Preparation method and application of iodine ion surface modified titanium dioxide photocatalytic material
By depositing iodine ions on the surface of titanium dioxide, activate CO2 and implementing its hydrogenation reaction, the problem that existing photocatalytic materials cannot effectively reduce CO2 as a high value-added product is solved, the efficiency of CO2 conversion to CH4 and C2H4 is improved, and carbon is achieved Recycling of basic energy.
Patent Information
- Application Number
- CN202210967909.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-08-12
AI Technical Summary
Existing photocatalytic materials cannot effectively reduce CO2 to high added value C-H products, and can only be reduced to CO, and the study of Lewis alkaline sites has not yet been developed.
By depositing iodine ions on the surface of titanium dioxide, CO2 is activated by selective deposition method to achieve hydrogenation reaction of CO2, and high added value C-H products, such as CH4 and C2H4.
The reduction selectivity and generation amount of CO2 are improved, and the efficient catalysis of CO2 conversion to CH4 and C2H4 is achieved, which solves the shortage of existing photocatalytic materials that can only be reduced to CO, and realizes the recycling of carbon-based energy.
Smart Images

Figure CN115282990B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a photocatalytic material. Background Art
[0002] At present, the active sites on the catalyst surface are concentrated in the construction of three sites: metal, metal cation and non-metal vacancy. By interacting with CO2 and transferring electrons to CO2, the CO2 molecule is activated and combined with H dissociated on the surface to obtain CH products. After summarizing and thinking about the literature on CO2 reduction, considering the high electron density of Lewis base sites relative to metal or metal cation sites, CO2 can be directed towards CH products. However, the research on Lewis base sites is still blank. Summary of the invention
[0003] The purpose of the present invention is to solve the problem that the existing Lewis base site research is still blank, CO2 cannot be converted to CH products, and most photocatalytic materials can only reduce CO2 to CO, and to provide a preparation method and application of iodine ion surface modified titanium dioxide photocatalytic material.
[0004] A method for preparing an iodine ion surface-modified titanium dioxide photocatalytic material is completed by the following steps:
[0005] 1. Preparation of TiO2:
[0006] ①, add HF acid dropwise into tetrabutyl titanate, stir, and obtain a mixture;
[0007] ②, transferring the mixture to a reactor lined with polytetrafluoroethylene, and then hydrothermally reacting it at 160°C to 200°C to obtain a reaction product I; washing the reaction product I, and then drying it to obtain TiO2;
[0008] 2. I - Surface modified TiO2:
[0009] First, TiO2 and NaIO3 are added into deionized water, and then stirred in the dark, and then irradiated under a xenon lamp to obtain a reaction product II; the reaction product II is washed and then dried to obtain an iodine ion surface-modified titanium dioxide photocatalytic material.
[0010] An iodide ion surface modified titanium dioxide photocatalytic material is used for photocatalytic reduction of CO2.
[0011] Principle of the present invention:
[0012] The present invention selectively deposits halogen ions, especially I -Ions are deposited on the TiO2 surface, activating CO2 molecules and causing them to undergo hydrogenation reactions to obtain CH products, thereby achieving the recycling of carbon-based energy.
[0013] Advantages of the present invention:
[0014] 1. The present invention is the first to use Lewis base active sites to catalyze CO2 reduction hydrogenation, which can transform the original weak reduction of CO2 to CO by TiO2 into a hydrogenation pathway with higher CH4 selectivity and production, so that CO2 is converted into CH substances with higher added value, among which CH4 is an important fuel and C2H4 is an important chemical raw material, which solves the problem that most current photocatalytic materials can only reduce CO2 to CO;
[0015] 2. I - After surface modification, the TiO2 sample can change from weak photocatalytic reduction of CO2 to significant photocatalytic reduction of CO2. - Surface modification can change the TiO2 photocatalytic CO2 reduction process from generating only CO to generating CO and CH products, with CH4 as the main product and a selectivity of up to 65%. At the same time, it is also accompanied by the generation of the more difficult reduction product C2H4; innovative development has been carried out in terms of performance and catalytic mechanism;
[0016] 3. I prepared by the present invention - After the surface-modified TiO2 photocatalytic material catalyzed the reduction of CO2, the yields of CO, CH4 and C2H4 could reach 3.16 μmol·g -1 ·h -1 , 13.83 μmol·g -1 ·h -1 and 4.39 μmol·g -1 ·h -1 , thereby realizing the recycling of carbon-based energy.
