to 3 times, and dried in a vacuum drying oven at 60°C for 12 h. The sample was then placed in a porcelain boat and calcined under a N2 atmosphere. The obtained sample was recorded as Co9S8 / Co-N / CP (4:3).
[0041] Example 4 Preparation and application of Co9S8 / Co-N / CP electrode material
[0042] 1) Carbon paper (CP) functionalization: The carbon paper was cut into small squares with an area of about 2×2 cm, and the carbon paper was ultrasonically washed with ethanol and deionized water in sequence, and then dried at 60°C for 12 h. Then, the washed and dried carbon paper was placed in a mixed solution and treated at 75°C for 2 h. After cooling naturally to room temperature, it was washed with deionized water until neutral and dried at 60°C overnight.
[0043] 2) Preparation of Co-N / CP: First, a mixed solution of deionized water and isopropanol (V H2O :V 异丙醇=7:1), then Co(NO3)2·6H2O and C6H9NO6 (nCo(NO3)2·6H2O:nC6H9NO6=1:1) were dissolved in the above mixed solution, stirred for 2h, and the mixed solution was transferred to a 20mL reactor liner, and then the functionalized carbon paper was placed in the reactor liner, and reacted in a 180°C blast drying oven for 18h. After the reaction was completed and naturally cooled to room temperature, the carbon paper was taken out and washed with deionized water several times, and dried in a 60°C vacuum drying oven overnight to obtain a pink sample. The sample was placed in a porcelain boat, calcined after passing N2, and the obtained sample was recorded as Co-N / CP;
[0044] 3) Preparation of Co9S8 / Co-N / CP: C2H5NS and CoCl2·6H2O in a molar ratio of 4:3 were dissolved in deionized water and stirred for 30 min to form a clear solution. The mixed solution was then transferred to the lining of the reactor, and Co-N / CP (1×2 cm) was then placed in the solution, reacted in a 130°C forced air drying oven for 2 h, naturally cooled to room temperature, rinsed with deionized water 2 to 3 times, and dried in a 60°C vacuum drying oven for 12 h. The sample was then placed in a porcelain boat and calcined under a N2 atmosphere. The obtained sample was recorded as Co9S8 / Co-N / CP (1-1).
[0045] Example 5 Preparation and application of Co9S8 / Co-N / CP electrode material
[0046] 1) Carbon paper (CP) functionalization: The carbon paper was cut into small squares with an area of about 2×2 cm, and the carbon paper was ultrasonically washed with ethanol and deionized water in sequence, and then dried at 60°C for 12 h. Then, the washed and dried carbon paper was placed in a mixed solution and treated at 75°C for 2 h. After cooling naturally to room temperature, it was washed with deionized water until neutral and dried at 60°C overnight.
[0047] 2) Preparation of Co-N / CP: First, a mixed solution of deionized water and isopropanol (V H2O :V 异丙醇 =7:1), then Co(NO3)2·6H2O and C6H9NO6 (nCo(NO3)2·6H2O:nC6H9NO6=2:1) were dissolved in the above mixed solution, stirred for 2h, and the mixed solution was transferred to a 20mL reactor liner, and then the functionalized carbon paper was placed in the reactor liner, and reacted in a 180°C blast drying oven for 18h. After the reaction was completed and naturally cooled to room temperature, the carbon paper was taken out and washed with deionized water several times, and dried in a 60°C vacuum drying oven overnight to obtain a pink sample. The sample was placed in a porcelain boat, passed through N2 and calcined, and the obtained sample was recorded as Co-N / CP;
[0048] 3) Preparation of Co9S8 / Co-N / CP: C2H5NS and CoCl2·6H2O in a molar ratio of 4:3 were dissolved in deionized water and stirred for 30 min to form a clear solution. The mixed solution was then transferred to the lining of the reactor, and Co-N / CP (1×2 cm) was then placed in the solution, reacted in a 130°C forced air drying oven for 2 h, naturally cooled to room temperature, rinsed with deionized water 2 to 3 times, and dried in a 60°C vacuum drying oven for 12 h. The sample was then placed in a porcelain boat and calcined under a N2 atmosphere. The obtained sample was recorded as Co9S8 / Co-N / CP (2-1).
[0049] Example 6 Preparation and application of Co9S8 / Co-N / CP electrode material
[0050] 1) Carbon paper (CP) functionalization: The carbon paper was cut into small squares with an area of about 2×2 cm, and the carbon paper was ultrasonically washed with ethanol and deionized water in sequence, and then dried at 60°C for 12 h. Then, the washed and dried carbon paper was placed in a mixed solution and treated at 75°C for 2 h. After cooling naturally to room temperature, it was washed with deionized water until neutral and dried at 60°C overnight.
