A low-carbon track pin sleeve steel and preparation method thereof
By adding Cr, Mn, Ti and Al elements to low carbon steel, and using electric furnace smelting, rolling and magnetic particle flaw detection processes, the hardness and wear resistance of track pin sleeve steel is improved, and the problem of track pin sleeve sleeve steel in the existing technology is solved. The problem of insufficient wear resistance and fatigue strength of steel enables long-life use in harsh environments.
Patent Information
- Application Number
- CN202210687035.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-17
AI Technical Summary
The existing steel used for track pin sleeves has insufficient wear resistance and fatigue strength in the harsh working environment of engineering machinery, resulting in serious wear and high failure rate in environments such as mines.
By adding Cr, Mn, Ti and a small amount of Al elements to low carbon steel, a low carbon track pin sleeve steel is prepared. Electric furnace smelting, rolling and magnetic particle flaw detection processes are used to improve the hardness, wear resistance and fatigue strength of the steel. .
The track pin sleeve steel has high hardness, wear resistance, fatigue resistance and good processability, extending the service life in harsh environments.
Smart Images

Figure BDA0003700031350000031 
Figure BDA0003700031350000041 
Figure BDA0003700031350000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a low-carbon track pin sleeve steel and a preparation method thereof. Background Art
[0002] The working environment of construction machinery is very harsh. Ore abrasives and iron media in mines can seriously wear the pin sleeves of construction machinery and cause them to fail. Therefore, it is extremely important to develop a long-life, high-quality steel for pin sleeves.
[0003] Chinese patent CN 107739977 B discloses "low-cost high-end pin sleeve steel and its production method", Chinese patent application CN 112410689 A discloses "a wind power gearbox pin shaft steel and its preparation method", Chinese patent CN102605266 B discloses "a crawler engineering machinery chain track section pin sleeve steel and its manufacturing method", and Chinese patent CN109112253 B discloses "track pin shaft steel with Cr and B elements to improve hardenability and its production method". The composition of the pin shaft pin sleeve steel disclosed in the above four patent applications is different from that of the present invention, and the performance is also different. The pin sleeve of the present invention not only provides the specific index values of the track pin sleeve steel specifications, grain size, hardness, decarburization layer depth, and hairline, but also discloses the production method of such steel. Summary of the invention
[0004] In view of the above-mentioned deficiencies, the object of the present invention is to provide a low-carbon track pin sleeve steel and a preparation method thereof. The steel of the present invention improves the surface hardness, wear resistance and fatigue strength of the steel by adding Cr, Mn, Ti and a small amount of Al elements to the low-carbon steel. The prepared track pin sleeve steel has the characteristics of high hardness, wear resistance, fatigue resistance, good processability and the like.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A low-carbon track pin sleeve steel, the chemical composition of the steel, measured by mass percentage, includes: C: 0.17-0.23%, Si: 0.17-0.37%, Mn: 0.80-1.10%, Cr: 1.00-1.30%, Ti: 0.04-0.1%, Cu≤0.20%, Al: 0.03-0.05%, P≤0.020%, S≤0.030%, O≤20×10 -4 %,H≤2×10 -4 %, the rest are Fe and other inevitable impurity elements; among them, 0.021C+0.025Si+0.017Mn+0.038Cr <Ti+Al<0.042C+0.051Si+0.038Mn+0.081Cr。
[0007] Preferably, the chemical composition of the low-carbon track pin bushing steel includes, by mass percentage, C: 0.18-0.23%, Si: 0.18-0.35%, Mn: 0.90-1.00%, Cr: 1.10-1.30%, Ti: 0.05-0.09%, Cu≤0.20%, Al: 0.03-0.05%, P≤0.020%, S≤0.030%, O≤20×10 -4 %,H≤2×10 -4 %, and the rest are Fe and other inevitable impurity elements.
[0008] The role of Cr: The addition of an appropriate amount of chromium to steel can not only improve the quenching performance of steel, but also improve the uniformity of material structure.
[0009] Role of Ti: Titanium is also one of the strong ferrite forming elements, which strongly increases the A1 and A3 temperatures of steel. Titanium can improve plasticity and toughness in ordinary low alloy steel. Since titanium fixes nitrogen and sulfur and forms titanium carbide, the strength of steel is improved. Normalizing to refine the grains and precipitate the carbides can significantly improve the plasticity and impact toughness of steel. Titanium-containing alloy structural steel has good mechanical properties and process properties, but slightly poor hardenability.