[0017] The invention can obtain an iodine ion surface modified titanium dioxide photocatalytic material. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 XRD diagram, in which 1 is TiO2 prepared in step 1 ② of Example 1, and 2 is TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0019] Figure 2is a Raman spectrum diagram, in which 1 is TiO2 prepared in step 1② of Example 1, and 2 is I prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0020] Figure 3 TEM images and element distribution diagrams, (a) and (b) are I prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, (c) is the TEM image of TiO2 prepared in step 1② of Example 1, (d) is the TEM image of TiO2 prepared in step 2 of Example 1 - Element distribution map of surface modified TiO2 photocatalytic materials;
[0021] Figure 4 I prepared in step 2 of Example 1 - XPS graph of surface modified TiO2 photocatalytic material, where (a) is Ti2p, (b) is O1s, and (c) is I 3d;
[0022] Figure 5 TiO2 and I - Performance diagram of the yield of CO, CH4 and C2H4 produced by photocatalytic reduction of CO2 by surface-modified TiO2 photocatalytic materials, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0023] Figure 6 TiO2 and I - Performance diagram of the photocatalytic reduction of CO2 to generate CO by surface-modified TiO2 photocatalytic material, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0024] Figure 7 TiO2 and I -Performance diagram of the production of CH4 by photocatalytic reduction of CO2 by surface-modified TiO2 photocatalytic materials, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0025] Figure 8 TiO2 and I - Performance diagram of the photocatalytic reduction of CO2 to C2H4 by surface-modified TiO2 photocatalytic material, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials. DETAILED DESCRIPTION
[0026] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.
[0027] Specific implementation method 1: In this implementation method, a preparation method of an iodine ion surface modified titanium dioxide photocatalytic material is completed by the following steps:
[0028] 1. Preparation of TiO2:
[0029] ①, add HF acid dropwise into tetrabutyl titanate, stir, and obtain a mixture;
[0030] ②, transferring the mixture to a reactor lined with polytetrafluoroethylene, and then hydrothermally reacting it at 160°C to 200°C to obtain a reaction product I; washing the reaction product I, and then drying it to obtain TiO2;
[0031] 2. I - Surface modified TiO2:
[0032] First, TiO2 and NaIO3 are added into deionized water, and then stirred in the dark, and then irradiated under a xenon lamp to obtain a reaction product II; the reaction product II is washed and then dried to obtain an iodine ion surface-modified titanium dioxide photocatalytic material.
[0033] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the mass fraction of the HF acid in step 1 is 35% to 45%; the volume ratio of the HF acid to tetrabutyl titanate in step 1 is (1 to 2): (5 to 15). The other steps are the same as those in specific implementation method 1.
[0034] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the stirring time in step 1 is 20 minutes to 40 minutes. The other steps are the same as those in specific implementation method 1 or 2.
[0035] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the time of the hydrothermal reaction in step 1② is 12h to 24h. The other steps are the same as those of specific embodiments 1 to 3.
[0036] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: in step 1 ②, the reaction product I is first washed with deionized water for 3 to 5 times, and then washed with anhydrous ethanol for 3 to 5 times; the drying temperature in step 1 ② is 60°C to 80°C, and the drying time is 6h to 12h. The other steps are the same as those in specific embodiments 1 to 4.
[0037] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: in step 1②, the mixture is transferred to a reactor lined with polytetrafluoroethylene, and then hydrothermally reacted at 180°C to obtain reaction product I; the reaction product I is washed and then dried to obtain TiO2. The other steps are the same as those of specific embodiments 1 to 5.
[0038] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the mass ratio of TiO2 to NaIO3 in step 2 is (0.1-0.5):(0.5-3); the mass ratio of TiO2 to deionized water in step 2 is (0.1g-0.5g):(50mL-60mL). The other steps are the same as those in specific embodiments 1 to 6.