[0051] 2) Preparation of Co-N / CP: First, a mixed solution of deionized water and isopropanol (V H2O :V 异丙醇 =7:3), then Co(NO3)2·6H2O and C6H9NO6 (nCo(NO3)2·6H2O:nC6H9NO6=5:4) were dissolved in the above mixed solution, stirred for 2h, and the mixed solution was transferred to the lining of a 20mL reactor, and then the functionalized carbon paper was placed in the reactor lining, and reacted in a 180°C forced air drying oven for 18h. After the reaction was completed and naturally cooled to room temperature, the carbon paper was taken out and washed with deionized water several times, and dried in a vacuum drying oven at 60°C overnight to obtain a pink sample. The sample was placed in a porcelain boat, calcined after passing N2, and the obtained sample was recorded as Co-N / CP;
[0052] 3) Preparation of Co9S8 / Co-N / CP: C2H5NS and CoCl2·6H2O in a molar ratio of 4:3 were dissolved in deionized water and stirred for 30 min to form a clear solution. The mixed solution was then transferred to the lining of the reactor, and Co-N / CP (1×2 cm) was then placed in the solution, reacted in a blast drying oven at 130°C for 2 h, naturally cooled to room temperature, rinsed with deionized water 2 to 3 times, and dried in a vacuum drying oven at 60°C for 12 h. The sample was then placed in a porcelain boat and calcined under a N2 atmosphere. The obtained sample was recorded as Co9S8 / Co-N / CP-2.
[0053] Example 7 Preparation and application of Co9S8 / Co-N / CP electrode material
[0054] 1) Carbon paper (CP) functionalization: The carbon paper was cut into small squares with an area of about 2×2 cm, and the carbon paper was ultrasonically washed with ethanol and deionized water in sequence, and then dried at 60°C for 12 h. Then, the washed and dried carbon paper was placed in a mixed solution and treated at 75°C for 2 h. After cooling naturally to room temperature, it was washed with deionized water until neutral and dried at 60°C overnight.
[0055] 2) Preparation of Co-N / CP: First, a mixed solution of deionized water and isopropanol (V H2O :V 异丙醇 =7:6), then Co(NO3)2·6H2O and C6H9NO6 (nCo(NO3)2·6H2O:nC6H9NO6=5:4) were dissolved in the above mixed solution, stirred for 2h, and the mixed solution was transferred to the lining of a 20mL reactor, and then the functionalized carbon paper was placed in the reactor lining, and reacted in a 180°C forced air drying oven for 18h. After the reaction was completed and naturally cooled to room temperature, the carbon paper was taken out and washed with deionized water several times, and dried in a 60°C vacuum drying oven overnight to obtain a pink sample. The sample was placed in a porcelain boat, calcined after passing N2, and the obtained sample was recorded as Co-N / CP;
[0056] 3) Preparation of Co9S8 / Co-N / CP: C2H5NS and CoCl2·6H2O in a molar ratio of 4:3 were dissolved in deionized water and stirred for 30 min to form a clear solution. The mixed solution was then transferred to the lining of the reactor, and Co-N / CP (1×2 cm) was then placed in the solution, reacted in a 130°C forced air drying oven for 2 h, naturally cooled to room temperature, rinsed with deionized water 2 to 3 times, and dried in a 60°C vacuum drying oven for 12 h. The sample was then placed in a porcelain boat and calcined under a N2 atmosphere. The obtained sample was recorded as Co9S8 / Co-N / CP (2-1).
