A low-temperature rapid discharge plasma diffusion connection method for zirconium and its alloys
Through the low-temperature rapid discharge plasma diffusion connection technology, the problems of high welding temperature and long insulation time of zirconium alloy are solved, efficient and reliable connection of zirconium is achieved, and joint performance is improved, and it is suitable for nuclear industry applications.
Patent Information
- Application Number
- CN202211038680.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-29
AI Technical Summary
In the existing zirconium and its alloy connection technology, high welding temperature and long insulation time lead to attenuation of joint performance, and zirconium alloy undergoes lattice transformation at high temperatures, reducing neutron irradiation performance and increasing the risk of nuclear fuel deoxygenation.
Using low-temperature rapid discharge plasma diffusion connection technology, the rapid connection of zirconium and its alloys can be achieved at low temperatures through electric field induced Joule heat and electric field effect. Two assembly methods are used for graphite molds or no molds, which reduces welding temperature and insulation time and reduces joints. Deformation and residual stress.
It realizes fast and seamless connection of zirconium at low temperatures, improves the strength and service reliability of the joints, avoids the problems of zirconium allogeneic transformation and nuclear fuel deoxygenation at high temperatures, and is suitable for the manufacturing of high-performance nuclear fuel zirconium clad components.
Smart Images

Figure CN115283807B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal material connection, and in particular relates to a low-temperature rapid discharge plasma diffusion connection method for zirconium and its alloys. Background Art
[0002] Zirconium and its alloys are widely used as nuclear fuel cladding tube materials due to their excellent corrosion resistance, neutron irradiation resistance and good processing characteristics, and are known as the "first metal of the atomic age". In the industrial application process of zirconium, the connection and assembly of large and complex structural parts are essential, which makes reliable connection technology a key requirement. Various welding technologies are used in the connection process of zirconium. Common fusion welding technologies (TIG, electron beam and laser welding, etc.) cause joint performance degradation (mechanical strength, corrosion resistance) due to high welding temperatures. Existing pressure welding technologies (resistance welding, friction welding and hot pressing diffusion welding) have problems such as high welding temperature, long insulation time, large weld deformation and high residual stress of the joint. At the same time, the connection temperature of the above welding technologies (except hot pressing) is higher than the melting point of zirconium (1852℃), which will cause zirconium alloy ignition and nuclear fuel deoxidation in the controlled area. At the same time, zirconium and its alloys will undergo lattice transformation at around 850℃, from the α phase with low neutron absorption cross section to the β phase that is not resistant to neutron irradiation. Although hot pressing welding can reduce the connection temperature of zirconium to a certain extent (≥900℃), its insulation time is often too long (>3h). Therefore, in order to promote the safe, reliable and efficient nuclear industry application of zirconium and its alloys, the development of a new type of low-temperature rapid connection technology for zirconium cladding components is a key issue that needs to be solved urgently.
[0003] In view of the problems of high welding temperature and long insulation time in the existing zirconium connection technology, the present invention proposes to use discharge plasma technology to diffuse and connect zirconium, and utilizes the Joule heat and electric field effect generated by the electric field inside the sample to promote rapid connection of zirconium and its alloys at low temperature. Summary of the invention
[0004] When connecting zirconium with existing welding technologies (TIG, electron beam and resistance welding, etc.), there are technical problems such as high welding temperature, which weakens the joint performance and reduces the service reliability of the joint, and long insulation time, which hinders the efficient nuclear industry application of zirconium. The present invention proposes a low-temperature rapid discharge plasma diffusion connection method for zirconium and its alloys. The method can effectively reduce the welding temperature and insulation time, realize the seamless connection of zirconium homogeneous joints, and the deformation of the joint is small and the residual stress is low, thereby improving the strength of the joint and the service reliability, which is conducive to the manufacture of high-performance nuclear fuel zirconium cladding components.