[0039] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: in step two, the reaction product II is first washed 3 to 5 times with deionized water, and then washed 3 to 5 times with anhydrous ethanol; the drying temperature in step two is 60°C to 80°C, and the drying time is 6h to 12h. The other steps are the same as those of specific embodiments one to seven.
[0040] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the stirring time in the dark in step 2 is 10 to 20 minutes, and the irradiation time under the xenon lamp in step 2 is 1 to 3 hours. The other steps are the same as those in specific embodiments 1 to 8.
[0041] Specific embodiment ten: This embodiment is an iodine ion surface modified titanium dioxide photocatalytic material for photocatalytic reduction of CO2.
[0042] The following examples are used to verify the beneficial effects of the present invention:
[0043] Embodiment 1: a kind of - The preparation method of the surface modified TiO2 photocatalytic material is completed according to the following steps:
[0044] 1. Preparation of TiO2:
[0045] ①, add 1.2 mL of HF acid dropwise into 10 mL of tetrabutyl titanate, stir for 30 min, and obtain a mixture;
[0046] The mass fraction of HF acid described in step 1 is 40%;
[0047] ②, transfer the mixture to a polytetrafluoroethylene-lined reactor, and then perform a hydrothermal reaction at 180°C for 24 hours to obtain a reaction product I; wash the reaction product I three times with deionized water, and then wash the reaction product I three times with anhydrous ethanol; and then dry at 60°C for 12 hours to obtain TiO2;
[0048] 2. I - Surface modified TiO2:
[0049] First, 0.2 g TiO2 and 1.2 g NaIO3 were added to 60 mL deionized water, and then stirred for 10 min in the dark, and then irradiated under a xenon lamp for 2 h to obtain reaction product II; the reaction product II was washed 3 times with deionized water, and then washed 3 times with anhydrous ethanol, and then dried at 60 ° C for 12 h to obtain I - Surface modified TiO2 photocatalytic material (I-TiO2).
[0050] Example 2: The difference between this example and Example 1 is that in step 2, 0.2 g TiO2 and 1.6 g NaIO3 are first added to 60 mL deionized water, then stirred for 10 min in the dark, and then irradiated under a xenon lamp for 2 h to obtain reaction product II. The other steps and parameters are the same as those in Example 1.
[0051] Example 3: The difference between this example and Example 1 is that in step 2, 0.2 g TiO2 and 1.8 g NaIO3 are first added to 60 mL deionized water, then stirred for 10 min in the dark, and then irradiated under a xenon lamp for 2 h to obtain reaction product II. The other steps and parameters are the same as those in Example 1.
[0052] Figure 1 XRD diagram, in which 1 is TiO2 prepared in step 1 ② of Example 1, and 2 is TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0053] Figure 2 is a Raman spectrum diagram, in which 1 is TiO2 prepared in step 1② of Example 1, and 2 is I prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0054] from Figure 1 and Figure 2 It can be seen that the TiO2 prepared in step 1② of Example 1 is anatase phase. From two different tests, it can be seen that the TiO2 prepared in step 2 of Examples 1 to 3 is anatase phase. - The XRD diffraction peaks and Raman peaks of the surface-modified TiO2 photocatalytic material did not change in half-peak width and peak position, indicating that - It was not doped into the sample but existed on the TiO2 surface in the form of ions, indicating that the Lewis base site was successfully constructed.
[0055] Figure 3 TEM images and element distribution diagrams, (a) and (b) are I prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, (c) is the TEM image of TiO2 prepared in step 1② of Example 1, (d) is the TEM image of TiO2 prepared in step 2 of Example 1 - Element distribution map of surface modified TiO2 photocatalytic materials;
[0056] from Figure 3It can be seen that the synthesized samples are all nanosheets with a thickness of about 5 nm, and the Lewis base site construction does not change the morphology and size of TiO2. Mapping tests show that Ti, O and I elements are evenly distributed, among which the I element content is relatively low and not aggregated, indicating that the Lewis base site is successfully constructed uniformly and monodispersely.
