Low dielectric composite film for copper-clad laminate and copper-clad laminate including the same
By using a low-dielectric composite film of expanded polytetrafluoroethylene porous substrate and polyimide compounds on the copper clad laminate, the problems of dielectric constant and dielectric loss in the high frequency band of 5G are solved, and excellent results are achieved The mechanical properties and low thermal expansion coefficient are suitable for signal transmission of 5G base stations or repeaters.
Patent Information
- Application Number
- CN202080097785.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-10
- Filing Date
- 2020-11-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-11-24
AI Technical Summary
The existing low-dielectric film and copper-clad foil laminate cannot effectively reduce dielectric constant and dielectric loss in the high frequency band of 5G, and the mechanical performance and thermal expansion coefficient are poor, which cannot meet the signal transmission needs of 5G base stations or repeaters.
Using a low-dielectric composite film containing expanded polytetrafluoroethylene porous substrate and polyimide compounds, polyimide-based substrate is filled with polyimide-based substrate and applied polyimide-based substrate on its surface and inside. and adhesive layer, optimize material composition to reduce dielectric constant and dielectric loss, while improving mechanical properties and reducing thermal expansion coefficient.
It achieves significantly low dielectric constant and dielectric loss, excellent mechanical properties and significantly low thermal expansion coefficient, and is suitable for substrate materials in the high frequency band of 5G to meet the needs of signal transmission.
Smart Images

Figure CN115210077B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a low dielectric composite film for copper clad laminates (CCLs), and more particularly to a low dielectric composite film for copper clad laminates having significantly low dielectric constant and dielectric loss and excellent mechanical properties and also exhibiting a significantly low thermal expansion coefficient effect, and a low dielectric copper clad laminate comprising the same. Background Art
[0002] The era of downloading 1GB in 10 seconds, that is, the era of 5G networks, is opening up. At the International Consumer Electronics Show 2017 (CES 2017), Intel announced the world's first 5G modem and predicted that based on gigabit speeds, innovations will appear in various fields such as self-driving cars, the Internet of Things, and wireless broadband. In this way, mobile telecommunications companies are already turning to the fifth generation of mobile communications. The International Telecommunication Union (ITU) held a radiocommunication conference in October 2015 and set the official technical name of 5G as "International Mobile Telecommunications (IMT)-2020". 5G is the abbreviation of "5th generation mobile communications".
[0003] According to the definition given by the International Telecommunication Union, 5G is a mobile communication technology with a maximum download speed of 20Gbps and a minimum download speed of 100Mbps. In addition, it can be 1km 2 One million devices within the radius provide Internet of Things (IoT) services, and free communication should be possible even on a high-speed train traveling at 500 km / h. 5G download speed is more than 70 times faster than 300Mbps, which is the current mobile communication speed, and 280 times faster than general LTE. This is the speed at which a 1GB movie can be downloaded in 10 seconds. 5G is not just about transmission speed. Not only transmission speed, but also response speed has been significantly improved. If data transmission speed is an indicator of how much data can pass at a time, response speed measures the time it takes for small data to pass. In 4G, the response speed has increased to 10ms to 50ms (milliseconds, one thousandth of a second). In 5G, the above response speed will be about 10 times faster. Thanks to this, 5G will be actively introduced into the fields of self-driving cars and the Internet of Things, which must constantly send and receive large amounts of data to and from central servers.
[0004] On the other hand, unlike 4G, which uses frequencies below 2GHz, 5G uses an ultra-high frequency band of 28GHz. The signals transmitted and received in the mobile communication system are radio waves. The 5G currently under construction uses high frequency bands of 3.5GHz and 28GHz, which is significantly higher than 4G. Therefore, the diffraction characteristics are lower than 4G (strong straightness) and the radio wave reach distance is short. Due to these communication characteristics, more base stations or repeaters need to be installed than 4G.
[0005] Electrical signals have the characteristic that the transmission loss increases with the frequency. In the case of conventional low dielectric films and copper-clad laminates, it is impossible to achieve the required level of low dielectric constant and dielectric loss, so it is impossible to minimize or prevent signal interference in the high-frequency band. Even if the predetermined low dielectric constant is achieved, there are problems such as reduced mechanical properties or high thermal expansion coefficient.
[0006] Therefore, there is an urgent need to develop a material with significantly low dielectric constant and dielectric loss, excellent mechanical properties, and significantly low thermal expansion coefficient. Summary of the invention
[0007] Technical issues
[0008] The present invention is developed in view of the above problems, and its purpose is to provide a low-dielectric composite film for copper-clad laminates having significantly low dielectric constant and dielectric loss and excellent mechanical properties, and also exhibiting a significantly low thermal expansion coefficient effect, and a low-dielectric copper-clad laminate comprising the same.
[0009] Solutions to the problem
[0010] In order to solve the above problems, the present invention provides a low dielectric composite film for copper-clad laminates, the low dielectric composite film comprising a core layer, the core layer being formed by a porous substrate comprising expanded polytetrafluoroethylene (ePTFE) and having a plurality of pores and a polyimide compound, the core layer comprising a polyimide matrix filled in the pores of the porous substrate.
[0011] According to an embodiment of the present invention, the content of the porous substrate may be 20 wt % to 85 wt % relative to the total weight of the core layer.
[0012] In addition, the porous substrate may be contained in an amount of 15 volume % to 80 volume % relative to the total volume of the core layer.