[0005] The technical solution of the present invention is as follows:
[0006] A low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys, characterized in that it comprises the following steps:
[0007] 1) Preparation of parent material:
[0008] Industrial zirconium or zirconium alloy is used as the base material, and the surface to be welded is polished with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, and then the surface to be welded of the base material is polished with 1μm diamond suspension polishing liquid, and the surface stains are removed by ultrasonic cleaning, and then dried for use;
[0009] 2) Assembly:
[0010] There are two assembly methods, one is to use a graphite mold, and the other is not to use a graphite mold; both are assembled in the order of graphite indenter-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-graphite indenter;
[0011] 3) Discharge plasma diffusion welding connection:
[0012] The spark plasma diffusion bonding technology is used to perform low-temperature solid phase diffusion bonding on two zirconium base materials to be welded, and the welding processes of the two assembly methods are different.
[0013] Furthermore, in step 3), if a graphite mold is used in the assembly process, the welding process is:
[0014] Place the graphite mold in the sintering furnace chamber, insert the main temperature measuring thermocouple into the thermocouple temperature measuring hole of the graphite film cavity, and use the thermocouples equipped by the system to detect the temperature of the upper and lower pressure heads; adjust the connection pressure, turn on the vacuum pump to make the vacuum degree in the furnace meet the specified requirements, adjust the power required for the connection process, and then pass a DC pulse current to raise the temperature to the diffusion welding temperature, keep it warm for a certain period of time, and then carry out the welding operation.
[0015] Furthermore, in step 3), if no graphite mold is used in the assembly process, the welding process is:
[0016] Place the zirconium to be welded on the graphite foil of the lower pressure head, and then place another zirconium material to ensure that the two parts to be welded are in the same axial position, put the graphite foil into the upper pressure head, add appropriate pressure, and contact the main temperature measuring thermocouple with the interface of the zirconium to be connected. At the same time, the upper and lower pressure heads also use the thermocouples equipped by the system to detect the temperature, set the connection pressure, turn on the vacuum pump to make the vacuum degree in the furnace meet the specified requirements, set the system temperature control mode to manual, manually control the temperature during the welding process to ensure that the temperature continues to rise steadily, and perform discharge plasma diffusion connection. When the welding temperature is reached, keep warm for a certain period of time, then immediately close the welding furnace and cool it with the furnace.
[0017] Furthermore, in step 3), the connection pressure is 15-50MPa, preferably 30MPa; the heating rate is 80-120°C / min, preferably 100°C / min; the diffusion welding temperature is 600-900°C, preferably 600°C, and the holding time at the diffusion welding temperature is 0-30min, preferably 10min.
[0018] The technical effects achieved by the present invention are as follows:
[0019] 1) The present invention discloses a method for low-temperature rapid discharge plasma diffusion connection of zirconium and its alloys, which utilizes the Joule heat and electric field effect induced by the electric field inside the sample to realize rapid connection of materials at a relatively low temperature. By changing the assembly mode and increasing the current density flowing through the sample, the present invention significantly reduces the welding temperature (600°C) and the heat preservation time (0-10min) of zirconium, avoids the practical problems of the reduction of neutron irradiation performance of the joint, deoxidation of nuclear fuel and ignition of zirconium in the control area caused by zirconium allotropic transformation at high temperature, solves the problem that the joint obtained by the existing connection technology is difficult to meet the nuclear application of zirconium, and the obtained joint is well combined without obvious unconnected areas; at the same time, the connection technology does not use an intermediate layer, avoiding the problem that the introduction of the intermediate layer causes excessive residual stress in the joint and mismatch of the radiation swelling rate during service.
[0020] 2) The method of the present invention only adds appropriate pressure to the ends of the workpiece to be welded, and the resulting weld joint has small deformation and low residual stress, which solves the technical problem of large deformation of the joint obtained by common pressure welding (friction stir welding, resistance welding) technology.