[0057] Figure 4 I prepared in step 2 of Example 1 - XPS graph of surface modified TiO2 photocatalytic material, where (a) is Ti2p, (b) is O1s, and (c) is I 3d;
[0058] Figure 4 Used to observe samples to show the chemical state of elements; Figure 4 (a) indicates that Ti is tetravalent. Figure 4 (b) shows that the surface oxygen of the sample has two forms, namely lattice oxygen and surface hydroxyl. Compared with TiO2, the surface hydroxyl content in I-TiO2 is reduced, indicating that I - Replaced a portion of the surface hydroxyl groups; Figure 4 (c) shows that there is -1 valence I element on the sample surface, further indicating that the Lewis base site is successfully constructed.
[0059] Photocatalytic reduction of CO2 experiment:
[0060] The photocatalytic reduction of CO2 was carried out in a gas-solid reaction device; CO2 and saturated water vapor were introduced into the reactor, and no additional sacrificial agent or precious metal co-catalyst was added during the reaction. The light source used was a 300W xenon lamp (PLS-SXE300, AM1.5G); the gas phase products (CO, CH4, C2H4) were analyzed using a gas chromatograph with a TCD detector.
[0061] Figure 5 TiO2 and I - Performance diagram of the yield of CO, CH4 and C2H4 produced by photocatalytic reduction of CO2 by surface-modified TiO2 photocatalytic materials, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0062] from Figure 5 It can be seen that unmodified TiO2 has almost no CO2 photoreduction performance. - After surface modification, CO2 is photoreduced to CO, CH4 and C2H4; wherein, the I prepared in step 2 of Example 2- The surface modified TiO2 photocatalytic material has the best performance. After photocatalytic reduction of CO2, the yields of CO, CH4 and C2H4 can reach 3.16 μmol·g -1 ·h -1 , 13.83 μmol·g -1 ·h -1 and 4.39 μmol·g -1 ·h -1 .
[0063] Figure 6 TiO2 and I - Performance diagram of the photocatalytic reduction of CO2 to generate CO by surface-modified TiO2 photocatalytic material, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0064] from Figure 6 It can be seen that unmodified TiO2 can only photoreduced CO2 to negligible CO. The I prepared in step 2 of Example 2 - After the surface modified TiO2 photocatalytic material photocatalyzed the reduction of CO2, the CO production was stabilized at 3.16 μmol in one hour, while the I prepared in step 2 of Example 1 and Example 3 - After the surface modified TiO2 photocatalytic material photocatalyzed the reduction of CO2, the CO production increased slightly with time, and the production was 4.92μmol and 4.71μmol after 4 hours, respectively.
[0065] Figure 7 TiO2 and I - Performance diagram of the production of CH4 by photocatalytic reduction of CO2 by surface-modified TiO2 photocatalytic materials, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials;
[0066] from Figure 7 It can be seen that no CH4 product is generated in the unmodified TiO2, while the CH4 production of the I-surface-modified TiO2 gradually increases with time. -After the surface modified TiO2 photocatalytic material photocatalyzed the reduction of CO2, the CH4 production increased rapidly, while the I prepared in step 2 of Example 1 and Example 3 - After the surface modified TiO2 photocatalytic material photocatalyzed the reduction of CO2, the CH4 production increased slowly. After 4 hours, the I prepared in step 2 of Example 2 - The surface modified TiO2 photocatalytic material has the best performance in photocatalytic reduction of CO2, with a CH4 yield of 26.92 μmol; I prepared in step 2 of Example 1 and Example 3 - After the surface modified TiO2 photocatalytic material photocatalyzed the reduction of CO2, the CH4 production was 12.46μmol and 13.55μmol respectively.
[0067] Figure 8 TiO2 and I - Performance diagram of the photocatalytic reduction of CO2 to C2H4 by surface-modified TiO2 photocatalytic material, in which 1 is the TiO2 prepared in step 1② of Example 1, and 2 is the TiO2 prepared in step 2 of Example 1 - Surface modified TiO2 photocatalytic material, 3 is the I prepared in step 2 of Example 2 - Surface modified TiO2 photocatalytic material, 4 is the I prepared in step 2 of Example 3 - Surface modified TiO2 photocatalytic materials.