[0013] In addition, the core layer may further include a polyimide layer, which is disposed on at least one of the upper surface and the lower surface of the porous substrate and is derived from the polyimide matrix.
[0014] Furthermore, the content of the polyimide layer may be 8 volume % to 80 volume % relative to the total volume of the core layer.
[0015] In addition, the ratio of the tensile strength in the MD direction to the tensile strength in the TD direction of the porous substrate may be 1:0.4 to 1:2.5.
[0016] Furthermore, the ratio of the total thickness of the polyimide-based layer to the thickness of the porous substrate may be 1:0.2 to 1:12.
[0017] In addition, the core layer may include a first polyimide layer and a second polyimide layer on the upper surface and the lower surface of the porous substrate, respectively, and a thickness ratio of the first polyimide layer to the second polyimide layer may be 1:0.5 to 1:1.5.
[0018] Furthermore, the imidization rate of the polyimide-based substrate measured according to the following measurement method 1 may be 90% or more.
[0019] [Measurement method 1]
[0020] The imidization rate of the standard sample imidized at 380°C for 60 minutes was assumed to be 100%. The 1,700 cm thick polyimide substrate was analyzed by infrared spectroscopy. -1 Wavelength and 1,615cm -1 After measuring the peak size at the wavelength, the PI index is calculated according to the following mathematical formula 1, and then the imidization rate is calculated according to the following mathematical formula 2.
[0021] [Mathematical formula 1]
[0022] PI index = 1,700 cm -1 Peak area at wavelength (PI peak) / 1,615㎝ -1 Peak area at wavelength (PAA peak)
[0023] [Mathematical formula 2]
[0024] Imidization rate (%) = (PI index of polyimide matrix / PI index of reference sample) × 100 (%)
[0025] In addition, an adhesive layer may be further included on one or both sides of the core layer.
[0026] In addition, the polyimide matrix can be formed by imidizing a polyamic acid formed by polymerizing a dianhydride and a diamine, wherein the dianhydride includes BPDA (3,3',4,4'-biphenyltetracarboxylic dianhydride), PMDA (pyromellitic dianhydride), ODPA (4,4'-oxydiphthalic anhydride), BTDA (benzophenone-3,3',4,4'-tetracarboxylic dianhydride), BPADA (2,2-Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride), and BPDA (2,2-Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride). At least one of the group consisting of pPDA (paraphenylenediamine), TAHQ (ditricarboxylic anhydride hydroquinone ester), 6FDA (2,2-bis(3,4-anhydrodicarboxyphenyl)hexafluoropropane), CBDA (cyclobutane-1,2,3,4-tetracarboxylic dianhydride) and CHDA (1,2,4,5-cyclohexanetetracarboxylic dianhydride), wherein the diamine comprises at least one selected from the group consisting of pPDA (paraphenylene diamine), 6FDA (2,2-bis(3,4-anhydrodicarboxyphenyl)hexafluoropropane), CBDA (cyclobutane-1,2,3,4-tetracarboxylic dianhydride) and CHDA (1,2,4,5-cyclohexanetetracarboxylic dianhydride). diamine), ODA (4,4'-oxydianiline), TPE-R (1,3-Bis(4-aminophenoxy)benzene), TPE-Q (1,4-Bis(4-aminophenoxy)benzene), BAPP (2,2-Bis[4-(4-aminophenoxy)Phenyl]Propane), M-Tolidine (2,2'-Dimethyl-4,4'-diamino-2,2'-dimethylbiphenyl), and TPE-Q (1,4-Bis(4-aminophenoxy)benzene).At least one of the group consisting of: 4,4'-diaminobiphenyl), O-Tolidine (4,4'-diamino-3,3'-dimethylbiphenyl), TFDB (2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diamine) and HFBAPP (2,2-Bis[4-(4-aminophenoxy)phenyl]hexafluoropropane).
[0027] In addition, the adhesive layer may be included in an amount of 2 volume % to 40 volume % relative to the total volume of the core layer and the adhesive layer.
[0028] Furthermore, the polyimide-based matrix may include at least one of fluorine-based particles and ceramic particles.
[0029] Furthermore, the fluorine-based particles may include at least one selected from the group consisting of polyvinyl fluoride (PTFE), perfluoroalkoxy copolymer (PFA, MFA), fluorinated ethylene propylene copolymer (FEP, fluorinated ethylene propylene copolymer), ethylene-tetrafluoroethylene copolymer (ETFE, ethylene tetrafluoroethylene copolymer) and ethylene-chlorotrifluoroethylene copolymer (ECTFE, ethylene chlorotrifluoroethylene copolymer).
[0030] Furthermore, the ceramic particles may be ceramic particles including at least one element selected from the group consisting of B, Na, Mg, Al, Si, P, K, Ca, and Ti.
[0031] Furthermore, the ceramic particles may include at least one of hollow ceramic particles and non-hollow ceramic particles.
[0032] In addition, the present invention provides a low-dielectric copper-clad laminate, which includes: a core layer, formed by including a porous substrate containing expanded polytetrafluoroethylene and having multiple pores and a polyimide compound, the core layer includes a polyimide matrix filled in the pores of the porous substrate; copper foil, arranged on one side or both sides of the core layer; and an adhesive layer, between the core layer and the copper foil.