[0021] 3) The present invention has a short heat preservation time and is simple and safe to operate. Therefore, the production efficiency is high and the degree of automation is high, which can be adapted to large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of two assembly modes of the present invention;
[0023] Figure 2 is a temperature and pressure parameter diagram under typical welding conditions of the present invention;
[0024] Figure 2 Figures a and b are the welding temperature and pressure parameter diagrams of 900°C, 10 min when using a graphite mold and 600°C, 10 min when not using a graphite mold;
[0025] Figure 3 When the graphite mold is used for the present invention, a connection pressure of 30 MPa is adopted and the SEM image of the Zr / Zr joint obtained at 900° C. for 10 min is obtained (Example 1);
[0026] Figure 3a and b represent the SEM images of the edge area and the center area of the welded joint when the temperature was kept at 900°C for 10 min (Example 1);
[0027] Figure 4 When the graphite mold is used for the present invention, a connection pressure of 30 MPa is adopted and the SEM image of the Zr / Zr joint obtained at 800° C. for 10 min is obtained (Example 2);
[0028] Figure 4 a and b represent the SEM images of the edge area and the center area of the welded joint when the temperature was kept at 800°C for 10 min (Example 2);
[0029] Figure 5 When the graphite mold is used for the present invention, a connection pressure of 30 MPa is adopted and the SEM image of the Zr / Zr joint obtained at 700° C. for 10 min is obtained (Example 3);
[0030] Figure 5 a and b represent the SEM images of the edge area and the center area of the welded joint when the temperature was kept at 700°C for 10 min (Example 3);
[0031] Figure 6 When the graphite mold is used for the present invention, a connection pressure of 30 MPa is adopted and the SEM image of the Zr / Zr joint obtained at 600° C. for 10 min is obtained (Example 4);
[0032] Figure 6 a and b represent the SEM images of the edge area and the center area of the welded joint when the temperature was kept at 600°C for 10 min (Example 4);
[0033] Figure 7 The SEM image of the Zr / Zr joint obtained by the present invention without using a graphite mold and using a connection pressure of 30 MPa and keeping at 600° C. for 10 min (Example 5);
[0034] Figure 7 a and b represent the SEM images of the edge area and the center area of the welded joint when the temperature was kept at 600°C for 10 min (Example 5);
[0035] Figure 8 When the graphite mold is not used in the present invention, a connection pressure of 30 MPa is used and the SEM image of the Zr / Zr joint obtained at 600° C. for 1 s is obtained (Example 6);
[0036] Figure 8 a and b represent the SEM images of the edge and center areas of the welded joint at 600°C for 1 s (Example 6);
[0037] Fig. 9 XRD diagrams of the base material and the joint obtained under typical welding conditions (900°C, 10 min with graphite die and 600°C, 10 min without graphite die) in the present invention;
[0038] Fig.10 A typical fracture diagram of a joint obtained in the present invention is shown;
[0039] Fig.10 ab represents the fracture morphology when the shear strength of the joint is higher than 303 MPa, and cd represents the fracture morphology when the shear strength of the joint is lower than 303 MPa. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0041] Embodiment 1:
[0042] In this embodiment, a low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys is as follows:
[0043] 1) Preparation of parent material
[0044] The method for low-temperature rapid discharge plasma diffusion bonding of zirconium and its alloys adopts a Zr702 cylinder with a size of Φ20mm and a height of 5mm, and grinds the surface to be welded with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, then polishes the surface to be welded of the parent material with a 1μm diamond suspension polishing liquid, removes surface stains with ultrasonic cleaning, and gently wipes with alcohol cotton to dry for use.
[0045] 2) Assembly
[0046] The zirconium base material to be welded is assembled into the graphite mold in the order of graphite indenter-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-graphite indenter, and then the assembled mold is placed into the furnace cavity.