[0010] Function of Al: Aluminum is added to steel as a deoxidizer or alloying element. Its deoxidizing ability is much stronger than that of silicon and manganese. The main function of aluminum in steel is to refine the grains and fix the nitrogen in the steel, thereby significantly improving the impact toughness of the steel and reducing the cold brittleness tendency and aging tendency. The presence of Al in chromium-molybdenum steel and chromium steel can increase its wear resistance. The presence of Al in high-carbon tool steel can cause quenching brittleness.
[0011] The grain size of the steel used for the track pin bushing is ≥ grade 5, the hardness of the steel is ≤217HBW, the total decarburization layer depth (ferrite + transition layer) on each side of the steel is not more than 1.5% of the diameter, and the hairline is inspected using a tower-shaped specimen. The total number of hairline cracks is not more than 5, the maximum length of a single crack is 3mm, and the total length of the hairline is not more than 10mm.
[0012] The present invention also provides a method for preparing steel for track pin bushings, the method comprising electric furnace smelting, rolling into bars, magnetic particle flaw detection and other processes, wherein: 1) Electric furnace smelting: the smelting process produces foam slag, uniform decarburization, and reduces nitrogen absorption. The steel tapping conditions are: the end point C ≥ 0.07%, P ≤ 0.015%, and the residual element content meets the standard requirements; the steel tapping temperature is 1620-1680°C. 2) Rolling: billet shape Preheating section 500~950℃, heating section 1 950~1150℃, heating section 2 1150~1250℃, soaking section 1200~1240℃, allowable temperature difference ≤30℃, total heating time 4.25~5.25h. 3) Magnetic particle inspection: The size of the steel for the pin sleeve is The magnetic field strength is 250-350A / 25mm; the magnetizing current uses alternating current, and the duration of each magnetizing current is generally not less than 0.5S; the magnetic suspension must be stirred evenly, and the sample must be clamped between the two magnetizing chucks of the magnetic particle testing equipment to ensure good contact at both ends to prevent loosening.
[0013] The steel type of the present application further improves the surface hardness of the steel by adding Cr, Mn, Ti and a small amount of Al elements to low carbon steel, while taking into account the characteristics of the steel such as wear resistance and fatigue strength.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] 1) The present invention uses the above-mentioned reasonable component design, smelting, rolling, flaw detection process and other simple operation processes to make the grain size of low-carbon track pin bushing steel ≥5 levels, the steel hardness ≤217HBW, the total decarburization layer depth (ferrite + transition layer) of each side of the steel not more than 1.5% of the diameter, and the tower-shaped test specimen is used to test the hairline, the total number of hairline is not more than 5, the maximum length of a single hairline is 3mm, and the total length of the hairline is not more than 10mm. The steel prepared by the present invention has the characteristics of high hardness, wear resistance, fatigue resistance, good processability, etc., so that the track pin bushing steel can serve for a longer time in a very harsh working environment of engineering machinery.
[0016] 2) The preparation method of the present invention stipulates the steel-making conditions and requirements of electric furnace smelting, as well as the rolled ingot specifications and rolling process parameters, and magnetic particle flaw detection process parameters, etc., which provide guarantees for the subsequent hardness, wear resistance, fatigue resistance, machinability and other characteristics of the steel.
[0017] 3) The steel type of the present invention is well adapted to the needs of engineering machinery used in harsh environments, and provides technical support for the development of engineering machinery pin sleeve steel with good mechanical properties, wear resistance, fatigue resistance and machinability. DETAILED DESCRIPTION
[0018] The following lists three types of track pin sleeve steels produced by the production process of the present invention, namely Examples 1, 2 and 3. The chemical composition ratios of the track pin sleeve steels obtained in the three examples are shown in Table 1, the specific production processes are shown in Table 2, and the actual properties are shown in Tables 3 and 4.
[0019] Examples 1-3
[0020] A method for producing track pin sleeve steel comprises the following steps:
[0021] 1) Electric furnace smelting: The smelting process produces good foam slag, uniform decarburization, and reduces nitrogen absorption. The steel-making conditions are: end point C: 0.15-0.18%, P: 0.014-0.015%, and the steel-making temperature is 1638-1641°C.
[0022] 2) Rolling: Billet Shape Preheating section 726 ~ 731 ℃, heating section 1 1050 ~ 1063 ℃, heating section 2 1170 ~ 1178 ℃, equalizing section 1180 ~ 1190 ℃, total heating time 4.5 ~ 4.7h.