[0033] Effects of the Invention
[0034] The low dielectric composite film for copper clad laminates and the low dielectric copper clad laminates comprising the same according to the present invention have significantly low dielectric constant and dielectric loss, excellent mechanical properties and significantly low thermal expansion coefficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a cross-sectional view of a low dielectric composite film for a copper-clad laminate according to an embodiment of the present invention,
[0036] Figure 2 is a cross-sectional view of a low dielectric composite film for a copper-clad laminate according to another embodiment of the present invention,
[0037] Figure 3 FIG. 4 is a cross-sectional view of a low dielectric copper clad laminate for copper clad laminates according to an embodiment of the present invention. DETAILED DESCRIPTION
[0038] Best Mode for Carrying Out the Invention
[0039] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings so that a person skilled in the art can easily implement the present invention. The present invention can be implemented in a variety of different embodiments and is not limited to the embodiments described in this specification. In order to clearly illustrate the present invention, parts not related to the description are omitted in the accompanying drawings, and the same reference numerals are given to the same or similar structural elements throughout the specification.
[0040] like Figure 1 and Figure 2 As shown, the low dielectric composite film 1000, 1001 according to the present invention comprises a core layer 100, wherein the core layer 100 comprises a porous substrate 10 including a plurality of pores and a polyimide matrix filled in the pores of the porous substrate.
[0041] The porous substrate performs a function of supporting the low dielectric composite film and a function of expressing low dielectric properties, and includes expanded polytetrafluoroethylene.
[0042] The ratio of the tensile strength in the MD direction of the porous substrate to the tensile strength in the TD direction may be 1:0.4 to 1:2.5, preferably, the ratio of the tensile strength in the MD direction to the tensile strength in the TD direction may be 1:0.8 to 1:1.7. If the ratio of the tensile strength in the MD direction to the tensile strength in the TD direction is less than 1:0.4 or greater than 1:2.5, the low dielectric composite film may be deformed due to shrinkage and stress differences in various directions.
[0043] Furthermore, the above-mentioned polyimide-based matrix performs the functions of exhibiting low dielectric properties and reducing a thermal expansion coefficient.
[0044] As described above, the polyimide-based matrix partially or completely blocks the pores of the porous substrate 10 . Preferably, the polyimide-based matrix can block all the pores of the porous substrate 10 .
[0045] On the other hand, the polyimide matrix can be formed by imidizing a polyamic acid formed by polymerizing a dianhydride and a diamine, wherein the dianhydride includes BPDA (3,3',4,4'-biphenyltetracarboxylic dianhydride), PMDA (pyromellitic dianhydride), ODPA (4,4'-oxydiphthalic anhydride), BTDA (benzophenone tetracarboxylic dianhydride), BPADA (2,2-Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride), and BPDA (2,2-Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride). At least one of the group consisting of pPDA (paraphenylenediamine), TAHQ (ditricarboxylic anhydride hydroquinone ester), 6FDA (2,2-bis(3,4-anhydrodicarboxyphenyl)hexafluoropropane), CBDA (cyclobutane-1,2,3,4-tetracarboxylic dianhydride) and CHDA (1,2,4,5-cyclohexanetetracarboxylic dianhydride), wherein the diamine comprises at least one selected from the group consisting of pPDA (paraphenylene diamine), 6FDA (2,2-bis(3,4-anhydrodicarboxyphenyl)hexafluoropropane), CBDA (cyclobutane-1,2,3,4-tetracarboxylic dianhydride) and CHDA (1,2,4,5-cyclohexanetetracarboxylic dianhydride). diamine), ODA (4,4'-oxydianiline), TPE-R (1,3-Bis(4-aminophenoxy)benzene), TPE-Q (1,4-Bis(4-aminophenoxy)benzene), BAPP (2,2-Bis[4-(4-aminophenoxy)Phenyl]Propane), M-Tolidine (2,2'-Dimethyl-4,4'-diamino-2,2'-dimethylbiphenyl), and TPE-Q (1,4-Bis(4-aminophenoxy)benzene).At least one of the group consisting of 4,4'-diaminobiphenyl), O-Tolidine (4,4'-diamino-3,3'-dimethylbiphenyl), TFDB (2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diamine) and HFBAPP (2,2-Bis[4-(4-aminophenoxy)phenyl]hexafluoropropane), preferably, the dianhydride comprises at least one selected from the group consisting of BPDA (3,3',4,4'-biphenyltetracarboxylic acid dianhydride). dianhydride), PMDA (pyromellitic dianhydride), ODPA (4,4'-oxydiphthalic anhydride), BTDA (benzophenone-3,3',4,4'-tetracarboxylic dianhydride) and 6FDA (2,2-bis(3,4-anhydrodicarboxyphenyl)hexafluoropropane), wherein the diamine comprises at least one selected from the group consisting of pPDA (paraphenylene diamine), diamine), ODA (4,4'-oxydianiline) and TFDB (2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diamine).
[0046] On the other hand, the above polymerization can be carried out in a mixture selected from the group consisting of DMF (N,N-dimethylformamide), DMAc (N,N-dimethylacetamide), NMP (1-methyl-2-pyrrolidone), NEP (N-ethyl-2-pyrrolidone), GBL (γ-butyrolactone), GVL (γ-valerolactone), DVL (δ-valerolactone), ethylene carbonate, propylene carbonate, The method is carried out in the presence of at least one solvent selected from the group consisting of carbonate, m-cresol, p-cresol, acetophenone, THF (tetrahydrofuran), dimethoxyethane, diethoxyethane, dibutyl ether, diethylene glycol dimethyl ether, methyl isobutyl ketone, diisobutyl ketone, cyclohexanone, methyl ethyl ketone, acetone, butanol, ethanol, xylene, toluene and chlorobenzene.