[0047] 3) Discharge plasma diffusion bonding
[0048] Place the graphite mold with the workpiece to be welded into the welding furnace cavity, fix the main temperature measuring thermocouple in the temperature measuring hole of the graphite mold cavity, and use another thermocouple equipped with the system to fix it in contact with the temperature measuring holes of the upper and lower graphite pressure heads for temperature monitoring, adjust the connection pressure to 30MPa, turn on the vacuum pump to make the vacuum degree in the furnace meet the requirements, and then pass a DC pulse current to increase the temperature to 900℃ at a heating rate of 100℃ / min, keep warm at 900℃ for 10min, and finally cool with the furnace. Vacuum is evacuated throughout the connection process, and discharge plasma diffusion welding is performed to finally obtain a zirconium joint.
[0049] Example 1 Figure 3 The SEM image of the obtained zirconium joint is shown, Figure 3 a is the edge area of the joint, showing that there are some unconnected areas in the joint. Figure 3 b shows that the middle area of the joint achieves seamless connection. The connection quality of the middle area of the joint is significantly higher than that of the edge area, mainly due to the difference in contact conditions between the two; Fig. 9 The XRD results of the joint show that there is no phase change of zirconium under the welding condition of assembling the graphite mold at 900℃; at the same time, the shear strength of the final zirconium joint was tested at room temperature, and the room temperature shear strength of the joint was 387.9±30.4MPa. Fig.10 The mixed fracture mode of ab also reflects the excellent performance of the joint.
[0050] Embodiment 2:
[0051] In this embodiment, a low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys is as follows:
[0052] 1) Preparation of parent material
[0053] The method for low-temperature rapid discharge plasma diffusion bonding of zirconium and its alloys adopts a Zr702 cylinder with a size of Φ20mm and a height of 5mm, and grinds the surface to be welded with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, then polishes the surface to be welded of the parent material with a 1μm diamond suspension polishing liquid, removes surface stains with ultrasonic cleaning, and gently wipes with alcohol cotton to dry for use.
[0054] 2) Assembly
[0055] The zirconium base material to be welded is assembled into the graphite mold in the order of graphite indenter-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-graphite indenter, and then the assembled mold is placed into the furnace cavity.
[0056] 3) Discharge plasma diffusion bonding
[0057] Place the graphite mold with the workpiece to be welded into the welding furnace cavity, fix the main temperature measuring thermocouple in the temperature measuring hole of the graphite mold cavity, and use another thermocouple equipped with the system to fix it in contact with the temperature measuring holes of the upper and lower graphite pressure heads for temperature monitoring, adjust the connection pressure to 30MPa, turn on the vacuum pump to make the vacuum degree in the furnace meet the requirements, then pass a DC pulse current to increase the temperature to 800℃ at a heating rate of 100℃ / min, keep warm at 800℃ for 10min, and finally cool with the furnace. Vacuum is evacuated throughout the connection process, and discharge plasma diffusion welding is performed to finally obtain a zirconium joint.
[0058] Example 2 Figure 4 The SEM image of the obtained zirconium joint is shown, Figure 4The edge region of the joint shows a Figure 4 b shows a poor connection state in the middle area of the joint; at the same time, the shear strength test of the final zirconium joint was carried out at room temperature. The room temperature shear strength of the joint was 302.1±84.59MPa. The typical failure modes of the joint are as follows Fig.10 cd shown.
[0059] Embodiment 3:
[0060] In this embodiment, a low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys is as follows:
[0061] 1) Preparation of parent material
[0062] The method for low-temperature rapid discharge plasma diffusion bonding of zirconium and its alloys adopts a Zr702 cylinder with a size of Φ20mm and a height of 5mm, and grinds the surface to be welded with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, then polishes the surface to be welded of the parent material with a 1μm diamond suspension polishing liquid, removes surface stains with ultrasonic cleaning, and dries for standby use.
[0063] 2) Assembly
[0064] The zirconium base material to be welded is assembled into the graphite mold in the order of graphite indenter-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-graphite indenter, and then the assembled mold is placed into the furnace cavity.