[0023] 3) Magnetic particle inspection: The size of the steel for the pin sleeve described in claim 3 is The magnetic field strength is 285-310A / 25mm; the magnetizing current uses alternating current, and the duration of each magnetizing current is 0.9-1.3S; the magnetic suspension must be stirred evenly, and the sample is clamped between the two magnetizing chucks of the magnetic particle testing equipment to ensure good contact between the two ends to prevent loosening;
[0024] Table 1 Chemical composition of round steel of Example 1-3
[0025]
[0026]
[0027] Table 2 Electric furnace smelting process, rolling process and magnetic particle flaw detection process of round steel in Example 1-3
[0028]
[0029] Table 3 Grain size, hardness, decarburization depth and cracking of round steel of Example 1-3
[0030]
[0031] In summary, the specifications of the track pin sleeve steel obtained by the present invention are The grain size reaches level 6 to 7, the hardness is 200 to 210 HBW, the depth of decarburization layer is 1.62 to 1.75 mm, the total number of hairline is 2 to 3, the maximum length of a single hairline is 3 mm, and the total length of hairline is 5 to 8 mm.
[0032] The process parameters (such as temperature, time, etc.) of the present invention can realize the method by taking upper and lower limits and interval values, and the embodiments are not listed one by one here.
[0033] Any contents not described in detail in the present invention can be based on the conventional technical knowledge in the art.
[0034] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit and scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.
Claims
1. A low-carbon track pin bushing steel, characterized in that: The chemical composition of the low-carbon track pin bushing steel includes, by mass percentage, C: 0.17-0.23%, Si: 0.17-0.37%, Mn: 0.80-1.10%, Cr: 1.00-1.30%, Ti: 0.04-0.10%, Cu≤0.20%, Al: 0.03-0.05%, P≤0.020%, S≤0.030%, O≤20×10 -4 %,H≤2×10 -4 %, the rest are Fe and other inevitable impurity elements, among which, 0.021C+0.025Si+0.017Mn+0.038Cr <Ti+Al<0.042C+0.051Si+0.038Mn+0.081Cr; The specifications of the obtained track pin bushing steel are φ160-180mm, the grain size reaches 6-7 levels, the hardness is 200-210HBW, the decarburization layer depth is 1.62-1.75mm, the total number of hairline is 2-3, the maximum length of a single hairline is 3mm, and the total length of hairline is 5-8mm; The method for preparing the low-carbon track pin bushing steel comprises the following steps: 1) Electric furnace smelting: During the smelting process, foamy slag is made, carbon is evenly decarburized, and nitrogen absorption is reduced. The tapping conditions are: end point C: 0.15-0.18%, P: 0.014-0.015%, tapping temperature: 1638-1641°C; 2) Rolling: Billet φ650mm, preheating section 726 ~ 731 ℃, heating section 1 1050 ~ 1063 ℃, heating section 2 1170 ~ 1178 ℃, soaking section 1180 ~ 1190 ℃, total heating time 4.5 ~ 4.7h; 3) Magnetic particle inspection: The size of the low-carbon track pin bushing steel is φ120~310mm, and the magnetic field strength is 250~350A / 25mm; the magnetizing current adopts alternating current, and the duration of each magnetizing current is 0.9~1.3S; By adding Cr, Mn, Ti and a small amount of Al elements to low carbon steel, the surface hardness of the steel is further improved while taking into account the wear resistance and fatigue strength of the steel.
2. The low carbon track pin bushing steel according to claim 1, characterized in that: The chemical composition of the low-carbon track pin sleeve steel includes, by mass percentage, C: 0.18-0.23%, Si: 0.18-0.35%, Mn: 0.90-1.00%, Cr: 1.10-1.30%, Ti: 0.05-0.09%, Cu≤0.20%, Al: 0.03-0.05%, P≤0.020%, S≤0.030%, O≤20×10 -4 %,H≤2×10 -4 %, and the rest are Fe and other inevitable impurity elements.
Citation Information
Patent Citations
Steel for caterpillar type engineering machinery caterpillar link pin bushes and production method thereof
CN102605266B
Low-cost high-end pin sleeve steel and its production method
CN107739977B
Track pin steel with improved hardenability using Cr and B elements and its production method
CN109112253B
Steel for pin shaft of wind power gear box and preparation method of steel
CN112410689A
Steel for hydraulic piece and manufacturing method for steel
CN102517522A