[0047] Specifically, the polyimide matrix can be formed by the method described below. Here, the method described below is explained by taking BPDA and PMDA as the dianhydride and pPDA and ODA as the diamine as an example.
[0048] First, at room temperature and nitrogen atmosphere, pPDA and ODA are completely dissolved in a polar aprotic solvent for general polyimide polymerization, and BPDA in two acid dianhydrides is added within 15 minutes to 45 minutes. After the above solution is stirred for 5 minutes to 15 minutes, PMDA is added within 15 minutes to 45 minutes. Afterwards, the reaction is carried out at a reaction temperature of 0°C to 60°C for 8 hours to 24 hours to prepare a polyamic acid solution. At this time, the solid content of the above polyamic acid solution can be 5% to 25% by weight, preferably, the solid content can be 10% to 20% by weight, and the viscosity of the above polyamic acid solution at 25°C can be 2000cps to 5000cps, preferably, the viscosity can be 2500cps to 4500cps. The above polyamic acid solution is filtered with a predetermined filter to prepare an impregnation solution. Afterwards, the porous substrate is immersed in the impregnation solution so that all the pores inside the porous substrate are blocked by the impregnation solution, and then the porous substrate is dried for 1 minute to 10 minutes at 65°C to 95°C, and then the solvent is removed by secondary drying at 100°C to 140°C for 5 minutes to 15 minutes, thereby preparing a composite film including a porous substrate and polyamic acid, wherein the polyamic acid is contained in the pores and both sides of the porous substrate. Finally, the polyamic acid is imidized by performing a heat treatment at 170°C to 260°C and a secondary heat treatment at 240°C to 360°C, thereby preparing a low dielectric composite film 1000, 1001 including a porous substrate 10 and a polyimide matrix. At this time, in order to minimize the shrinkage and curling of the film, the heat treatment can be performed under transverse (TD) stretching conditions by a tenter (roller stretching machine) device.
[0049] On the other hand, the content of the porous substrate 10 may be 20% to 85% by weight, preferably 60% to 80% by weight, relative to the total weight of the core layer 100. If the content of the porous substrate is less than 20% by weight relative to the total weight of the core layer, the dielectric constant and dielectric loss of the low-dielectric composite film and the low-dielectric copper-clad laminate increase, making it difficult to use them as 5G high-frequency substrate materials. If the content of the porous substrate exceeds 85% by weight, the mechanical strength may be reduced.
[0050] In addition, the content of the porous substrate 10 may be 15 volume % to 80 volume %, preferably 50 volume % to 75 volume %, relative to the total volume of the core layer 100. If the content of the porous substrate is less than 15 volume % relative to the total volume of the core layer, the dielectric constant and dielectric loss may increase, and if the content of the porous substrate exceeds 80 volume %, the mechanical strength may decrease.
[0051] On the other hand, the core layer 100 may further include polyimide layers 20a and 20b, which are disposed on at least one of the upper surface and the lower surface of the porous substrate 10 and are derived from the polyimide matrix.
[0052] At this time, since the polyimide-based layer is derived from the polyimide-based matrix, it can be formed by including the same compound as the polyimide-based compound of the polyimide-based matrix.
[0053] On the other hand, the content of the polyimide layers 20a and 20b may be 8% to 80% by volume, preferably 10% to 40% by volume, relative to the total volume of the core layer 100. If the content of the polyimide layers is less than 8% by volume relative to the total volume of the porous substrate and the polyimide matrix, the mechanical strength may be reduced, and if the content exceeds 80% by volume, the dielectric constant and dielectric loss may be increased.
[0054] In addition, the thickness ratio between the total thickness of the polyimide layers 20a and 20b and the thickness of the porous substrate 10 may be 1:0.2 to 1:12, and preferably, the thickness ratio may be 1:4 to 1:11.5. If the thickness ratio between the total thickness of the polyimide layers and the thickness of the porous substrate is less than 1:0.2, the dielectric constant and dielectric loss may increase, and if the thickness ratio exceeds 1:12, the mechanical strength may decrease.
[0055] On the other hand, Figure 1 and Figure 2 As shown, in the core layer 100, the first polyimide layer 20a and the second polyimide layer 20b may be respectively included on the upper surface and the lower surface of the porous substrate 10. Specifically, the first polyimide layer 20a may be included on the upper surface of the porous substrate 10, and the second polyimide layer 20b may be included on the lower surface of the porous substrate 10.
[0056] At this time, the thickness ratio of the first polyimide layer 20a to the second polyimide layer 20b may be 1:0.5 to 1:1.5, preferably, the thickness ratio may be 1:0.7 to 1:1.3. If the thickness ratio exceeds the above range, uneven interlayer stress occurs, causing the composite film and / or copper-clad laminate to curl, and may be deformed due to excessive internal stress.
[0057] On the other hand, the imidization rate of the polyimide-based substrate measured according to the following measurement method 1 may be 90% or more, and preferably, the imidization rate measured according to the following measurement method 1 may be 95% or more.