[0065] 3) Discharge plasma diffusion bonding
[0066] Place the graphite mold with the workpiece to be welded into the welding furnace cavity, fix the main temperature measuring thermocouple in the temperature measuring hole of the graphite mold cavity, and use another thermocouple equipped with the system to fix it in contact with the temperature measuring holes of the upper and lower graphite pressure heads for temperature monitoring, adjust the connection pressure to 30MPa, turn on the vacuum pump to make the vacuum degree in the furnace meet the requirements, then pass a DC pulse current to increase the temperature to 700℃ at a heating rate of 100℃ / min, keep warm at 700℃ for 10min, and finally cool with the furnace. Vacuum is evacuated throughout the connection process, and discharge plasma diffusion welding is performed to finally obtain a zirconium joint.
[0067] Example 3 Figure 5 The SEM image of the obtained zirconium joint is shown, Figure 5 The edge region of the joint shows a Figure 5 The connection state in the middle area of the joint of b is poor, and due to the decrease in connection temperature, Figure 5 b shows that there is also an unbonded interface in the middle area of the joint; at the same time, the shear strength of the final zirconium joint was tested at room temperature. The room temperature shear strength of the joint was 80.4±44.79MPa, and the fracture morphology was relatively smooth, similar to Fig.10 cd, showing a typical brittle fracture mode.
[0068] Embodiment 4:
[0069] In this embodiment, a low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys is as follows:
[0070] 1) Preparation of parent material
[0071] The method for low-temperature rapid discharge plasma diffusion bonding of zirconium and its alloys adopts a Zr702 cylinder with a size of Φ20mm and a height of 5mm, and grinds the surface to be welded with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, then polishes the surface to be welded of the parent material with a 1μm diamond suspension polishing liquid, removes surface stains with ultrasonic cleaning, and gently wipes with alcohol cotton to dry for use.
[0072] 2) Assembly
[0073] The zirconium base material to be welded is assembled into the graphite mold in the order of graphite indenter-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-graphite indenter, and then the assembled mold is placed into the furnace cavity.
[0074] 3) Discharge plasma diffusion bonding
[0075] Place the graphite mold with the workpiece to be welded into the welding furnace cavity, fix the main temperature measuring thermocouple in the temperature measuring hole of the graphite mold cavity, and use another thermocouple equipped with the system to fix it in contact with the temperature measuring holes of the upper and lower graphite pressure heads for temperature monitoring, adjust the connection pressure to 30MPa, turn on the vacuum pump to make the vacuum degree in the furnace meet the requirements, then pass a DC pulse current to increase the temperature to 600℃ at a heating rate of 100℃ / min, keep warm at 600℃ for 10min, and finally cool with the furnace. Vacuum is evacuated throughout the connection process, and discharge plasma diffusion welding is performed to finally obtain a zirconium joint.
[0076] Example 4 Figure 6 The SEM image of the obtained zirconium joint is shown, Figure 6 It shows that there are obvious unconnected areas in the middle and edge areas of the weld, indicating that the graphite mold assembly experiment at a low temperature of 600°C failed;
[0077] At the same time, the shear strength test of the final zirconium joint was carried out at room temperature, and the fracture form of the joint was similar to Fig.10 Brittle fracture mode of cd.
[0078] Embodiment 5:
[0079] In this embodiment, a low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys is as follows:
[0080] 1) Preparation of parent material
[0081] The method for low-temperature rapid discharge plasma diffusion bonding of zirconium and its alloys adopts a Zr702 cylinder with a size of Φ20mm and a height of 5mm, and grinds the surface to be welded with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, then polishes the surface to be welded of the parent material with a 1μm diamond suspension polishing liquid, removes surface stains with ultrasonic cleaning, and gently wipes with alcohol cotton to dry for use.