[0057] The microstructure of the crystals grown on carbon paper was observed by electron scanning microscopy. Figure 1The SEM images of Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (2:1) and Co9S8 / Co-N / CP (4:3) obtained with different molar ratios of C2H5NS and CoCl2·6H2O in Examples 1, 2 and 3 are shown. The original Co-N grown on carbon paper is in the form of nanorods. After the second hydrothermal reaction, block crystals grow on the Co-N nanorods. When the molar ratio of thioacetamide and CoCl2·6H2O is 2:1, the crystals grown on the synthesized Co9S8 / Co-N / CP (2:1) nanorods are irregular in shape. The crystals on the Co9S8 / Co-N / CP (4:3) nanorods obtained when the molar ratio is 4:3 are regular rhombuses. As the molar ratio increases, the crystals on the Co9S8 / Co-N / CP (1:1) nanorods appear smaller rods in addition to irregular block crystals, which will affect the stability of the material during the reaction process. Figure 2 The SEM images of Co9S8 / Co-N / CP obtained in different ratios of Co(NO3)2·6H2O and C6H9NO6 in Examples 4 and 5. When nCo(NO3)2·6H2O:nC6H9NO6=1:1, the multi-level structure of Co9S8 / Co-N / CP obtained is not uniform and has cracks. When nCo(NO3)2·6H2O:nC6H9NO6=2:1, the rod-like structure of Co9S8 / Co-N / CP obtained is not uniform and there are also cracks on the surface of the active material, so the electrochemical performance cannot be further tested. Figure 3 : The SEM images of Co9S8 / Co-N / CP obtained in Examples 6 and 7 at different ratios of deionized water to isopropanol. H2O :V 异丙醇 =7:3 obtained Co9S8 / Co-N / CP SEM image (such as Figure 3 A), the flower-like and rod-like structures all exist, the morphology is not uniform, and the active sites exposed on the catalyst surface are limited; in Example 7, V H2O :V 异丙醇 =7:6 obtained Co9S8 / Co-N / CP SEM image (such as Figure 3 As shown in Figure B), the active material grown on the surface of the carbon cloth has an uneven morphology, and the active material has a weak interaction with the carbon cloth matrix material, and is easy to fall off in large quantities. Therefore, the subsequent electrode catalytic performance test cannot be carried out.
[0058] The crystal structure and composition of the materials were further analyzed by X-ray diffraction of Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (4:3) and Co9S8 / Co-N / CP (2:1). Figure 4It can be seen that these samples all have a broad peak at 26°, which matches the (002) crystal plane of carbon. For the samples Co9S8 / Co-N / CP (1:1) and Co9S8 / Co-N / CP (4:3), the diffraction peaks at 30.0°, 31.4°, 47.6°, 52.2°, 61.3°, 62.2° and 73.3° can be clearly determined to correspond to the (311), (222), (511), (440), (533) and (731) crystal planes in the standard card Co9S8 (PDF#03-0631).
[0059] The XPS spectrum measured by X-ray photoelectron spectrometer can further analyze the valence state and bonding mode of the material. Figure 5 The full spectra of Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (2:1), and Co9S8 / Co-N / CP (4:3) are shown. The electron binding energies of Co 1s, N 1s, C 1s, and O 1s orbits can be observed from the full spectrum of Co-N / CP, indicating the presence of Co, N, and C elements in the material. In addition to the above elements, the full spectrum of the sample after hydrothermal vulcanization also contains the S1s peak. The presence of Co and S elements indicates that Co9S8 or Co-S may exist in the composite material.
[0060] Analysis of electrocatalytic oxygen evolution performance: The OER performance of the electrode was tested in a three-electrode system with an electrolyte of 1 mol / L KOH, a graphite rod as an auxiliary electrode, and Hg / HgO as a reference electrode. Figure 6 A shows the LSV polarization curves of CP, Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (4:3) and Co9S8 / Co-N / CP (2:1). It can be observed from the figure that these electrodes have a high conductivity at 20 mA cm -2 The overpotentials are 510mV, 340mV, 310mV, 240mV and 330mV respectively. Figure 6 B is the current of these electrodes at 20 mA cm -2 and 50mA cm -2 From the overpotential bar graph, it can be clearly seen that Co9S8 / Co-N / CP (4:3) has the lowest oxygen evolution overpotential. This proves that the oxygen evolution performance of the electrode is improved after the composite of Co-N and Co9S8. The OER performance of the Co9S8 / Co-N / CP (4:3) electrode synthesized in this work is better than that of the Co9S8 nanoring synthesized by Zhang et al. The Tafel curve calculated based on the LSV curve. Figure 6As shown in Figure C, the Tafel slope of carbon paper is 108.47mV dec-1, and the Tafel slopes of Co-N / CP, Co9S8 / Co-N / CP (1:1), and Co9S8 / Co-N / CP (2:1) are 105.00mV dec-1, 101.33mV dec-1, and 117.12mV dec-1, respectively, which are all greater than the Tafel slope of Co9S8 / Co-N / CP (4:3) of 99.39V dec-1. This shows that the combination of Co9S8 and Co-N can reduce the kinetic resistance of the electrode, benefit the proton and electron transport during the reaction, and improve the catalytic activity of the electrode. Measuring the it curve by constant potential method is a common method to characterize the stability of electrocatalysts. Figure 6 D is the IT curve of Co9S8 / Co-N / CP (4:3) obtained at a voltage of 1.48 V (vs. RHE). After a long cycle of 24 h, the current density still remains at a high value, indicating that the electrode has excellent durability.