[0058] [Measurement method 1]
[0059] The imidization rate of the standard sample imidized at 380°C for 60 minutes was assumed to be 100%. The 1,700 cm thick polyimide substrate was analyzed by infrared spectroscopy. -1 Wavelength and 1,615cm -1 After measuring the peak size at the wavelength, the PI index is calculated according to the following mathematical formula 1, and then the imidization rate is calculated according to the following mathematical formula 2.
[0060] [Mathematical formula 1]
[0061] PI index = 1,700 cm -1 Peak area at wavelength (PI peak) / 1,615㎝ -1 Peak area at wavelength (PAA peak)
[0062] [Mathematical formula 2]
[0063] Imidization rate (%) = (PI index of polyimide matrix / PI index of reference sample) × 100 (%)
[0064] If the imidization rate measured according to the above-mentioned measurement method 1 is less than 90%, the dielectric constant and dielectric loss may increase, and there may be a problem of an increase in the thermal expansion coefficient.
[0065] At this time, the PI index may be calculated according to the following Mathematical Formula 3, but the present invention is not limited thereto.
[0066] [Mathematical formula 3]
[0067] PI index = 1,700 cm -1 Peak area at wavelength (PI peak) / 1,510㎝ -1 Peak area at wavelength (PI, PAA peak)
[0068] On the other hand, Figure 2 As shown, the low dielectric composite film 1001 according to an embodiment of the present invention may further include an adhesive layer 200 on one or both sides of the core layer 100 .
[0069] The adhesive layer 200 performs the function of fixing the copper foil of the copper-clad laminate described below on the low dielectric composite film. As the adhesive layer, any adhesive layer formed of an adhesive layer material commonly used in the art can be used without restriction, and preferably, it can be at least one adhesive layer selected from the group consisting of an epoxy adhesive layer, a thermoplastic polyimide adhesive layer, a silicone adhesive layer, and an acrylic adhesive layer.
[0070] On the other hand, the content of the adhesive layer 200 may be 2 volume % to 40 volume %, preferably 4 volume % to 30 volume %, relative to the total volume of the core layer 100 and the adhesive layer 200. If the content of the adhesive layer 200 is less than 2 volume % relative to the total volume of the core layer 100 and the adhesive layer 200, the adhesion between the copper foil and the polyimide matrix is insufficient, resulting in interlayer delamination in the low-dielectric copper-clad laminate and reduced mechanical properties. If the content of the adhesive layer is greater than 40 volume %, the dielectric constant and dielectric loss may increase.
[0071] On the other hand, according to another embodiment of the present invention, the polyimide-based matrix may include at least one of fluorine-based particles and ceramic particles.
[0072] As the above-mentioned fluorine-based particles, any fluorine-based particles commonly used in the art can be used without restriction. Preferably, the above-mentioned fluorine-based particles can include at least one selected from the group consisting of polyfluoroethylene (PTFE), perfluoroalkoxy copolymer (PFA, MFA, perfluoroalkoxy copolymer), fluorinated ethylene propylene copolymer (FEP, fluorinated ethylene propylene copolymer), ethylene-tetrafluoroethylene copolymer (ETFE, ethylene tetrafluoroethylene copolymer) and ethylene-chlorotrifluoroethylene copolymer (ECTFE, ethylene chlorotrifluoroethylene copolymer).
[0073] In addition, as the above-mentioned ceramic particles, any ceramic particles commonly used in the art can be used without limitation, and preferably, the above-mentioned ceramic particles can include at least one element selected from the group consisting of B, Na, Mg, Al, Si, P, K, Ca and Ti. In this case, the composition of the above-mentioned ceramic particles can include the above-mentioned elements, and the method of including the above-mentioned elements can be changed according to the purpose, such as by forming by doping the above-mentioned elements on the surface, etc., and there is no particular limitation on this in the present invention.
[0074] Furthermore, the ceramic particles may include at least one of hollow ceramic particles including a hollow portion and non-hollow ceramic particles.
[0075] On the other hand, depending on the size of the fluorine-based particles and / or ceramic particles, the particles may not exist in the polyimide matrix contained in the porous substrate, but may exist only in the polyimide layer, but the present invention is not limited thereto.
[0076] like Figure 3As shown, the low dielectric copper clad laminate 2000 according to the present invention includes: a core layer 100, including: a porous substrate 10, having a plurality of pores; and a polyimide matrix, filled in the pores of the above-mentioned porous substrate; a copper foil 300, arranged on one side or both sides of the above-mentioned core layer 100; and an adhesive layer 200, between the above-mentioned core layer and the copper foil.
[0077] The copper foil 300 may be a copper foil with known specifications commonly used in the art, and there is no particular limitation on this in the present invention.
[0078] Modes for carrying out the invention
[0079] The present invention will be described in more detail by the following examples, but the following examples should not be construed as limiting the scope of the present invention but should be construed as helping to understand the present invention.
[0080] [Example]
[0081] <Example 1: Preparation of low dielectric composite film for copper clad laminate>
[0082] First, under nitrogen atmosphere, pPDA and ODA were added to DMAc as a polymerization solvent, completely dissolved at room temperature, and then BPDA was added within 30 minutes. After stirring the above solution for 10 minutes, PMDA was added within 30 minutes. Afterwards, a polyamic acid solution was prepared by reacting at a temperature below 20°C for 16 hours. Thus, a polyamic acid solution having a solid content of 15% by weight and a viscosity of 3500cps at 25°C was obtained, and then filtered with a MINIFLOW filter (CTS-CAP10 A grade) of Chungsoo Technofil, South Korea, and finally a dipping solution having a solid content of 15% by weight was prepared.