[0082] 2) Assembly
[0083] The zirconium base material to be welded is assembled in the order of graphite indenter-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-graphite indenter. Different from welding with graphite mold, the zirconium is directly placed on the graphite foil of the lower graphite indenter in the furnace chamber, the zirconium cylinder is kept coaxially placed, and the graphite paper foil and the upper graphite indenter are placed on the base material in sequence, and then the welding operation can be carried out.
[0084] 3) Discharge plasma diffusion bonding
[0085] Prepare the zirconium base material to be welded assembled in step 2) for discharge plasma diffusion connection, fix the main temperature measuring thermocouple in contact with the surfaces of the two zirconium to be connected, and use another thermocouple equipped with the system to fix it in contact with the upper and lower graphite pressure head temperature measuring holes for temperature monitoring, adjust the connection pressure to 30MPa, turn on the vacuum pump to make the vacuum degree in the sintering furnace reach the specified requirement, change the temperature control mode to manual temperature control, ensure that the temperature continues to rise steadily during the welding process, keep warm for 10 minutes when the zirconium connection temperature of 600°C is reached, then stop the welding operation immediately, cool with the furnace, and finally obtain the zirconium joint.
[0086] Example 5 Figure 7 The SEM image of the obtained zirconium joint is shown, Figure 7 a is the edge area of the joint showing the unconnected area due to poor contact. Figure 7 b shows that the middle area of the joint achieves seamless connection; Fig. 9 The XRD results show that there is no phase change of zirconium under this welding condition. At the same time, the shear strength of the final zirconium joint was tested at room temperature. The room temperature shear strength of the joint was 404.9±78.9MPa, reaching 80% of the shear strength of the parent material. The failure mode of the fracture is also similar to Fig.10 Mixed fracture of ab.
[0087] Embodiment 6:
[0088] In this embodiment, a low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys is as follows:
[0089] 1) Preparation of parent material
[0090] The method for low-temperature rapid discharge plasma diffusion bonding of zirconium and its alloys adopts a Zr702 cylinder with a size of Φ20mm and a height of 5mm, and grinds the surface to be welded with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, then polishes the surface to be welded of the parent material with a 1μm diamond suspension polishing liquid, removes surface stains with ultrasonic cleaning, and gently wipes with alcohol cotton to dry for use.
[0091] 2) Assembly
[0092] The zirconium base material to be welded is assembled in the order of graphite indenter-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-graphite indenter. Different from welding with graphite mold, the zirconium is directly placed on the graphite foil of the lower graphite indenter in the furnace chamber, the zirconium cylinder is kept coaxially placed, and the graphite paper foil and the upper graphite indenter are placed on the base material in sequence, and then the welding operation can be carried out.
[0093] 3) Discharge plasma diffusion bonding
[0094] Prepare the zirconium base material to be welded assembled in step 2) for discharge plasma diffusion connection, fix the main temperature measuring thermocouple in contact with the surfaces of the two zirconium pieces to be connected, and use another thermocouple equipped with the system to fix it in contact with the temperature measuring hole of the upper graphite pressure head for temperature monitoring, adjust the connection pressure to 30MPa, turn on the vacuum pump to make the vacuum degree in the sintering furnace reach the specified requirement, change the temperature control mode to manual temperature control, ensure that the temperature continues to rise steadily during the welding process, stop the welding operation immediately when the zirconium connection temperature of 600°C is reached, cool with the furnace, and finally obtain the zirconium joint.
[0095] Example 6 Figure 8 The SEM image of the obtained zirconium joint is shown, Figure 8 a is the edge area of the joint, showing that there is an obvious unconnected area in the joint. Figure 8 b shows that the middle area of the joint is seamlessly connected; at the same time, the shear strength of the final zirconium joint is tested at room temperature. The room temperature shear strength of the joint is 154.09±84.75MPa, and the fracture mode is similar to Fig.10 Brittle fracture of cd.