[0061] Electrocatalytic hydrogen evolution performance analysis: The HER performance of the electrode was tested using a three-electrode electrolytic cell. The electrolyte was 1 mol / L KOH solution, a graphite rod was used as an auxiliary electrode, and Hg / HgO was used as a reference electrode. The LSV polarization curve of the electrode in this system was used to test the HER activity of the combined catalyst in an alkaline electrolyte (e.g. Figure 7 shown). Figure 7 A is the LSV curves of electrocatalytic hydrogen evolution of CP, Co-NC / CP (1:1), Co-NC / CP (1:2), Co-NC / CP (1:3), and Co-NC / CP (1:4). These materials have a low electrocatalytic activity at -10 mA cm -2 The overpotentials of hydrogen evolution at current densities of -568, -365, -181, -312, and -297 mV are respectively. -2 When the overpotential of Co-NC / CP (1:2) is -181 mV, which is lower than that of most self-supporting cobalt-based electrocatalysts based on carbon paper that have been reported so far. The lower overpotential indicates that nitrogen doping is beneficial to the electrocatalytic hydrogen evolution reaction, providing a large number of active sites and reducing the kinetic resistance of the HER reaction. The overpotential of hydrogen evolution of Co-NC / CP (1:1) is only better than that of carbon paper, indicating that excess cobalt is also not conducive to the HER reaction and cannot provide active sites for the HER reaction. -2 ,20mA cm -2 and 50mA cm -2 ) under oxygen evolution overpotential histogram as shown in Figure 7 As shown in Figure B, the change in hydrogen evolution overpotential of electrode materials with different molar ratios is intuitively displayed. Figure 7C is the Tafel curve obtained by fitting the LSV polarization curve of HER. It can be observed from the figure that the Tafel slopes of CP, Co-NC / CP (1:1), Co-NC / CP (1:2), Co-NC / CP (1:3), and Co-NC / CP (1:4) are 667.02, 128.32, 123.26, 127.01, and 127.04 mV dec, respectively. -1 The Tafel slope of Co-NC / CP (1:2) is close to 120 mV dec. -1 , which is smaller than that of other materials, further proving that the kinetic resistance of this material in the hydrogen evolution reaction is relatively slow. Figure 7 D is the It curve of Co-NC / CP (1:2). The It curve is one of the important means to test the stability of materials. By testing the It curve, the electrocatalytic durability of the material can be verified. At an overpotential of 181 mV, the current density of Co-NC / CP (1:2) can still be maintained at 8.86 mA cm after 24 h. -2 , proving that the material has good long-term cycle stability.
[0062] EIS analysis: through impedance Figure 8 The electrocatalytic performance of the materials can be further analyzed to verify that these materials have small kinetic resistance. The AC impedance spectra of CP, Co-N / CP, Co9S8 / Co-N / CP (1:1), Co9S8 / Co-N / CP (4:3) and Co9S8 / Co-N / CP (2:1) in 1 mol / L KOH solution are shown in Figure 2. Figure 8 As shown in A, it can be seen from the figure that the arc of Co9S8 / Co-N / CP (4:3) is the smallest, so the resistance is the smallest. The resistance of the catalyst is significantly reduced after the composite Co9S8, and the Co9S8 / Co-N / CP (4:3) catalyst has lower resistance and higher OER activity at the electrode / electrolyte interface.
[0063] Analysis of electrocatalytic dual hydrolysis performance: From the above analysis, it can be seen that Co9S8 / Co-N / CP (4:3) has the best OER activity in 1 mol / L KOH solution, and Co-N / CP has the best HER activity in this electrolyte. In order to compare the electrocatalytic dual hydrolysis performance of these two materials, Co-N / CP and Co9S8 / Co-N / CP (4:3) were used as the anode and cathode of the dual-electrode electrolyzer in the same electrolyte. The LSV curves are shown in the figure below. Fig. 9 As shown in A. It can be seen from the figure that the electrolytic cells of Co-N / CP∥Co-N / CP and Co9S8 / Co-N / CP(4:3)∥Co9S8 / Co-N / CP(4:3) reach 20mA cm -2The required overpotentials are 340 mV and 300 mV respectively. After 1500 cycles, 20 mA cm -2 The required overpotentials are 360 mV and 310 mV, respectively. For the Pt / C / CP||RuO2 / CP electrolytic cell, when the current density is 20 mA cm -2 When the current density is 50 mA cm -2 When the overpotential of Co-N / CP, Co9S8 / Co-N / CP (4:3) and Pt / C / CP∥RuO2 / CP electrolytic cells was 370mV, 350mV and 400mV respectively. After 1500 cycles, the overpotential of Co-N / CP and Co9S8 / Co-N / CP (4:3) reached 50mA cm -2 The required overpotentials are 400mV and 350mV, respectively. From these data, it can be seen that the electrocatalytic double hydrolysis performance of Co-N / CP and Co9S8 / Co-N / CP (4:3) electrodes at higher current density is better than that of Pt / C / CP∥RuO2 / CP, and is also better than other cobalt-based bifunctional electrocatalysts reported so far. This result shows that S and N co-doping can increase the active sites on the catalyst surface and promote the improvement of the double hydrolysis performance of the catalyst in alkaline electrolyte. In order to evaluate the stability and durability of the electrocatalyst in alkaline electrolyte, we conducted a 1 mol L - 1 The it curves of Co-N / CP and Co9S8 / Co-N / CP samples tested in KOH solution are as follows: Fig. 9 B and Fig. 9 C. After 24 hours of reaction in alkaline electrolyte, the current density of Co9S8 / Co-N / CP electrode decreased slightly, while the current density of Co-N / CP electrode decreased significantly and the IT curve fluctuated greatly. This result proves that the introduction of S into the cobalt-based catalyst increases the stability of the catalyst.