[0083] After that, the porous substrate including a plurality of pores, which is expanded polytetrafluoroethylene having a thickness of 40 μm, was impregnated into the impregnation solution prepared above to block all the plurality of pores of the porous substrate, and then, in order to remove the solvent, primary drying was performed at a temperature of 80° C. for 5 minutes and secondary drying was performed at a temperature of 120° C. for 10 minutes. At this time, the tensile strength of the porous substrate in the MD direction was 30 MPa, the tensile strength in the TD direction was 25 MPa, and the ratio of the tensile strength in the MD direction to the tensile strength in the TD direction was 1:0.8.
[0084] Thereafter, the polyamic acid was imidized by performing a primary heat treatment at a temperature of 250° C. for 10 minutes and a secondary heat treatment at a temperature of 350° C. for 5 minutes, thereby preparing Figure 1The low dielectric composite film including the porous substrate and the polyimide matrix is shown. At this time, in order to minimize the occurrence of shrinkage and curling of the film, heat treatment is performed under transverse stretching conditions by a tenter (roller stretching machine) device.
[0085] In the prepared low dielectric composite film, the thickness of the first polyimide layer and the second polyimide layer are 5 μm, respectively, the content of the porous substrate is 73% by weight relative to the total weight of the prepared low dielectric composite film, the content of the porous substrate is 64% by volume relative to the total volume of the prepared low dielectric composite film, and the content of the polyimide layer is 25% by volume. In addition, in the prepared low dielectric composite film, the imidization rate of the polyimide matrix measured according to the following measurement method 1 is 98%.
[0086] [Measurement method 1]
[0087] The imidization rate was analyzed by Fourier transform infrared spectroscopy (FT-IR). The imidization rate of the standard sample imidized at 380°C for 60 minutes was assumed to be 100%. The imidization rate of the polyimide substrate of 1,700 cm was analyzed by infrared spectrometer. -1 Wavelength and 1,615cm -1 After measuring the peak size at the wavelength, the PI index is calculated according to the following mathematical formula 1, and then the imidization rate is calculated according to the following mathematical formula 2.
[0088] [Mathematical formula 1]
[0089] PI index = 1,700 cm -1 Peak area at wavelength (PI peak) / 1,615㎝ -1 Peak area at wavelength (PAA peak)
[0090] [Mathematical formula 2]
[0091] Imidization rate (%) = (PI index of polyimide matrix / PI index of reference sample) × 100 (%)
[0092] <Examples 2 to 13 and Comparative Examples 1 to 2>
[0093] Except for changing the weight percentage, volume percentage of the porous substrate, the volume percentage of the polyimide layer, the thickness ratio between the total thickness of the polyimide layer and the thickness of the porous substrate, the imidization rate of the polyimide matrix, whether the porous substrate is included, and whether the polyimide matrix is included, the rest is prepared in the same manner as in Example 1, thereby preparing low dielectric composite films as shown in Tables 1 to 3.
[0094] <Experimental Example 1>
[0095] The following physical properties of each low dielectric composite film prepared according to the examples and comparative examples were evaluated, and the results are shown in Tables 1 to 3.
[0096] 1. Dielectric constant and dielectric loss measurement
[0097] For each low dielectric composite film, a network analyzer (E8364A (45 MHz to 50 GHz), Agilent Technologies, Inc., USA) was used to measure the dielectric constant and dielectric loss of the thin film type sample in the gigahertz (GHz) region through a resonant cavity.
[0098] 2. Mechanical properties evaluation
[0099] For each low dielectric composite film, the tensile strength was measured using a Universal Testing Machine (UTM) according to ASTM-D882 standard.
[0100] 3. Thermal expansion coefficient measurement
[0101] For each low dielectric composite film, the thermal expansion coefficient was measured using a thermal mechanical analyzer (Pyris Diamond TMA, Perkin Elmer Instrument, USA). The measurement was performed at a temperature range of 30°C to 400°C under a nitrogen flow at a temperature increase of 10°C / min, and then the average value between 50°C and 250°C was calculated.
[0102] Table 1
[0103]
[0104] Table 2
[0105]
[0106]
[0107] Table 3
[0108]
[0109]
[0110] It can be seen from Tables 1 to 3 above that Examples 1, 3, 4, 8, 11 and 12, which all meet the conditions of the weight percentage of the porous substrate, the volume percentage of the polyimide layer, the thickness ratio between the total thickness of the polyimide layer and the thickness of the porous substrate, the imidization rate of the polyimide matrix, whether the porous substrate is included, and whether the polyimide matrix is included, have significantly lower dielectric constants and dielectric losses, excellent mechanical properties, and a low thermal expansion coefficient, compared with Examples 2, 5, 6, 7, 9, 10, 13 and Comparative Examples 1 to 2, which do not meet at least one of the conditions.
[0111] On the other hand, the thermal expansion coefficient of Comparative Example 2 was too high to be measured.
[0112] <Examples 14 to 19>
[0113] Low dielectric composite films were prepared in the same manner as in Example 1, except that BPDA and PMDA as dianhydrides in Example 1 were changed to BPDA and ODPA (Example 14), BPDA and BTDA (Example 15), BPDA and 6FDA (Example 16), PMDA and ODPA (Example 17), PMDA and BTDA (Example 18), and PMDA and 6FDA (Example 19).