[0096] Summary of the results of Examples 1 to 6: When connecting zirconium using existing welding technologies (laser welding, electron beam and friction welding, etc.), there are technical problems such as the connection temperature is too high, which weakens the joint performance and makes it difficult for the obtained components to meet nuclear applications and the welding efficiency is low. The present invention adopts discharge plasma diffusion connection technology to achieve reliable connection of zirconium. When a graphite mold is used, the connection of zirconium can be achieved at a welding temperature similar to hot pressing diffusion welding (900°C), and the insulation time is significantly reduced (10 minutes). More importantly, by not using a graphite mold, the current density flowing through the sample is increased. When the insulation time is 10 minutes, the connection temperature (600°C) can be further reduced while ensuring the joint performance. The obtained joint does not have obvious macroscopic deformation and phase change of zirconium, the joint performance is good, and the shear strength reaches 80% of the parent material. At the same welding temperature of 600°C, the holding time seems to have a greater impact on the performance of the joint under mold-free assembly, showing that the joint strength of 1s holding is 38% of that of 10min, but it is 7 times the shear strength of the joint obtained with graphite mold assembly at 600°C, which broadens the ideas for developing new zirconium connection technology. The method provided by the present invention can effectively reduce the welding temperature and holding time of zirconium, achieve high-quality connection of zirconium, and the shear mechanical properties of the joint are excellent, with high engineering use value.
[0097] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.
Claims
1. A low-temperature rapid discharge plasma diffusion bonding method for zirconium and its alloys, It is characterized in that The steps include: 1) Preparation of parent material: Use a Φ20mm high 5mm Zr702 cylinder, and grind the surface to be welded with 320#, 600#, 800#, 1000#, 1500#, and 2000# sandpaper respectively, then polish the surface to be welded of the parent material with 1μm diamond suspension polishing liquid, remove surface stains with ultrasonic cleaning, and gently wipe with alcohol cotton to dry for use; 2) Assembly: The zirconium base material to be welded is assembled in the order of lower graphite pressure head-graphite foil-zirconium base material to be welded-zirconium base material to be welded-graphite foil-upper graphite pressure head. Different from welding with graphite mold, the zirconium base material is directly placed on the graphite foil of the lower graphite pressure head in the furnace chamber. The cylindrical zirconium base material is placed coaxially, and the graphite paper foil and the upper graphite pressure head are placed on the base material in sequence, and then the welding operation can be carried out; 3) Discharge plasma diffusion welding connection: Prepare the assembled zirconium base materials to be welded for discharge plasma diffusion connection, fix the main temperature measuring thermocouple in contact with the surfaces of the two zirconium base materials to be connected, and use another thermocouple equipped with the system to fix it in contact with the upper and lower graphite pressure head temperature measuring holes for temperature monitoring, adjust the connection pressure to 30MPa, turn on the vacuum pump to make the vacuum degree in the sintering furnace reach the specified requirements, change the temperature control mode to manual temperature control, ensure that the temperature continues to rise steadily during the welding process, keep the temperature for 1S or 10min when the zirconium connection temperature of 600℃ is reached, then stop the welding operation immediately, cool with the furnace, and finally obtain the zirconium joint; There is no phase change of zirconium under the welding conditions of connection temperature 600℃ and holding temperature 10min; The shear strength of the zirconium joint finally obtained at room temperature reaches 80% of the shear strength of the parent material; Under the welding conditions of connection temperature of 600℃ and insulation for 1S, the joint strength is 38% of that of insulation for 10min.
Citation Information
Patent Citations
Connecting method of carbon steel and zirconia ceramic
CN105712731A
Discharge plasma diffusion bonding method for silicon carbide ceramic
CN110041090A
Method for diffusion bonding of zirconium and zirconium alloy and stainless steel
CN113814550A
Method for carrying out spark plasma diffusion bonding on silicon carbide ceramics by adopting refractory high-entropy alloy interlayer
CN113828880A
Zirconium alloy low-temperature diffusion bonding method
CN114101888A