[0068] from Figure 8 It can be seen that unmodified TiO2 cannot photoreduced CO2 to C2H4; - The surface-modified TiO2 can continuously photoreduced CO2 to C2H4; among them, the I prepared in step 2 of Example 2 - The surface modified TiO2 photocatalytic material has the best performance. After photocatalytic reduction of CO2, the increase rate of C2H4 production is faster than that of the I prepared in step 2 of Example 1 and Example 3. - Surface modified TiO2 photocatalytic material, prepared in step 2 of Example 2 - After the surface modified TiO2 photocatalytic material was illuminated for 4 hours, the C2H4 production reached 8.92 μmol; I prepared in step 2 of Example 1 and Example 3 - After 4 hours of illumination, the C2H4 production of the surface-modified TiO2 photocatalytic material was 4.13 μmol and 4.52 μmol respectively.
[0069] In summary, the TiO2 sample can only convert a trace amount of CO2 into CO. However, after the Lewis base site was constructed, the I-TiO2 sample showed a higher CO2 photoreduction conversion efficiency. In addition, the Lewis base construction also changed the CO2 photoreduction process, from CO to CH compounds with more added value, including CH4 and C2H4, which is more difficult to produce, among which CH4 has a higher selectivity. From the time evolution experiment, it can be seen that the generation of CO gradually slows down with time, while the generation of CH4 and C2H4 gradually increases with time, indicating that CH compounds are further conversions of CO intermediates, which intuitively shows that Lewis has changed the reduction process of CO2 while improving the CO2 conversion efficiency.
Claims
1. A method for preparing an iodine ion surface-modified titanium dioxide photocatalytic material, characterized in that The preparation method is to prepare an iodine ion surface-modified titanium dioxide photocatalytic material for photocatalytic reduction of CO2 to generate CO, CH4 and C2H4, and the preparation method is completed according to the following steps:
1. Preparation of TiO2: ①, add HF acid dropwise into tetrabutyl titanate, stir, and obtain a mixture; ②, transferring the mixture to a reactor lined with polytetrafluoroethylene, and then hydrothermally reacting at 160°C to 200°C to obtain reaction product I; The reaction product I is washed and dried to obtain TiO2; 2. I - Surface modified TiO2: First, TiO2 and NaIO3 are added into deionized water, and then stirred in the dark, and then irradiated under a xenon lamp to obtain reaction product II; The reaction product II is washed and dried to obtain a titanium dioxide photocatalytic material with an iodine ion surface modified; The mass ratio of TiO2 to NaIO3 described in step 2 is 0.2:1.6; The volume ratio of the mass of TiO2 described in step 2 to deionized water is (0.1g~0.5g):(50mL~60mL); the stirring time in dark conditions in step 2 is 10min~20min; the irradiation time under a xenon lamp in step 2 is 1h~3h.
2. The method for preparing a titanium dioxide photocatalytic material surface modified with iodine ions according to claim 1, characterized in that The mass fraction of the HF acid described in step one is 35% to 45%; the volume ratio of the HF acid described in step one to tetrabutyl titanate is (1 to 2): (5 to 15).
3. The method for preparing a titanium dioxide photocatalytic material surface modified with iodine ions according to claim 1, characterized in that The stirring time in step 1 is 20 min to 40 min.
4. The method for preparing a titanium dioxide photocatalytic material with iodine ion surface modification according to claim 1, characterized in that The time of the hydrothermal reaction described in step 1② is 12h to 24h.
5. The method for preparing a titanium dioxide photocatalytic material surface modified with iodine ions according to claim 1, characterized in that In step 1②, the reaction product I is first washed with deionized water for 3 to 5 times, and then washed with anhydrous ethanol for 3 to 5 times; the drying temperature in step 1② is 60°C to 80°C, and the drying time is 6h to 12h.
6. The method for preparing a titanium dioxide photocatalytic material surface modified with iodine ions according to claim 1, characterized in that In step 1②, the mixture is transferred to a polytetrafluoroethylene-lined reactor, and then subjected to a hydrothermal reaction at 180°C to obtain a reaction product I; the reaction product I is washed and then dried to obtain TiO2.
7. The method for preparing a titanium dioxide photocatalytic material surface modified with iodine ions according to claim 1, characterized in that In step 2, the reaction product II is first washed with deionized water for 3 to 5 times, and then washed with anhydrous ethanol for 3 to 5 times; the drying temperature in step 2 is 60° C. to 80° C., and the drying time is 6 h to 12 h.