[0114] <Examples 20 to 21>
[0115] A low dielectric composite film was prepared in the same manner as in Example 1 except that pPDA and ODA as diamines in Example 1 were changed to pPDA and TFDB (Example 20) and ODA and TFDB (Example 21).
[0116] <Examples 22 to 24>
[0117] The low dielectric composite film was prepared in the same manner as in Example 1, except that BPDA and PMDA as dianhydrides in Example 1 were changed to 6FDA (Example 22), ODPA (Example 23), and BTDA (Example 24) and used separately to prepare polyamic acid.
[0118] <Examples 25 to 26>
[0119] The low dielectric composite film was prepared in the same manner as in Example 1, except that pPDA and ODA as diamines in Example 1 were replaced by TFDB (Example 25) and BAPP (Example 26) and were used separately to prepare polyamic acid.
[0120] <Experimental Example 2>
[0121] The following physical properties of each of the low dielectric composite films prepared according to Examples 14 to 26 were evaluated, and the results are shown in Tables 4 and 5.
[0122] 1. Dielectric constant and dielectric loss measurement
[0123] For each low dielectric composite film, a network analyzer (E8364A (45 MHz to 50 GHz), Agilent Technologies, Inc.) was used to measure the dielectric constant and dielectric loss in the gigahertz region of the thin film type sample through a resonant cavity.
[0124] 2. Mechanical properties evaluation
[0125] For each low dielectric composite film, the tensile strength was measured using a Universal Testing Machine (UTM) according to ASTM-D882 standard.
[0126] 3. Thermal expansion coefficient measurement
[0127] For each low dielectric composite film, the thermal expansion coefficient was measured using a thermal mechanical analyzer (Pyris Diamond TMA, Perkin Elmer Instrument, USA). The measurement was performed at a temperature range of 30°C to 400°C under a nitrogen flow at a temperature increase of 10°C / min, and then the average value between 50°C and 250°C was calculated.
[0128] Table 4
[0129]
[0130]
[0131] Table 5
[0132]
[0133] It can be seen from the above Tables 4 and 5 that Examples 14 to 21 satisfying the types of dianhydride and diamine according to the present invention have significantly lower dielectric constants and dielectric losses than Examples 22 to 26 not satisfying them, and at the same time exhibit the effects of excellent mechanical properties and low thermal expansion coefficient.
[0134] <Preparation Example 1>
[0135] A single-liquid epoxy solution containing a latent curing agent and an acrylic resin was applied to the upper surface of the low dielectric composite film prepared according to Example 1, and then dried at a temperature of 100° C. to prepare a low dielectric composite film including an adhesive layer having a thickness of 6 μm. Wherein, 10 parts by weight of dicyandiamide (DICY) and an acrylic resin as a latent curing agent were included relative to 100 parts by weight of the single-liquid epoxy resin. At this time, the content of the adhesive layer was 6% by volume relative to the total volume of the prepared low dielectric composite film.
[0136] <Preparation Examples 2 to 6>
[0137] The low dielectric composite films shown in Table 6 below were prepared in the same manner as Preparation Example 1 except that the volume percentage of the adhesive layer relative to the total volume of the low dielectric composite film was changed.
[0138] <Experimental Example 3>
[0139] The following physical properties of the low dielectric composite films prepared according to the above Preparation Examples 1 to 6 were evaluated, and the results are shown in Table 6 below.
[0140] 1. Dielectric constant and dielectric loss measurement
[0141] For each low dielectric composite film, a network analyzer (E8364A (45 MHz to 50 GHz), Agilent Technologies, Inc.) was used to measure the dielectric constant and dielectric loss in the gigahertz region of the thin film type sample through a resonant cavity.
[0142] 2. Adhesion Strength Measurement
[0143] For each low dielectric composite film according to the preparation example, the time point at which the copper layer was peeled off when pulled up in a 90 degree direction was measured and evaluated according to the evaluation specification of IPC-TM-650 2.4.9.1.
[0144] Table 6
[0145]
[0146] It can be seen from Table 6 above that Preparation Examples 1, 3 and 4 that meet the volume percentage of the adhesive layer and the volume percentage of the polyimide layer according to the present invention show significantly lower dielectric constants and dielectric losses and excellent bonding strength compared with Preparation Examples 2 and 6 that do not meet them.
[0147] As described above, one embodiment of the present invention is described, but the subject matter of the present invention is not limited to the embodiment in the present invention. A person skilled in the art can easily propose other embodiments within the scope of the same subject matter by adding, modifying, deleting, increasing, etc. the constituent elements, and these belong to the scope of the subject matter of the present invention.