[0064] In summary, the Co9S8 / Co-N / CP of the present invention has the best OER performance in 1 mol / L KOH solution, reaching 20 mA cm -2 The required overpotential is 240 mV and the Tafel slope is 99.39 mV dec -1. The electrocatalytic double hydrolysis performance of Co9S8 / Co-N / CP is better than that of Co-N / CP. At high current density, the electrocatalytic double hydrolysis performance of these two materials is better than that of precious metal catalysts coated on carbon paper. Good nitrogen-doped cobalt-based compounds have good HER activity in alkaline electrolytes, and nitrogen doping can significantly increase the HER reaction active sites of the material. After Co-N is composited with Co9S8, the resistance of the electrocatalyst can be reduced, the electron and proton transfer rate between the electrode and the electrolyte in the OER reaction can be increased, and the number of exposed active sites can be increased, thereby improving the OER and electrocatalytic double hydrolysis performance of the material.
Claims
1. A method for preparing a Co9S8 / Co-N / CP electrode, characterized in that: The method comprises the following steps: 1) Ultrasonic washing of carbon paper with ethanol and deionized water in sequence and drying, placing the washed and dried carbon paper in a mixed solution containing concentrated sulfuric acid and concentrated nitric acid, soaking at high temperature, and washing with deionized water to neutrality after natural cooling to room temperature and drying overnight to obtain functionalized carbon paper; 2) preparing a mixed solution II of deionized water and isopropanol, then dissolving Co(NO3)2·6H2O and C6H9NO6 in the mixed solution II and stirring, then placing the functionalized carbon paper prepared in step 1) into the inner lining of a reactor, and preparing Co-N / CP through the first hydrothermal reaction and the first calcination; 10 ml~20 ml of the mixed solution II is added to each piece of functionalized carbon paper; the volume ratio of deionized water and isopropanol in the mixed solution II is 7: 1~6; the molar ratio of Co(NO3)2·6H2O and C6H9NO6 is 1:1~2:1; 3) C2H5NS and CoCl2·6H2O are dissolved in deionized water to form a mixed solution III and stirred; the mixed solution III is transferred to the inner lining of the reactor, and then the Co-N / CP prepared in step 2) is placed in the mixed solution III, and the sample Co9S8 / Co-N / CP is obtained after a second hydrothermal reaction and a second calcination; 10 ml~20 ml of the mixed solution III is added to each piece of Co-N / CP; the molar ratio of C2H5NS and CoCl2·6H2O is 1:1~2:
1.
2. The method according to claim 1, characterized in that: In the step 1), the volume ratio of concentrated sulfuric acid to concentrated nitric acid in the mixed solution 1 is 3:1; the temperature used for soaking at high temperature is 70-85°C, and the soaking time is 1-3h; the drying temperature used for drying overnight is 60-80°C.
3. The method according to claim 2, characterized in that: The temperature of the first hydrothermal reaction is 140° C.-180° C.; the temperature of the first calcination is 500° C., the heating rate is 3° C. / min, and the calcination time is 2 hours.
4. The method according to claim 3, characterized in that: The temperature of the second hydrothermal reaction is 120°C-140°C; the temperature of the second calcination is 450-600°C, the heating rate is 1-3°C / min, and the calcination time is 1-2 hours.
5. The method according to claim 4, characterized in that: The molar ratio of C2H5NS to CoCl2·6H2O is 4:
3.
6. A Co9S8 / Co-N / CP electrode material prepared by the method according to any one of claims 1 to 5.
7. Use of the Co9S8 / Co-N / CP electrode material as claimed in claim 6 in water electrolysis materials.