Claims
1. A low dielectric composite film for copper-clad laminates, characterized in that: The invention comprises a core layer, wherein the core layer is formed by a porous substrate including expanded polytetrafluoroethylene and having a plurality of pores and a polyimide compound, wherein the core layer comprises a polyimide matrix filled in the pores of the porous substrate, The core layer is disposed on at least one of the upper surface and the lower surface of the porous substrate, and further comprises a polyimide layer derived from the polyimide matrix. The content of the porous substrate is 20 wt % to 85 wt % relative to the total weight of the core layer. The content of the porous substrate is 15 volume % to 80 volume % relative to the total volume of the core layer. The content of the polyimide layer is 8 volume % to 40 volume % relative to the total volume of the core layer. The imidization rate of the polyimide matrix measured according to the following measurement method 1 is 90% or more: [Measurement method 1] The imidization rate of the standard sample imidized at 380°C for 60 minutes was assumed to be 100%. The 1,700 cm thick polyimide substrate was analyzed by infrared spectroscopy. -1 Wavelength and 1,615cm -1 After measuring the peak size at the wavelength, the PI index is calculated according to the following mathematical formula 1, and then the imidization rate is calculated according to the following mathematical formula 2: [Mathematical formula 1] PI index = 1,700 cm -1 Peak area at wavelength (PI peak) / 1,615㎝ -1 Peak area at wavelength (PAA peak) [Mathematical formula 2] Imidization ratio (%)=(PI index of polyimide-based matrix / PI index of reference sample)×100 (%).
2. The low dielectric composite film for copper-clad laminate according to claim 1, characterized in that: The ratio of the tensile strength in the MD direction to the tensile strength in the TD direction of the porous substrate is 1:0.4 to 1:2.
5.
3. The low dielectric composite film for copper-clad laminate according to claim 1, characterized in that: The ratio of the total thickness of the polyimide layer to the thickness of the porous substrate is 1:0.2 to 1:
12.
4. The low dielectric composite film for copper-clad laminate according to claim 1, characterized in that: The core layer includes a first polyimide layer and a second polyimide layer on the upper surface and the lower surface of the porous substrate, respectively. The thickness ratio of the first polyimide layer to the second polyimide layer is 1:0.5 to 1:1.
5.
5. The low dielectric composite film for copper-clad laminate according to claim 1, characterized in that: An adhesive layer is further included on one or both sides of the core layer.
6. The low dielectric composite film for copper-clad laminate according to claim 1, characterized in that: The polyimide matrix is formed by imidizing a polyamic acid formed by polymerizing a dianhydride and a diamine. The dianhydride includes at least one selected from the group consisting of 3,3',4,4'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, 4,4'-oxydiphthalic anhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, p-phenylene-diphenyltrimethylol dianhydride, 2,2-bis-(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, cyclobutane-1,2,3,4-tetracarboxylic dianhydride and 1,2,4,5-cyclohexanetetracarboxylic dianhydride, The diamine includes at least one selected from the group consisting of p-phenylenediamine, 4,4'-oxydiphenylamine, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxyphenyl)]propane, 4,4'-diamino-2,2'-dimethylbiphenyl, 4,4'-diamino-3,3'-dimethylbiphenyl, 2,2'-bistrifluoromethyl-4,4'-diaminobiphenyl and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.
7. The low dielectric composite film for copper-clad laminate according to claim 5, characterized in that: The content of the adhesive layer is 2 volume % to 40 volume % relative to the total volume of the core layer and the adhesive layer.
8. The low dielectric composite film for copper-clad laminate according to claim 1, characterized in that: The polyimide matrix includes at least one of fluorine particles and ceramic particles.
9. The low dielectric composite film for copper-clad laminate according to claim 8, characterized in that: The fluorine-based particles include at least one selected from the group consisting of vinyl fluoride, perfluoroalkoxy copolymer, fluorinated ethylene propylene copolymer, ethylene-tetrafluoroethylene copolymer and ethylene-chlorotrifluoroethylene copolymer.
10. The low dielectric composite film for copper-clad laminate according to claim 8, characterized in that: The ceramic particles are ceramic particles including at least one element selected from the group consisting of B, Na, Mg, Al, Si, P, K, Ca and Ti.
11. The low dielectric composite film for copper-clad laminate according to claim 8, characterized in that: The ceramic particles include at least one of hollow ceramic particles and non-hollow ceramic particles.
12. A low dielectric copper-clad laminate, characterized in that: include: A core layer is formed by including a porous substrate containing expanded polytetrafluoroethylene and having a plurality of pores and a polyimide compound, wherein the core layer includes a polyimide matrix filled in the pores of the porous substrate; Copper foil, disposed on one or both sides of the core layer; and The bonding layer is between the core layer and the copper foil. The core layer is disposed on at least one of the upper surface and the lower surface of the porous substrate, and further comprises a polyimide layer derived from the polyimide matrix. The content of the porous substrate is 20 wt % to 85 wt % relative to the total weight of the core layer. The content of the porous substrate is 15 volume % to 80 volume % relative to the total volume of the core layer. The content of the polyimide layer is 8 volume % to 40 volume % relative to the total volume of the core layer. The imidization rate of the polyimide matrix measured according to the following measurement method 1 is 90% or more: [Measurement method 1] The imidization rate of the standard sample imidized at 380°C for 60 minutes was assumed to be 100%. The 1,700 cm thick polyimide substrate was analyzed by infrared spectroscopy. -1 Wavelength and 1,615cm -1 After measuring the peak size at the wavelength, the PI index is calculated according to the following mathematical formula 1, and then the imidization rate is calculated according to the following mathematical formula 2: [Mathematical formula 1] PI index = 1,700 cm -1 Peak area at wavelength (PI peak) / 1,615㎝ -1 Peak area at wavelength (PAA peak) [Mathematical formula 2] Imidization ratio (%)=(PI index of polyimide-based matrix / PI index of reference sample)×100 (%).